Preparation method of passivation layer of TOPCon battery and passivation layer thereof

The method for preparing a passivation layer with a tunnel oxide and multiple poly-Si layers in TOPCon cells addresses high recombination rates and poor phosphorus diffusion, enhancing the passivation effect and efficiency.

CN119092596APending Publication Date: 2024-12-06JINNENG PHOTOVOLTAIC TECH LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411211380.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing TOPCon cells experience high internal carrier recombination rates and poor phosphorus diffusion, leading to poor passivation effects and low photoelectric conversion efficiency due to the structure of the passivation layer.

Method used

A method involving multiple vacuum treatments and gas introductions in a PECVD reactor to form a passivation layer with a tunnel oxide layer, multiple poly-Si layers, and a molecular sieve layer, enhancing the phosphorus diffusion effect and reducing recombination rates.

Benefits of technology

The improved passivation layer significantly reduces carrier recombination, enhances anti-PID performance, and increases the open circuit voltage factor, thereby improving the photoelectric conversion efficiency of TOPCon cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092596A_ABST
    Figure CN119092596A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a passivation layer of a TOPCon cell and the passivation layer thereof, and belongs to the technical field of photovoltaic cell preparation. Comprising the step of sequentially depositing a tunneling oxide layer, a first poly-si layer, a molecular sieve layer, a second poly-si layer, a third poly-si layer and a mask layer on the back surface of an N-type silicon wafer so as to obtain the prepared passivation layer of the TOPCon battery. By adding the molecular sieve layer and the third poly-si layer on the back surfaces of the plurality of N-type silicon wafers, compared with the prior art that the passivation layer of the TOPCon cell has a structure of a doped polycrystalline silicon film layer and a heavily doped polycrystalline silicon layer, the passivation layer of the TOPCon cell is beneficial to reducing the recombination loss of the back surface, improving the phosphorus diffusion effect of the back surfaces of the N-type silicon wafers, and improving the performance of the TOPCon cell. The passivation effect of the TOPCon cell is improved, the recombination rate of carriers on the back surface of the N-type silicon wafer is reduced, and the photoelectric conversion efficiency of the TOPCon cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic cell preparation, and in particular to a preparation method of a passivation layer of a TOPCon cell and the passivation layer thereof. Background Art

[0002] TOPCon (Tunnel Oxide Passivated Contact) cells, a new type of crystalline silicon solar cell technology, aim to improve photoelectric conversion efficiency and reduce manufacturing costs by improving traditional cell structure and materials. A key feature of TOPCon cells is their use of a passivation contact technology that utilizes a tunneling silicon oxide layer and a doped polysilicon layer. Passivation contact uses an ultra-thin dielectric film to isolate the metal electrode from the semiconductor, enabling carrier tunneling while passivating the cell silicon wafer surface. This effectively reduces recombination losses caused by direct contact between the metal electrode and the cell silicon wafer, while simultaneously achieving both passivation and contact effects.

[0003] The doped polysilicon film layer in the passivation layer, namely the poly-Si layer, protects the tunneling oxide layer and prevents it from being damaged. Heavily doping the poly-Si layer can form a high-low junction on the back of the cell silicon wafer, effectively reducing the recombination rate of carriers on the back of the cell silicon wafer and further improving the photoelectric conversion efficiency of the TOPCon cell. Therefore, the heavily doped polysilicon layer is crucial to the passivation performance of the TOPCon cell. Although the existing TOPCon cell passivation layer is provided with a doped polysilicon film layer and a heavily doped polysilicon layer, it is still found in actual applications that the internal carriers recombine more frequently on the back of the cell silicon wafer and the phosphorus diffusion effect is poor, resulting in poor passivation effect and low photoelectric conversion efficiency of the existing TOPCon cell passivation layer. Summary of the Invention

[0004] To solve the above technical problems, the present invention provides a method for preparing a passivation layer of a TOPCon battery and the passivation layer thereof. The technical solution of the present invention is as follows:

[0005] In a first aspect, the present invention provides a method for preparing a passivation layer of a TOPCon battery, comprising the following steps:

[0006] S1, placing a graphite boat loaded with multiple N-type silicon wafers into the chamber of a PECVD reactor tube, and then performing a first vacuum treatment, preheating treatment, and leak detection treatment on the chamber to obtain a reaction chamber for performing a PECVD reaction;

[0007] S2, introducing nitrous oxide into the reaction chamber to perform a pre-deposition treatment and a deposition treatment of a tunnel oxide layer on a plurality of N-type silicon wafers, so that a tunnel oxide layer is formed on the back side of the plurality of N-type silicon wafers, and then performing a second vacuum treatment on the reaction chamber after the tunnel oxide layer deposition treatment is completed;

[0008] S3, introducing silane, hydrogen and phosphine into the reaction chamber after the second vacuum treatment, to perform pre-deposition treatment and deposition treatment of the first poly-Si layer on multiple N-type silicon wafers, so that the first poly-Si layer is formed on the back side of the tunnel oxide layer, and then the reaction chamber after the deposition treatment of the first poly-Si layer is vacuumed for the third time;

[0009] S4, introducing laughing gas into the reaction chamber after the third vacuum treatment, to perform pre-deposition treatment and deposition treatment of molecular sieve layer on multiple N-type silicon wafers, so that the back side of the first poly-Si layer forms a molecular sieve layer, and then vacuuming the reaction chamber after the deposition treatment of the molecular sieve layer for the fourth time;

[0010] S5, introducing silane, hydrogen and phosphine into the reaction chamber after the fourth vacuum treatment to perform pre-deposition treatment and deposition treatment of the second poly-Si layer on multiple N-type silicon wafers, so that the second poly-Si layer is formed on the back of the molecular sieve layer, and then the reaction chamber after the second poly-Si layer deposition treatment is completed is vacuumed for the fifth time;

[0011] S6, introducing silane, hydrogen and phosphine into the reaction chamber that has completed the fifth vacuum treatment to perform a pre-deposition treatment and a deposition treatment of a third poly-Si layer on multiple N-type silicon wafers, so that a third poly-Si layer is formed on the back of the second poly-Si layer, and then the reaction chamber that has completed the deposition treatment of the third poly-Si layer is vacuumed for the sixth time;

[0012] S7, introducing silane and laughing gas into the reaction chamber that has completed the sixth vacuum treatment to perform pre-deposition treatment and deposition treatment of the mask layer on multiple N-type silicon wafers, so that a mask layer is formed on the back side of the third poly-Si layer, and then the reaction chamber that has completed the deposition treatment of the mask layer is vacuumed for the seventh time;

[0013] S8, introducing a purge gas into the reaction chamber that has completed the seven vacuum treatments to purge the reaction chamber, and then sending the graphite boat that has completed the purge treatment out of the PECVD reaction furnace tube to obtain the passivation layer of the prepared TOPCon battery.

