Epitaxial growth method and device
The epitaxial growth method and device address inefficiencies in resistivity uniformity by adjusting the temperature field through automated resistivity testing and heating module power adjustments, enhancing production efficiency and yield.
Patent Information
- Application Number
- CN202411195919.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing epitaxial growth methods suffer from inefficient and inaccurate adjustments to resistivity uniformity in epitaxial layers, leading to poor device yield due to manual and offline testing processes.
An epitaxial growth method and device that adjusts the temperature field of the epitaxial reaction chamber by measuring resistivity at multiple preset test points and adjusting the power of the target heating module based on resistivity comparisons to improve uniformity.
Efficient and accurate adjustment of the temperature field enhances resistivity uniformity in epitaxial wafers, improving production efficiency and reducing manual intervention.
Smart Images

Figure CN119092422A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to an epitaxial growth method and device. Background Art
[0002] The epitaxial growth process of wafers is an important process in semiconductor chip manufacturing. Epitaxial growth refers to the process of growing an epitaxial layer (with the crystal orientation consistent with that of the substrate) on a single-crystal silicon substrate through epitaxy technology. The entire production process of epitaxial wafers includes five major processes: crystal growth (pulling silicon crystal rods from polysilicon materials) → molding (slicing and grinding) → polishing (double-sided polishing) → cleaning (removing surface particles, metal ions and organic matter) → epitaxy (vapor deposition). Epitaxy is the last important process, which can improve the crystal properties, native defects, resistivity and flatness of the polished wafer.
[0003] The resistivity uniformity of the epitaxial layer is an important indicator of the performance of the epitaxial layer. Poor resistivity uniformity of the epitaxial layer will affect the device yield. The resistivity of the epitaxial layer is mainly related to temperature. In related technologies, when adjusting the resistivity uniformity of the epitaxial layer, the production equipment is manually adjusted when the equipment is shut down, samples are grown, and offline tests are performed. Finally, according to the test results, the production equipment is manually adjusted and confirmed again. This is inefficient and has poor accuracy. It is also time-consuming and affects normal production. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an epitaxial growth method and device, which can efficiently and accurately adjust the temperature field of the epitaxial reaction chamber and improve the resistivity uniformity of the epitaxial wafer.
[0005] In order to achieve the above object, the technical solution adopted by the embodiment of the present invention is:
[0006] An epitaxial growth method comprising:
[0007] Sending a wafer into an epitaxial reaction chamber to grow an epitaxial layer on the wafer;
[0008] Acquiring resistivity of a plurality of preset test points of the epitaxial layer, wherein the plurality of preset test points include a first test point located at the center of the epitaxial layer and other test points;
[0009] calculating the resistivity uniformity of the epitaxial layer;
[0010] When the resistivity uniformity of the epitaxial layer is greater than a preset threshold, the resistivity of the first test point is compared with the resistivity of the other test points, and the power of the target heating module of the epitaxial reaction chamber is adjusted according to the comparison result.
[0011] In some embodiments, calculating the resistivity uniformity of the epitaxial layer includes:
[0012] The maximum resistivity value among the plurality of preset test points is recorded as R_max, and the minimum resistivity value is recorded as R_min;
[0013] The resistivity uniformity of the epitaxial layer is calculated using the following formula: (R_max-R_min) / (R_max+R_min).
[0014] In some embodiments, the preset threshold is 2-3%.
[0015] In some embodiments, adjusting the power of the target heating module of the epitaxial reaction chamber according to the comparison result includes:
[0016] Determining a minimum value among the resistivities of the plurality of preset test points;
[0017] Comparing the resistivity of the first test point with the minimum value;
[0018] If the resistivity of the first test point is greater than the minimum value, the power of the target heating module is increased according to a preset ratio; if the resistivity of the first test point is less than the minimum value, the power of the target heating module is reduced according to a preset ratio.
[0019] In some embodiments, the preset ratio is 2-4%.
[0020] In some embodiments, the heating module of the epitaxial reaction chamber includes an external heating module and an internal heating module, the internal heating module is located on a side of the external heating module close to the wafer, and the target heating module is the internal heating module.
[0021] In some embodiments, the plurality of preset test points include a first test point located at the center of the epitaxial layer, and four test points located at the edge of the epitaxial layer: a sixth test point, a seventh test point, an eighth test point, and a ninth test point, wherein the sixth test point and the eighth test point are located on a first diameter of the wafer, the seventh test point and the ninth test point are located on a second diameter of the wafer, and the first diameter is perpendicular to the second diameter;
[0022] The plurality of preset test points also include:
[0023] a second test point located at the center of a line connecting the sixth test point and the first test point, a third test point located at the center of a line connecting the seventh test point and the first test point, a fourth test point located at the center of a line connecting the eighth test point and the first test point, and a fifth test point located at the center of a line connecting the ninth test point and the first test point.
[0024] The embodiment of the present invention further provides an epitaxial growth device, comprising:
[0025] A growth module, used for sending a wafer into an epitaxial reaction chamber and growing an epitaxial layer on the wafer;
[0026] An acquisition module, used for acquiring the resistivity of a plurality of preset test points of the epitaxial layer, wherein the plurality of preset test points include a first test point located at the center of the epitaxial layer and other test points;
[0027] A calculation module, used for calculating the resistivity uniformity of the epitaxial layer;
[0028] A processing module is used to compare the resistivity of the first test point with the resistivity of the other test points when the resistivity uniformity of the epitaxial layer is greater than a preset threshold, and adjust the power of the target heating module of the epitaxial reaction chamber according to the comparison result.
[0029] In some embodiments, the calculation module is specifically used to record the maximum resistivity among the multiple preset test points as R_max and the minimum resistivity as R_min; and calculate the resistivity uniformity of the epitaxial layer using the following formula: (R_max-R_min) / (R_max+R_min).
[0030] In some embodiments, the processing module is specifically used to determine the minimum value among the resistivities of the multiple preset test points; compare the resistivity of the first test point with the minimum value; if the resistivity of the first test point is greater than the minimum value, increase the power of the target heating module according to a preset ratio; if the resistivity of the first test point is less than the minimum value, reduce the power of the target heating module according to a preset ratio.
[0031] The beneficial effects of the present invention are:
[0032] In this embodiment, after growing the epitaxial layer, the resistivities of multiple preset test points are obtained and the resistivity uniformity of the epitaxial layer is calculated. When the resistivity uniformity of the epitaxial layer does not meet the requirements, the power of the target heating module is adjusted according to the comparison results of the resistivities of multiple preset test points, so that the temperature field of the epitaxial reaction chamber can be adjusted efficiently and accurately, thereby improving the resistivity uniformity of the epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 A schematic diagram showing the structure of an epitaxial reaction chamber;
[0034] Figure 2 A schematic diagram showing a flow chart of an epitaxial growth method according to an embodiment of the present invention;
[0035] Figure 3 A schematic diagram showing test points according to an embodiment of the present invention;
[0036] Figure 4-Figure 6 A schematic diagram showing how the resistivity uniformity of an epitaxial wafer is improved according to an embodiment of the present invention;
[0037] Figure 7 A schematic diagram showing the structure of an epitaxial growth device according to an embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0039] Figure 1 A schematic diagram showing the structure of an epitaxial reaction chamber is shown in FIG. Figure 1 As shown, the epitaxial reaction chamber includes an upper quartz bell jar 1, a lower quartz bell jar 2, a halogen lamp 3, a base support rod 4, a pin 5, a pin support rod 6, a mounting component 7, a base 8, a preheating ring 9, a bottom pyrometer 10 and a top pyrometer 11 and other components.