[0014] Optionally, the S1, when implemented, includes:

[0015] S11, opening the furnace door of the PECVD reactor tube, placing a graphite boat loaded with multiple N-type silicon wafers into the cavity of the PECVD reactor tube, and closing the furnace door;

[0016] S12, performing a first vacuum treatment on the cavity of the PECVD reaction furnace tube loaded with the quartz boat, so that the pressure inside the cavity is the bottom pressure value;

[0017] S13, preheating the cavity of the furnace tube so that the temperature range of the cavity is 435±15°C;

[0018] S14, performing a leak detection process on the cavity that has completed the preheating process to confirm that there is no gas leakage inside the cavity, thereby obtaining a reaction cavity for performing a PECVD reaction.

[0019] Optionally, when S2 is implemented, it includes:

[0020] S21, introducing nitrous oxide (NNO) at a flow rate of 10,000 sccm / min into the reaction chamber while maintaining a reaction chamber temperature of 435±15° C. and controlling the pressure within the reaction chamber to 1,800 mTorr, and performing a tunneling oxide pre-deposition treatment on a plurality of N-type silicon wafers using the NNO. The tunneling oxide pre-deposition treatment lasts for 30 seconds.

[0021] S22, performing a first glow discharge treatment on the plurality of N-type silicon wafers that have undergone a pre-deposition treatment of a tunnel oxide layer using a radio frequency power supply, thereby performing a tunnel oxide layer deposition treatment on the plurality of N-type silicon wafers, so that a tunnel oxide layer is formed on the back side of the plurality of N-type silicon wafers; wherein the tunnel oxide layer deposition treatment time is 116 seconds;

[0022] S23, performing a second vacuuming process on the reaction chamber that has completed the first glow discharge, so as to extract the laughing gas in the reaction chamber out of the reaction chamber.

[0023] Optionally, when S3 is implemented, it includes:

[0024] S31, under the condition that the reaction chamber temperature range is 435±15°C, silane with a flow rate of 3450 sccm / min, hydrogen with a flow rate of 11160 sccm / min, and phosphine with a flow rate of 295 sccm / min are introduced into the reaction chamber after the second vacuum treatment, and the pressure inside the reaction chamber is controlled to be 3050 mTorr. A first poly-Si layer is pre-deposited on multiple N-type silicon wafers using silane, hydrogen, and phosphine; wherein the pre-deposition time of the first poly-Si layer is 60 seconds;

[0025] S32, performing a second glow discharge treatment on the plurality of N-type silicon wafers that have completed the pre-deposition treatment of the first poly-Si layer using a radio frequency power supply, so as to deposit the first poly-Si layer on the plurality of N-type silicon wafers, so as to form the first poly-Si layer on the back side of the tunnel oxide layer; wherein the deposition time of the first poly-Si layer is 100 seconds;

[0026] S33, performing a third vacuuming process on the reaction chamber that has completed the second glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

[0027] Optionally, when S4 is implemented, it includes:

[0028] S41, introducing nitrous oxide at a flow rate of 10,000 sccm / min into the reaction chamber after the third vacuuming process, while controlling the pressure inside the reaction chamber to 1,800 mTorr, and performing a pre-deposition treatment of a molecular sieve layer on multiple N-type silicon wafers using the nitrous oxide; wherein the pre-deposition treatment of the molecular sieve layer lasts for 30 seconds;

[0029] S42, performing a third glow discharge treatment on the plurality of N-type silicon wafers that have undergone the pre-deposition treatment of the molecular sieve layer using a radio frequency power supply to deposit the molecular sieve layer on the plurality of N-type silicon wafers, so that a molecular sieve layer is formed on the back side of the first poly-Si layer; wherein the deposition treatment time of the molecular sieve layer is 120 seconds;

[0030] S43, performing a fourth vacuuming process on the reaction chamber that has completed the third glow discharge, so as to extract the laughing gas inside the reaction chamber out of the reaction chamber.

[0031] Optionally, when S5 is specifically implemented, it includes:

[0032] S51, under the condition that the reaction chamber temperature range is 435±15°C, silane with a flow rate of 3450 sccm / min, hydrogen with a flow rate of 10800 sccm / min, and phosphine with a flow rate of 460 sccm / min are introduced into the reaction chamber that has completed the fourth vacuum treatment, and the pressure in the reaction chamber is controlled to be 3050 mTorr. A second poly-Si layer is pre-deposited on multiple N-type silicon wafers using silane, hydrogen, and phosphine; wherein the pre-deposition time of the second poly-Si layer is 30 seconds;

[0033] S52, performing a fourth glow discharge treatment on the plurality of N-type silicon wafers that have completed the pre-deposition treatment of the second poly-Si layer using a radio frequency power supply, thereby performing a second poly-Si layer deposition treatment on the plurality of N-type silicon wafers, so as to form a second poly-Si layer on the back side of the molecular sieve layer; wherein the deposition treatment time of the second poly-Si layer is 265 seconds;

[0034] S53, performing a fifth vacuuming process on the reaction chamber that has completed the fourth glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

[0035] Optionally, when S6 is implemented, it includes:

[0036] S61, under the condition that the reaction chamber temperature range is 435±15° C., introducing silane at a flow rate of 3450 sccm / min, hydrogen at a flow rate of 10080 sccm / min, and phosphine at a flow rate of 1017 sccm / min into the reaction chamber that has completed the fifth vacuum treatment, and controlling the pressure inside the reaction chamber to 3100 mTorr, performing a pre-deposition treatment of a third poly-Si layer on multiple N-type silicon wafers using silane, hydrogen, and phosphine; wherein the pre-deposition treatment time of the third poly-Si layer is 60 seconds;

[0037] S62, performing a fifth glow discharge treatment on the plurality of N-type silicon wafers that have completed the pre-deposition treatment of the third poly-Si layer using a radio frequency power supply, thereby performing a third poly-Si layer deposition treatment on the plurality of N-type silicon wafers, so as to form a third poly-Si layer on the back side of the second poly-Si layer; wherein the deposition treatment time of the third poly-Si layer is 212 seconds;

[0038] S63, performing a sixth vacuuming process on the reaction chamber that has completed the fifth glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

[0039] Optionally, when S7 is implemented, it includes:

[0040] S71, introducing silane at a flow rate of 1622 sccm / min and nitrous oxide at a flow rate of 7084 sccm / min into the reaction chamber after the sixth vacuuming process, with the reaction chamber temperature in the range of 435±15° C., and controlling the pressure inside the reaction chamber to be 1750 mTorr, to perform a pre-deposition treatment of a mask layer on multiple N-type silicon wafers using the silane and nitrous oxide; wherein the pre-deposition treatment of the mask layer lasts for 30 seconds;

[0041] S72, performing a sixth glow discharge treatment on the plurality of N-type silicon wafers that have undergone the pre-deposition treatment of the mask layer using a radio frequency power supply to deposit a mask layer on the plurality of N-type silicon wafers, so as to form a mask layer on the back side of the third poly-Si layer; wherein the deposition time of the mask layer is 60 seconds;

[0042] S73, performing a seventh vacuuming process on the reaction chamber that has completed the sixth glow discharge, so as to extract the silane and nitrous oxide inside the reaction chamber out of the reaction chamber.

[0043] Optionally, when S8 is specifically implemented, it includes:

[0044] S81, introducing a purge gas into the reaction chamber that has completed the seventh vacuuming process to purge the reaction chamber so that the pressure in the reaction chamber returns to atmospheric pressure;

[0045] S82, after the purge treatment is completed, the furnace door of the PECVD reaction furnace tube is opened, the graphite boat loaded with multiple N-type silicon wafers is sent out of the reaction chamber, and the furnace door is closed to obtain the prepared passivation layer of the TOPCon battery.

[0046] In a second aspect, the present invention provides a passivation layer of a TOPCon battery, which is prepared by the above-mentioned method for preparing a passivation layer of a TOPCon battery. The passivation layer of the TOPCon battery includes an N-type silicon wafer and a tunneling oxide layer, a first poly-Si layer, a molecular sieve layer, a second poly-Si layer, a third poly-Si layer and a mask layer formed in sequence on the back of the N-type silicon wafer; the total thickness of the first poly-Si layer, the molecular sieve layer, the second poly-Si layer and the third poly-Si layer is 99.5nm±2nm.

[0047] All the above optional technical solutions can be combined arbitrarily, and the present invention does not provide detailed descriptions of the structures after each combination.

[0048] By means of the above solution, the beneficial effects of the present invention are as follows:

[0049] By introducing nitrous oxide into the reaction chamber, a molecular sieve layer is pre-deposited and deposited on multiple N-type silicon wafers, so that a molecular sieve layer is formed on the back of the first poly-Si layer. Then, silane, hydrogen and phosphine are introduced into the reaction chamber to pre-deposit and deposit a third poly-Si layer on the multiple N-type silicon wafers, so that a third poly-Si layer is formed on the back of the second poly-Si layer. Compared with the structure of the passivation layer of the TOPCon battery in the prior art having a doped polysilicon film layer and a heavily doped polysilicon layer, the passivation layer of the TOPCon battery of the present invention adds a molecular sieve layer and a third poly-Si layer, which significantly improves the phosphorus diffusion effect on the back of the N-type silicon wafer, improves the passivation effect and anti-PID performance of the TOPCon battery, reduces the recombination rate of carriers on the back of the N-type silicon wafer, reduces the metal contact recombination between the back metal electrode of the TOPCon battery and the N-type silicon wafer, improves the open circuit voltage factor, and improves the photoelectric conversion efficiency of the TOPCon battery.

[0050] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is a preparation flow chart of the present invention;

[0052] Figure 2 This is a schematic structural diagram of the passivation layer of the TOPCon battery provided by the present invention.

[0053] Description of Figure Numbers:

[0054] 1. N-type silicon wafer; 2. Tunneling oxide layer; 3. First poly-Si layer; 4. Molecular sieve layer; 5. Second poly-Si layer; 6. Third poly-Si layer; 7. Mask layer. DETAILED DESCRIPTION

[0055] The following embodiments of the present invention are described in further detail with reference to the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0056] like Figure 1 As shown, the present invention provides a method for preparing a passivation layer of a TOPCon battery, comprising the following steps:

[0057] S1, placing a graphite boat loaded with a plurality of N-type silicon wafers 1 into the chamber of a PECVD reactor tube, and then subjecting the chamber to a first vacuum treatment, preheating treatment, and leak detection treatment to obtain a reaction chamber for performing a PECVD reaction;

[0058] S2, introducing laughing gas into the reaction chamber to perform pre-deposition treatment and deposition treatment of the tunnel oxide layer 2 on multiple N-type silicon wafers 1, so that the back side of the multiple N-type silicon wafers 1 forms a tunnel oxide layer 2, and then the reaction chamber on which the deposition treatment of the tunnel oxide layer 2 is completed is vacuumed for a second time;

[0059] S3, introducing silane, hydrogen and phosphine into the reaction chamber after the second vacuum treatment, to perform pre-deposition treatment and deposition treatment of the first poly-Si layer 3 on the multiple N-type silicon wafers 1, so that the first poly-Si layer 3 is formed on the back side of the tunnel oxide layer 2, and then the reaction chamber after the deposition treatment of the first poly-Si layer 3 is vacuumed for the third time;