[0040] When epitaxial growth is performed, the wafer is input into the epitaxial reaction chamber and carried on the susceptor 8 in the epitaxial reaction chamber. The wafer is heated by the upper heating module arranged on the upper side of the susceptor 8 and the lower heating module arranged on the lower side of the susceptor 8. In addition, the raw material gas is supplied to the main surface of the wafer, thereby performing vapor phase growth. After the vapor phase growth, the epitaxial wafer obtained by the vapor phase growth is output to the outside of the epitaxial reaction chamber. During the growth process, the susceptor support rod 4 plays the role of fixing the susceptor 8 and driving the susceptor 8 to rotate, so that the epitaxial growth can be performed uniformly on the wafer.
[0041] The present invention provides an epitaxial growth method and device, which can efficiently and accurately adjust the temperature field of an epitaxial reaction chamber and improve the resistivity uniformity of an epitaxial wafer.
[0042] The embodiment of the present invention provides an epitaxial growth method, such as Figure 2As shown, including:
[0043] Step 101: sending a wafer into an epitaxial reaction chamber to grow an epitaxial layer on the wafer;
[0044] Step 102: Obtain the resistivity of a plurality of preset test points of the epitaxial layer, wherein the plurality of preset test points include a first test point located at the center of the epitaxial layer and other test points;
[0045] In this embodiment, the resistivity of 5 or 9 test points on the epitaxial layer can be tested. In order to improve the accuracy of the test, the resistivity of 9 test points on the epitaxial layer can be tested. Figure 3 As shown, the 9 preset test points include a first test point P1 located at the center of the epitaxial layer, and four test points located at the edge of the epitaxial layer: a sixth test point P6, a seventh test point P7, an eighth test point P8 and a ninth test point P9, the sixth test point P6 and the eighth test point P8 are located on the first diameter of the wafer, the seventh test point P7 and the ninth test point P9 are located on the second diameter of the wafer, and the first diameter is perpendicular to the second diameter;
[0046] The 9 preset test points also include:
[0047] A second test point P2 located at the center of a line connecting the sixth test point P6 and the first test point P1, a third test point P3 located at the center of a line connecting the seventh test point P7 and the first test point P1, a fourth test point P4 located at the center of a line connecting the eighth test point P8 and the first test point P1, and a fifth test point P5 located at the center of a line connecting the ninth test point P9 and the first test point P1.
[0048] Among them, the distance between the sixth test point P6, the seventh test point P7, the eighth test point P8 and the ninth test point P9 and the edge of the wafer may be about 5 mm.
[0049] Step 103: Calculating the resistivity uniformity of the epitaxial layer;
[0050] Specifically, the maximum resistivity value among the plurality of preset test points may be recorded as R_max, and the minimum resistivity value may be recorded as R_min; and the resistivity uniformity of the epitaxial layer may be calculated using the following formula:
[0051] (R_max-R_min) / (R_max+R_min).
[0052] Step 104: When the resistivity uniformity of the epitaxial layer is greater than a preset threshold, the resistivity of the first test point is compared with the resistivity of the other test points, and the power of the target heating module of the epitaxial reaction chamber is adjusted according to the comparison result.
[0053] When the resistivity uniformity of the epitaxial layer is greater than a preset threshold, it indicates that the resistivity uniformity of the epitaxial layer is poor and the resistivity uniformity of the epitaxial layer needs to be adjusted. The resistivity of the epitaxial layer is mainly related to the temperature. The higher the temperature of the wafer, the lower the resistivity of the grown epitaxial layer. Therefore, the resistivity uniformity of the epitaxial wafer can be improved by adjusting the power of the target heating module of the epitaxial reaction chamber. When the resistivity uniformity of the epitaxial layer is not greater than the preset threshold, it indicates that the resistivity uniformity of the epitaxial layer is good and the resistivity uniformity of the epitaxial layer does not need to be adjusted.
[0054] In some embodiments, the preset threshold may be 2-3%, for example, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9% or 3%.