[0060] S4, introduces laughing gas into the reaction chamber that has completed the third vacuum treatment, performs pre-deposition treatment and deposition treatment on multiple N-type silicon wafers 1 of molecular sieve layer 4, so that the back side of the first poly-Si layer 3 forms molecular sieve layer 4, and then vacuumizes the reaction chamber that has completed the deposition treatment of molecular sieve layer 4 for the fourth time;

[0061] S5, introducing silane, hydrogen and phosphine into the reaction chamber that has completed the fourth vacuum treatment to perform a pre-deposition treatment and a deposition treatment of the second poly-Si layer 5 on the multiple N-type silicon wafers 1, so that the second poly-Si layer 5 is formed on the back side of the molecular sieve layer 4, and then the reaction chamber that has completed the deposition treatment of the second poly-Si layer 5 is vacuumed for the fifth time;

[0062] S6, introducing silane, hydrogen and phosphine into the reaction chamber that has completed the fifth vacuum treatment to perform a pre-deposition treatment and a deposition treatment of the third poly-Si layer 6 on the multiple N-type silicon wafers 1, so that the third poly-Si layer 6 is formed on the back side of the second poly-Si layer 5, and then the reaction chamber that has completed the deposition treatment of the third poly-Si layer 6 is vacuumed for the sixth time;

[0063] S7, introducing silane and laughing gas into the reaction chamber that has completed the sixth vacuum treatment, to perform pre-deposition treatment and deposition treatment of the mask layer 7 on the multiple N-type silicon wafers 1, so that the mask layer 7 is formed on the back side of the third poly-Si layer 6, and then the reaction chamber that has completed the deposition treatment of the mask layer 7 is vacuumed for the seventh time;

[0064] S8, introducing a purge gas into the reaction chamber that has completed the seven vacuum treatments to purge the reaction chamber, and then sending the graphite boat that has completed the purge treatment out of the PECVD reaction furnace tube to obtain the passivation layer of the prepared TOPCon battery.

[0065] By introducing nitrous oxide into the reaction chamber, a molecular sieve layer 4 is pre-deposited and deposited on multiple N-type silicon wafers 1, so that a molecular sieve layer 4 is formed on the back of the first poly-Si layer 3. Then, silane, hydrogen and phosphine are introduced into the reaction chamber to pre-deposit and deposit a third poly-Si layer 6 on the multiple N-type silicon wafers 1, so that a third poly-Si layer 6 is formed on the back of the second poly-Si layer 5. Compared with the structure of the passivation layer of the TOPCon cell in the prior art having a doped polysilicon film layer and a heavily doped polysilicon layer, the passivation layer of the TOPCon cell of the present invention adds a molecular sieve layer 4 and a third poly-Si layer 6, which significantly improves the phosphorus diffusion effect on the back of the N-type silicon wafer 1, improves the passivation effect and anti-PID performance of the TOPCon cell, reduces the recombination rate of carriers on the back of the N-type silicon wafer 1, reduces the metal contact recombination between the back metal electrode of the TOPCon cell and the N-type silicon wafer 1, improves the open circuit voltage factor, and improves the photoelectric conversion efficiency of the TOPCon cell.

[0066] Optionally, the S1, when implemented, includes:

[0067] S11, opening the furnace door of the PECVD reaction furnace tube, placing a graphite boat loaded with multiple N-type silicon wafers 1 into the cavity of the PECVD reaction furnace tube, and closing the furnace door;

[0068] S12, performing a first vacuum treatment on the cavity of the PECVD reaction furnace tube loaded with the quartz boat, so that the pressure inside the cavity is the bottom pressure value;

[0069] S13, preheating the cavity of the furnace tube so that the temperature range of the cavity is 435±15°C;

[0070] S14, performing a leak detection process on the cavity that has completed the preheating process to confirm that there is no gas leakage inside the cavity, thereby obtaining a reaction cavity for performing a PECVD reaction.

[0071] Specifically, the bottom pressure value in the present invention is 5Pa.

[0072] In a specific implementation, the cavity is subjected to a leak detection process. If there is no air leakage in the cavity, the system operates normally. If there is air leakage in the cavity, the leak point should be promptly checked and repaired.

[0073] Optionally, when S2 is implemented, it includes:

[0074] S21, introducing nitrous oxide (NNO) at a flow rate of 10,000 sccm / min into the reaction chamber while maintaining a reaction chamber temperature of 435±15° C. and controlling the pressure within the reaction chamber to be 1,800 mTorr, and performing a tunneling oxide layer 2 pre-deposition treatment on a plurality of N-type silicon wafers 1 using the NNO. The tunneling oxide layer 2 pre-deposition treatment lasts for 30 seconds.

[0075] S22, performing a first glow discharge treatment on the plurality of N-type silicon wafers 1 that have undergone a pre-deposition treatment of the tunnel oxide layer 2 using a radio frequency power supply, thereby performing a tunnel oxide layer 2 deposition treatment on the plurality of N-type silicon wafers 1, so that the tunnel oxide layer 2 is formed on the back surface of the plurality of N-type silicon wafers 1; wherein the tunnel oxide layer 2 deposition treatment time is 116 seconds;

[0076] S23, performing a second vacuuming process on the reaction chamber that has completed the first glow discharge, so as to extract the laughing gas in the reaction chamber out of the reaction chamber.

[0077] Specifically, the thickness of the tunnel oxide layer 2 in the present invention is 1.5 nm±0.5 nm.

[0078] Optionally, when S3 is implemented, it includes:

[0079] S31, under the condition that the reaction chamber temperature range is 435±15°C, silane with a flow rate of 3450 sccm / min, hydrogen with a flow rate of 11160 sccm / min, and phosphine with a flow rate of 295 sccm / min are introduced into the reaction chamber after the second vacuum treatment, and the pressure in the reaction chamber is controlled to 3050 mTorr. A first poly-Si layer 3 is pre-deposited on multiple N-type silicon wafers 1 using silane, hydrogen, and phosphine. The pre-deposition time of the first poly-Si layer 3 is 60 seconds.

[0080] S32, performing a second glow discharge treatment on the plurality of N-type silicon wafers 1 that have completed the pre-deposition treatment of the first poly-Si layer 3 using a radio frequency power supply, so as to deposit the first poly-Si layer 3 on the plurality of N-type silicon wafers 1, so as to form the first poly-Si layer 3 on the back side of the tunnel oxide layer 2; wherein the deposition time of the first poly-Si layer 3 is 100 seconds;

[0081] S33, performing a third vacuuming process on the reaction chamber that has completed the second glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

[0082] Optionally, when S4 is implemented, it includes:

[0083] S41, introducing nitrous oxide at a flow rate of 10,000 sccm / min into the reaction chamber after the third vacuuming process, while controlling the pressure inside the reaction chamber to 1,800 mTorr, and performing a pre-deposition treatment of a molecular sieve layer 4 on the plurality of N-type silicon wafers 1 using the nitrous oxide; wherein the pre-deposition treatment time of the molecular sieve layer 4 is 30 seconds;

[0084] S42, performing a third glow discharge treatment on the plurality of N-type silicon wafers 1 that have undergone the pre-deposition treatment of the molecular sieve layer 4 using a radio frequency power supply to deposit the molecular sieve layer 4 on the plurality of N-type silicon wafers 1, so that the molecular sieve layer 4 is formed on the back surface of the first poly-Si layer 3; wherein the deposition treatment time of the molecular sieve layer 4 is 120 seconds;

[0085] S43, performing a fourth vacuuming process on the reaction chamber that has completed the third glow discharge, so as to extract the laughing gas inside the reaction chamber out of the reaction chamber.

[0086] Optionally, when S5 is specifically implemented, it includes:

[0087] S51, under the condition that the reaction chamber temperature range is 435±15°C, silane with a flow rate of 3450 sccm / min, hydrogen with a flow rate of 10800 sccm / min, and phosphine with a flow rate of 460 sccm / min are introduced into the reaction chamber that has completed the fourth vacuum treatment, and the pressure in the reaction chamber is controlled to 3050 mTorr. A second poly-Si layer 5 is pre-deposited on the plurality of N-type silicon wafers 1 using silane, hydrogen, and phosphine. The pre-deposition time of the second poly-Si layer 5 is 30 seconds.

[0088] S52, performing a fourth glow discharge treatment on the plurality of N-type silicon wafers 1 that have undergone the pre-deposition treatment of the second poly-Si layer 5 using a radio frequency power supply, thereby performing a second poly-Si layer 5 deposition treatment on the plurality of N-type silicon wafers 1, so as to form a second poly-Si layer 5 on the back side of the molecular sieve layer 4; wherein the deposition treatment time of the second poly-Si layer 5 is 265 seconds;

[0089] S53, performing a fifth vacuuming process on the reaction chamber that has completed the fourth glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

[0090] Optionally, when S6 is implemented, it includes:

[0091] S61, under the condition that the reaction chamber temperature range is 435±15° C., silane at a flow rate of 3450 sccm / min, hydrogen at a flow rate of 10080 sccm / min, and phosphine at a flow rate of 1017 sccm / min are introduced into the reaction chamber that has completed the fifth vacuum treatment, and the pressure in the reaction chamber is controlled to be 3100 mTorr. A third poly-Si layer 6 is pre-deposited on the plurality of N-type silicon wafers 1 using silane, hydrogen, and phosphine. The pre-deposition time of the third poly-Si layer 6 is 60 seconds.

[0092] S62, performing a fifth glow discharge treatment on the plurality of N-type silicon wafers 1 that have undergone the pre-deposition treatment of the third poly-Si layer 6 using a radio frequency power supply, thereby performing a deposition treatment of the third poly-Si layer 6 on the plurality of N-type silicon wafers 1, so that the third poly-Si layer 6 is formed on the back surface of the second poly-Si layer 5; wherein the deposition treatment time of the third poly-Si layer 6 is 212 seconds;

[0093] S63, performing a sixth vacuuming process on the reaction chamber that has completed the fifth glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

[0094] Optionally, when S7 is implemented, it includes:

[0095] S71, under the condition that the reaction chamber temperature range is 435±15° C., introducing silane at a flow rate of 1622 sccm / min and nitrous oxide at a flow rate of 7084 sccm / min into the reaction chamber that has completed the sixth vacuum treatment, and controlling the pressure inside the reaction chamber to 1750 mTorr, performing a pre-deposition treatment of a mask layer 7 on multiple N-type silicon wafers 1 using the silane and nitrous oxide; wherein the pre-deposition treatment time of the mask layer 7 is 30 seconds;

[0096] S72, performing a sixth glow discharge treatment on the plurality of N-type silicon wafers 1 that have undergone the pre-deposition treatment of the mask layer 7 using a radio frequency power supply, thereby depositing the mask layer 7 on the plurality of N-type silicon wafers 1, so that the mask layer 7 is formed on the back surface of the third poly-Si layer 6; wherein the deposition time of the mask layer 7 is 60 seconds;

[0097] S73, performing a seventh vacuuming process on the reaction chamber that has completed the sixth glow discharge, so as to extract the silane and nitrous oxide inside the reaction chamber out of the reaction chamber.

[0098] Optionally, when S8 is specifically implemented, it includes:

[0099] S81, introducing a purge gas into the reaction chamber that has completed the seventh vacuuming process to purge the reaction chamber so that the pressure in the reaction chamber returns to atmospheric pressure;

[0100] S82, after the purge treatment is completed, the furnace door of the PECVD reaction furnace tube is opened, the graphite boat loaded with multiple N-type silicon wafers 1 is sent out of the reaction chamber, and the furnace door is closed to obtain the prepared passivation layer of the TOPCon battery.

[0101] Specifically, the purge gas in the present invention can be nitrogen or other inert gases commonly used in the prior art.

[0102] The present invention also provides a passivation layer of a TOPCon battery, which is prepared by the above-mentioned method for preparing a passivation layer of a TOPCon battery, such as Figure 2 As shown, the passivation layer of the TOPCon cell includes an N-type silicon wafer 1 and a tunneling oxide layer 2, a first poly-Si layer 3, a molecular sieve layer 4, a second poly-Si layer 5, a third poly-Si layer 6 and a mask layer 7 sequentially formed on the back of the N-type silicon wafer 1; the total thickness of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5 and the third poly-Si layer 6 is 99.5nm±2nm.