[0055] In some embodiments, the heating module of the epitaxial reaction chamber includes an upper heating module located on the upper side of the pedestal and a lower heating module located on the lower side of the pedestal, the upper heating module includes an external heating module and an internal heating module, the lower heating module includes an external heating module and an internal heating module, the internal heating module is located on the side of the external heating module close to the wafer, and the target heating module is the internal heating module. Compared with the external heating module, the internal heating module is closer to the wafer and has a greater impact on the epitaxial layer, so the resistivity uniformity of the epitaxial wafer can be improved by adjusting the power of the internal heating module.
[0056] In some embodiments, adjusting the power of the target heating module of the epitaxial reaction chamber according to the comparison results includes: determining the minimum value among the resistivities of the multiple preset test points; comparing the resistivity of the first test point with the minimum value; if the resistivity of the first test point is greater than the minimum value, increasing the power of the target heating module according to a preset ratio; if the resistivity of the first test point is less than the minimum value, reducing the power of the target heating module according to a preset ratio.
[0057] Specifically, the preset ratio can be 2-4%, for example, it can be 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9% or 4%.
[0058] For example, when the resistivity at point P1 is less than the minimum value, the power of the target heating module is reduced by 2-4%; when the resistivity at point P1 is greater than the minimum value, the power of the target heating module is increased by 2-4%; when the resistivity at point P1 is equal to the minimum value, the power of the target heating module does not need to be adjusted.
[0059] This embodiment can periodically perform the above steps 101-104 according to a preset cycle. Through the technical solution of this embodiment, after the epitaxial layer is grown, the resistivity of multiple preset test points is obtained, and the resistivity uniformity of the epitaxial layer is calculated. When the resistivity uniformity of the epitaxial layer does not meet the requirements, the power of the target heating module is adjusted according to the comparison results of the resistivity of multiple preset test points, so that the temperature field of the epitaxial reaction chamber can be adjusted efficiently and accurately, the resistivity uniformity of the epitaxial wafer can be improved, and the normal production of the equipment is not affected, avoiding many inconveniences of manual operation.
[0060] Figure 4 The resistivity diagram of the 9 test points before and after adjustment in Example 1, where blue represents the resistivity of the 9 test points before adjusting the power of the target heating module, and yellow represents the resistivity of the 9 test points after adjusting the power of the target heating module, where the horizontal axis represents the serial number of the test point, and the vertical axis represents the resistivity of the test point. Before adjustment, the resistivity of point P1 is less than the minimum resistivity of the 9 test points, R(P1)-Rmin<0, then the power of the target heating module is reduced by 2-4%. Since the power of the heating module corresponding to the center area of the wafer is reduced, the temperature of the corresponding area will also decrease. The decrease in temperature will cause an increase in resistivity, such as Figure 4 As shown in Figure 2, the resistivity of the adjusted P1-P4 points has increased. Figure 6 As shown in Table 1, the resistivity uniformity of the epitaxial wafer decreased from 3.05% before adjustment to 2.22%, and the resistivity uniformity of the epitaxial wafer was significantly improved.
[0061] Figure 5 The resistivity diagram of the 9 test points before and after adjustment in Example 2, where blue represents the resistivity of the 9 test points before adjusting the power of the target heating module, and yellow represents the resistivity of the 9 test points after adjusting the power of the target heating module, where the horizontal axis represents the serial number of the test point, and the vertical axis represents the resistivity of the test point. Before adjustment, the resistivity of point P1 is greater than the minimum resistivity of the 9 test points, R(P1)-Rmin>0, then the power of the target heating module is increased by 2-4%. Since the power of the heating module corresponding to the center area of the wafer increases, the temperature of the corresponding area will also increase. The increase in temperature will cause a decrease in resistivity, such as Figure 5As shown in the figure, the resistivity of point P1 after adjustment is the minimum of the 9 test points, and the resistivity of points P1-P5 has decreased. Figure 6 As shown in Table 1, the resistivity uniformity of the epitaxial wafer is reduced from 3.08% before adjustment to 2.50%, and the resistivity uniformity of the epitaxial wafer is significantly improved.