[0103] Specifically, the total thickness of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5 and the third poly-Si layer 6 in the present invention is 99.5nm±2nm. The passivation layer structure of the TOPCon battery in the prior art is a tunneling oxide layer, a first poly-Si layer and a second poly-Si layer, wherein the thickness of the tunneling oxide layer in the prior art is 1.5nm, and the total thickness of the first poly-Si layer and the second poly-Si layer is 102.37nm±2nm; therefore, when preparing the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5 and the third poly-Si layer 6, the present invention controls the time of the pre-deposition treatment and the deposition treatment by changing the gas flow rate introduced into the reaction chamber to achieve thinning of the thickness of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5 and the third poly-Si layer 6, thereby further improving the passivation performance and photoelectric conversion efficiency of the TOPCon battery.

[0104] In order to verify the beneficial effects achieved by the method for preparing the passivation layer of the TOPCon battery provided by the present invention, four passivation layers prepared in Example 1, Example 2, Example 3 and the comparative example are specially set up, and the preparation of the TOPCon battery is continued on the basis of the four passivation layers to obtain four TOPCon batteries, and then the electrical performance of the four TOPCon batteries is tested, and the test results are compared.

[0105] Example 1 is a method for preparing a passivation layer of a TOPCon battery provided by the present invention. The passivation layer obtained is recorded as a first passivation layer. The preparation of a TOPCon battery is completed on the basis of the first passivation layer to obtain a first TOPCon battery. The specific process of preparing the first TOPCon battery is as follows:

[0106] 1. Perform double-sided texturing, front-side boron diffusion, front-side SE treatment, double-sided oxidation, and back-side BSG removal alkaline polishing on the N-type silicon wafer 1 in sequence;

[0107] 2. The front side of the N-type silicon wafer 1 after the back side BSG removal and alkaline polishing is subjected to the prior art method for preparing a passivation layer of a TOPCon cell to form a passivation layer on the front side of the N-type silicon wafer 1. The back side of the N-type silicon wafer 1 is subjected to the method for preparing a passivation layer of a TOPCon cell provided by the present invention to form a tunneling oxide layer 2, a first poly-Si layer 3, a molecular sieve layer 4, a second poly-Si layer 5, a third poly-Si layer 6, and a mask layer 7 on the back side of the N-type silicon wafer 1.

[0108] 3. Annealing the N-type silicon wafer 1 on which the passivation layer is prepared, converting the amorphous silicon layer in the passivation layer on the front side of the N-type silicon wafer 1 formed by the preparation method of the passivation layer of the TOPCon battery provided by the prior art into a polycrystalline silicon layer at a high temperature, and converting the first poly-Si layer 3, the second poly-Si layer 5, and the third poly-Si layer 6 on the back side of the N-type silicon wafer 1 formed by the preparation method provided by the present invention into a first poly-Si polycrystalline silicon layer, a second poly-Si polycrystalline silicon layer, and a third poly-Si polycrystalline silicon layer;

[0109] 4. Perform RCA cleaning on the annealed N-type silicon wafer 1 to remove the mask layer 7;

[0110] 5. The N-type silicon wafer 1 that has completed the RCA cleaning process is sequentially subjected to front-side aluminum oxide coating, front-side anti-reflection coating, and back-side anti-reflection coating, so that the front side of the passivation layer on the front side of the N-type silicon wafer 1 is sequentially formed with a front-side aluminum oxide film layer and a front-side anti-reflection film layer, and the back side of the third poly-Si layer 6 on the back side of the N-type silicon wafer 1 is formed with a back-side anti-reflection film layer;

[0111] 6. Performing a screen sintering process on the N-type silicon wafer 1 after the back side anti-reflection film coating process, so that the front side of the front silicon oxide film layer forms a front metal electrode, and the back side of the back silicon oxide film layer forms a back metal electrode;

[0112] 7. Perform light injection processing on the N-type silicon wafer 1 that has completed the screen sintering process, thereby completing the preparation of the first TOPCon cell.

[0113] The difference between Example 2 and Example 1 is that step S5 is missing, that is, the pre-deposition treatment, deposition treatment and fifth vacuum treatment of the third poly-Si layer 6 are missing; in Example 2, when the tunneling oxide layer 2 is deposited, the deposition treatment time is 122s; when the first poly-Si layer 3 is pre-deposited, the pressure inside the reaction chamber is controlled to be 3100mTorr; when the first poly-Si layer 3 is deposited, the deposition treatment time of the first poly-Si layer 3 is 110s; when the molecular sieve layer 4 is deposited, the deposition treatment time of the molecular sieve layer 4 is 122s; when the second poly-Si layer 5 is pre-deposited, the flow rate of hydrogen is 10080sccm / min, the flow rate of phosphine is 345sccm / min, and the pressure inside the reaction chamber is controlled to be 3100mTorr; when the second poly-Si layer 5 is deposited, the deposition treatment time of the second poly-Si layer 5 is 550s;

[0114] The passivation layer prepared in Example 2 is recorded as the second passivation layer. On the basis of the second passivation layer, the second TOPCon cell is prepared according to the preparation method of the first TOPCon cell. The total thickness of the first poly-Si layer 3, the molecular sieve layer 4, and the second poly-Si layer 5 in the second passivation layer is 103.65 nm.

[0115] The difference between Example 3 and Example 1 is that when the tunnel oxide layer 2 is deposited, the deposition time is 122s; when the first poly-Si layer 3 is pre-deposited, the pressure inside the reaction chamber is controlled to be 3100mTorr; when the first poly-Si layer 3 is deposited, the deposition time of the first poly-Si layer 3 is 110s; when the molecular sieve layer 4 is deposited, the deposition time of the molecular sieve layer 4 is 122s; when the second poly-Si layer 5 is pre-deposited, the hydrogen The flow rate of phosphine is 11160 sccm / min, the flow rate of phosphine is 400 sccm / min, and the pressure inside the reaction chamber is controlled to be 3100 mTorr; when the second poly-Si layer 5 is deposited, the deposition time of the second poly-Si layer 5 is 300 s; when the third poly-Si layer 6 is pre-deposited, the flow rate of phosphine is 400 sccm / min; when the third poly-Si layer 6 is deposited, the deposition time of the third poly-Si layer 6 is 240 s;

[0116] The passivation layer prepared in Example 3 is recorded as the third passivation layer. On the basis of the third passivation layer, the third TOPCon cell is prepared according to the preparation method of the first TOPCon cell. The total thickness of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5 and the third poly-Si layer 6 in the third passivation layer is 107.15nm±2nm.

[0117] The comparative example shows a conventional method for preparing a passivation layer for a TOPCon cell. The resulting passivation layer is designated as a fourth passivation layer. Based on the fourth passivation layer, a fourth TOPCon cell is prepared according to the method for preparing the first TOPCon cell. The combined thickness of the doped polysilicon layer and the heavily doped polysilicon layer in the fourth passivation layer is 102.37 nm ± 2 nm.

[0118] The comparison of the electrical performance test results of the first TOPCon battery, the second TOPCon battery, the third TOPCon battery and the fourth TOPCon battery is shown in Table 1 below.

[0119] Table 1

[0120] Group Eta / % Uoc / V Isc / A FF / % Rs / Ω Rsh / Ω IRev2 / A The first TOPCon battery 26.09 0.7328 13.7788 86.48 0.001 1358 0.04 Second TOPCon battery 26.01 0.7323 13.757 86.41 0.001 1272 0.07 Third TOPCon battery 26.06 0.7315 13.8042 86.38 0.001 1471 0.05 Fourth TOPCon battery 25.95 0.7277 13.824 86.34 0.001 1172 0.11

[0121] As shown in Table 1, on the basis of the fourth passivation layer obtained by the preparation method of the passivation layer of the TOPCon battery in the prior art, a molecular sieve layer 4 and a third poly-Si layer 6 are added to obtain a first passivation layer, and by changing the gas flow rate introduced into the reaction chamber and controlling the time of the pre-deposition treatment and the deposition treatment, the thicknesses of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5, and the third poly-Si layer 6 are all reduced, so that the electrical performance data of the first TOPCon battery are significantly improved;

[0122] By adding a molecular sieve layer 4 to the fourth passivation layer to obtain a second passivation layer, the electrical performance of the second TOPCon cell is improved compared to the electrical performance data of the fourth TOPCon cell, but is lower than the improvement effect of the electrical performance data of the first TOPCon cell;

[0123] The third passivation layer is obtained by adding a molecular sieve layer 4 and a third poly-Si layer 6 on the basis of the fourth passivation layer, but the thickness of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5, and the third poly-Si layer 6 are not thinned, so that the electrical performance data of the third TOPCon battery are improved compared with the electrical performance data of the second TOPCon battery and the electrical performance data of the fourth TOPCon battery, but are lower than the electrical performance data of the first TOPCon battery.

[0124] Therefore, if a molecular sieve layer 4 and a third poly-Si layer 6 are added to the passivation layer obtained by the preparation method of the passivation layer of the TOPCon cell provided by the prior art, the passivation performance and photoelectric conversion efficiency of the TOPCon cell can be significantly improved. If the thickness of the first poly-Si layer 3, the molecular sieve layer 4, the second poly-Si layer 5, and the third poly-Si layer 6 are thinned, the absorption of light by the TOPCon cell can be improved, and the photoelectric conversion efficiency of the TOPCon cell can be further improved.

[0125] In summary, the passivation layer obtained by the preparation method of the passivation layer of the TOPCon battery provided by the present invention can significantly improve the phosphorus diffusion effect on the back side of the N-type silicon wafer 1, reduce the recombination of carriers on the back side of the N-type silicon wafer 1, reduce the metal contact recombination between the back metal electrode of the TOPCon battery and the N-type silicon wafer 1, improve the open circuit voltage factor, and significantly improve the passivation performance and photoelectric conversion efficiency of the TOPCon battery prepared by the passivation layer provided by the present invention.

[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a passivation layer of a TOPCon battery, characterized in that: The following steps are involved: S1, placing a graphite boat loaded with a plurality of N-type silicon wafers (1) into the cavity of a PECVD reaction furnace tube, and then subjecting the cavity to a first vacuum treatment, a preheating treatment, and a leak detection treatment, so as to obtain a reaction cavity for performing a PECVD reaction; S2, introducing laughing gas into the reaction chamber to perform a pre-deposition process and a deposition process of the tunneling oxide layer (2) on the plurality of N-type silicon wafers (1), so that the back sides of the plurality of N-type silicon wafers (1) all form the tunneling oxide layer (2), and then performing a second vacuuming process on the reaction chamber after the deposition process of the tunneling oxide layer (2); S3, introducing silane, hydrogen and phosphine into the reaction chamber that has completed the second vacuum treatment, to perform a pre-deposition treatment and a deposition treatment of the first poly-Si layer (3) on the plurality of N-type silicon wafers (1), so that the first poly-Si layer (3) is formed on the back side of the tunnel oxide layer (2), and then performing a third vacuum treatment on the reaction chamber that has completed the deposition treatment of the first poly-Si layer (3); S4, introducing laughing gas into the reaction chamber that has completed the third vacuum treatment, to perform a pre-deposition treatment and a deposition treatment of the molecular sieve layer (4) on the plurality of N-type silicon wafers (1), so that the molecular sieve layer (4) is formed on the back side of the first poly-Si layer (3), and then performing a fourth vacuum treatment on the reaction chamber that has completed the deposition treatment of the molecular sieve layer (4); S5, introducing silane, hydrogen and phosphine into the reaction chamber that has completed the fourth vacuum treatment to perform a pre-deposition treatment and a deposition treatment of the second poly-Si layer (5) on the plurality of N-type silicon wafers (1), so that the second poly-Si layer (5) is formed on the back side of the molecular sieve layer (4), and then performing a fifth vacuum treatment on the reaction chamber that has completed the deposition treatment of the second poly-Si layer (5); S6, introducing silane, hydrogen and phosphine into the reaction chamber that has completed the fifth vacuum treatment to perform a pre-deposition treatment and a deposition treatment of a third poly-Si layer (6) on the plurality of N-type silicon wafers (1), so that a third poly-Si layer (6) is formed on the back side of the second poly-Si layer (5), and then performing a sixth vacuum treatment on the reaction chamber that has completed the deposition treatment of the third poly-Si layer (6); S7, introducing silane and laughing gas into the reaction chamber that has completed the sixth vacuum treatment, to perform a pre-deposition treatment and a deposition treatment of a mask layer (7) on the plurality of N-type silicon wafers (1), so that a mask layer (7) is formed on the back side of the third poly-Si layer (6), and then performing a seventh vacuum treatment on the reaction chamber that has completed the deposition treatment of the mask layer (7); S8, introducing a purge gas into the reaction chamber that has completed seven vacuum treatments to purge the reaction chamber, and then sending the graphite boat that has completed the purge treatment out of the PECVD reaction furnace tube to obtain the passivation layer of the prepared TOPCon battery.