[0062] Table 1
[0063]
[0064]
[0065] The embodiment of the present invention also provides an epitaxial growth device, such as Figure 7 As shown, including:
[0066] A growth module 21 is used to send a wafer into an epitaxial reaction chamber and grow an epitaxial layer on the wafer;
[0067] An acquisition module 22, used for acquiring the resistivity of a plurality of preset test points of the epitaxial layer, wherein the plurality of preset test points include a first test point located at the center of the epitaxial layer and other test points;
[0068] A calculation module 23, used for calculating the resistivity uniformity of the epitaxial layer;
[0069] The processing module 24 is used to compare the resistivity of the first test point with the resistivity of the other test points when the resistivity uniformity of the epitaxial layer is greater than a preset threshold, and adjust the power of the target heating module of the epitaxial reaction chamber according to the comparison result.
[0070] In this embodiment, after growing the epitaxial layer, the resistivities of multiple preset test points are obtained and the resistivity uniformity of the epitaxial layer is calculated. When the resistivity uniformity of the epitaxial layer does not meet the requirements, the power of the target heating module is adjusted according to the comparison results of the resistivities of multiple preset test points, so that the temperature field of the epitaxial reaction chamber can be adjusted efficiently and accurately, thereby improving the resistivity uniformity of the epitaxial wafer.
[0071] In this embodiment, the resistivity of 5 or 9 test points on the epitaxial layer can be tested. In order to improve the accuracy of the test, the resistivity of 9 test points on the epitaxial layer can be tested. Figure 3As shown, the 9 preset test points include a first test point P1 located at the center of the epitaxial layer, and four test points located at the edge of the epitaxial layer: a sixth test point P6, a seventh test point P7, an eighth test point P8 and a ninth test point P9, the sixth test point P6 and the eighth test point P8 are located on the first diameter of the wafer, the seventh test point P7 and the ninth test point P9 are located on the second diameter of the wafer, and the first diameter is perpendicular to the second diameter;
[0072] The 9 preset test points also include:
[0073] A second test point P2 located at the center of a line connecting the sixth test point P6 and the first test point P1, a third test point P3 located at the center of a line connecting the seventh test point P7 and the first test point P1, a fourth test point P4 located at the center of a line connecting the eighth test point P8 and the first test point P1, and a fifth test point P5 located at the center of a line connecting the ninth test point P9 and the first test point P1.
[0074] Among them, the distance between the sixth test point P6, the seventh test point P7, the eighth test point P8 and the ninth test point P9 and the edge of the wafer may be about 5 mm.
[0075] In some embodiments, the calculation module 23 is specifically used to record the maximum resistivity among the multiple preset test points as R_max and the minimum resistivity as R_min; and calculate the resistivity uniformity of the epitaxial layer using the following formula: (R_max-R_min) / (R_max+R_min).
[0076] In some embodiments, the processing module 24 is specifically used to determine the minimum value among the resistivities of the multiple preset test points; compare the resistivity of the first test point with the minimum value; if the resistivity of the first test point is greater than the minimum value, increase the power of the target heating module according to a preset ratio; if the resistivity of the first test point is less than the minimum value, reduce the power of the target heating module according to a preset ratio.
[0077] Specifically, the preset ratio can be 2-4%, for example, it can be 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9% or 4%.
[0078] For example, when the resistivity at point P1 is less than the minimum value, the power of the target heating module is reduced by 2-4%; when the resistivity at point P1 is greater than the minimum value, the power of the target heating module is increased by 2-4%; when the resistivity at point P1 is equal to the minimum value, the power of the target heating module does not need to be adjusted.
[0079] It should be noted that each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments, since they are basically similar to the product embodiments, the description is relatively simple, and the relevant parts can be referred to the partial description of the product embodiments.
[0080] Unless otherwise defined, the technical terms or scientific terms used in the present disclosure should be understood by people with ordinary skills in the field to which the present disclosure belongs. The "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0081] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being “on” or “under” another element, it can be “directly on” or “under” the other element or intervening elements may be present.
[0082] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0083] The above is only a specific embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.
Claims
1. An epitaxial growth method, characterized in that: include: Sending a wafer into an epitaxial reaction chamber to grow an epitaxial layer on the wafer; Obtaining resistivity of a plurality of preset test points of the epitaxial layer, wherein the plurality of preset test points include a first test point located at the center of the epitaxial layer and other test points; calculating the resistivity uniformity of the epitaxial layer; When the resistivity uniformity of the epitaxial layer is greater than a preset threshold, the resistivity of the first test point is compared with the resistivity of the other test points, and the power of the target heating module of the epitaxial reaction chamber is adjusted according to the comparison result.
2. The epitaxial growth method according to claim 1, characterized in that: The calculating the resistivity uniformity of the epitaxial layer comprises: The maximum resistivity value among the plurality of preset test points is recorded as R_max, and the minimum resistivity value is recorded as R_min; The resistivity uniformity of the epitaxial layer is calculated using the following formula: (R_max-R_min) / (R_max+R_min).
3. The epitaxial growth method according to claim 1, characterized in that: The preset threshold is 2-3%.
4. The epitaxial growth method according to claim 1, characterized in that: The adjusting the power of the target heating module of the epitaxial reaction chamber according to the comparison result includes: Determining a minimum value among the resistivities of the plurality of preset test points; Comparing the resistivity of the first test point with the minimum value; If the resistivity of the first test point is greater than the minimum value, the power of the target heating module is increased according to a preset ratio; if the resistivity of the first test point is less than the minimum value, the power of the target heating module is reduced according to a preset ratio.
5. The epitaxial growth method according to claim 4, characterized in that: The preset ratio is 2-4%.
6. The epitaxial growth method according to claim 1, characterized in that: The heating module of the epitaxial reaction chamber comprises an external heating module and an internal heating module. The internal heating module is located on a side of the external heating module close to the wafer, and the target heating module is the internal heating module.
7. The epitaxial growth method according to claim 1, characterized in that: The plurality of preset test points include a first test point located at the center of the epitaxial layer, and four test points located at the edge of the epitaxial layer: a sixth test point, a seventh test point, an eighth test point, and a ninth test point, wherein the sixth test point and the eighth test point are located on a first diameter of the wafer, the seventh test point and the ninth test point are located on a second diameter of the wafer, and the first diameter is perpendicular to the second diameter; The plurality of preset test points also include: a second test point located at the center of a line connecting the sixth test point and the first test point, a third test point located at the center of a line connecting the seventh test point and the first test point, a fourth test point located at the center of a line connecting the eighth test point and the first test point, and a fifth test point located at the center of a line connecting the ninth test point and the first test point.
8. An epitaxial growth device, characterized in that: include: A growth module, used for sending a wafer into an epitaxial reaction chamber and growing an epitaxial layer on the wafer; An acquisition module, used for acquiring the resistivity of a plurality of preset test points of the epitaxial layer, wherein the plurality of preset test points include a first test point located at the center of the epitaxial layer and other test points; A calculation module, used for calculating the resistivity uniformity of the epitaxial layer; A processing module is used to compare the resistivity of the first test point with the resistivity of the other test points when the resistivity uniformity of the epitaxial layer is greater than a preset threshold, and adjust the power of the target heating module of the epitaxial reaction chamber according to the comparison result.
9. The epitaxial growth device according to claim 8, characterized in that: The calculation module is specifically used to record the maximum resistivity among the plurality of preset test points as R_max, and the minimum resistivity as R_min; The resistivity uniformity of the epitaxial layer is calculated using the following formula: (R_max-R_min) / (R_max+R_min).
10. The epitaxial growth device according to claim 8, characterized in that: The processing module is specifically used to determine the minimum value among the resistivities of the multiple preset test points; compare the resistivity of the first test point with the minimum value; if the resistivity of the first test point is greater than the minimum value, increase the power of the target heating module according to a preset ratio; if the resistivity of the first test point is less than the minimum value, reduce the power of the target heating module according to a preset ratio.