2. The method for preparing a passivation layer of a TOPCon battery according to claim 1, characterized in that: When S1 is specifically implemented, it includes: S11, opening the furnace door of the PECVD reaction furnace tube, placing a graphite boat loaded with a plurality of N-type silicon wafers (1) into the cavity of the PECVD reaction furnace tube, and closing the furnace door; S12, performing a first vacuum treatment on the cavity of the PECVD reaction furnace tube with the quartz boat loaded therein, so that the gas pressure inside the cavity is the bottom pressure value; S13, preheating the cavity of the furnace tube so that the temperature range of the cavity is 435±15°C; S14, performing a leak detection process on the cavity that has completed the preheating process to confirm that there is no leakage inside the cavity, thereby obtaining a reaction cavity for performing a PECVD reaction.

3. A method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S2 is specifically implemented, it includes: S21, under the condition that the temperature range of the reaction chamber is 435±15° C., nitrous oxide at a flow rate of 10000 sccm / min is introduced into the reaction chamber, and the pressure inside the reaction chamber is controlled to be 1800 mTorr, and a tunneling oxide layer (2) pre-deposition treatment is performed on a plurality of N-type silicon wafers (1) using nitrous oxide; wherein the tunneling oxide layer (2) pre-deposition treatment time is 30 seconds; S22, performing a first glow discharge treatment on the plurality of N-type silicon wafers (1) that have completed the pre-deposition treatment of the tunneling oxide layer (2) by means of a radio frequency power supply, so as to perform a deposition treatment of the tunneling oxide layer (2) on the plurality of N-type silicon wafers (1), so that a tunneling oxide layer (2) is formed on the back side of the plurality of N-type silicon wafers (1); wherein the deposition treatment time of the tunneling oxide layer (2) is 116 seconds; S23, performing a second vacuuming process on the reaction chamber that has completed the first glow discharge, so as to extract the laughing gas in the reaction chamber out of the reaction chamber.

4. A method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S3 is specifically implemented, it includes: S31, under the condition that the temperature range of the reaction chamber is 435±15°C, silane with a flow rate of 3450sccm / min, hydrogen with a flow rate of 11160sccm / min and phosphine with a flow rate of 295sccm / min are introduced into the reaction chamber that has completed the second vacuum treatment, and the pressure inside the reaction chamber is controlled to be 3050mTorr, and a first poly-Si layer (3) is pre-deposited on multiple N-type silicon wafers (1) using silane, hydrogen and phosphine; wherein the pre-deposition time of the first poly-Si layer (3) is 60s; S32, performing a second glow discharge treatment on the plurality of N-type silicon wafers (1) that have completed the pre-deposition treatment of the first poly-Si layer (3) by using a radio frequency power supply, so as to perform a deposition treatment of the first poly-Si layer (3) on the plurality of N-type silicon wafers (1), so as to form the first poly-Si layer (3) on the back side of the tunnel oxide layer (2); wherein the deposition treatment time of the first poly-Si layer (3) is 100 seconds; S33, performing a third vacuuming process on the reaction chamber that has completed the second glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

5. The method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S4 is specifically implemented, it includes: S41, under the condition that the temperature of the reaction chamber is in the range of 435±15°C, introducing nitrous oxide at a flow rate of 10000 sccm / min into the reaction chamber that has completed the third vacuum treatment, and controlling the pressure inside the reaction chamber to be 1800 mTorr, performing a pre-deposition treatment of a molecular sieve layer (4) on a plurality of N-type silicon wafers (1) using nitrous oxide; wherein the pre-deposition treatment time of the molecular sieve layer (4) is 30 seconds; S42, performing a third glow discharge treatment on the plurality of N-type silicon wafers (1) that have completed the pre-deposition treatment of the molecular sieve layer (4) by means of a radio frequency power supply, so as to perform a deposition treatment of the molecular sieve layer (4) on the plurality of N-type silicon wafers (1), so that a molecular sieve layer (4) is formed on the back side of the first poly-Si layer (3); wherein the deposition treatment time of the molecular sieve layer (4) is 120 seconds; S43, performing a fourth vacuuming process on the reaction chamber that has completed the third glow discharge, so as to extract the laughing gas in the reaction chamber out of the reaction chamber.

6. A method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S5 is specifically implemented, it includes: S51, under the condition that the temperature range of the reaction chamber is 435±15°C, silane with a flow rate of 3450sccm / min, hydrogen with a flow rate of 10800sccm / min and phosphine with a flow rate of 460sccm / min are introduced into the reaction chamber that has completed the fourth vacuum treatment, and the pressure inside the reaction chamber is controlled to be 3050mTorr, and a second poly-Si layer (5) is pre-deposited on multiple N-type silicon wafers (1) using silane, hydrogen and phosphine; wherein the pre-deposition time of the second poly-Si layer (5) is 30s; S52, performing a fourth glow discharge treatment on the plurality of N-type silicon wafers (1) that have completed the pre-deposition treatment of the second poly-Si layer (5) by using a radio frequency power supply, so as to perform a deposition treatment of the second poly-Si layer (5) on the plurality of N-type silicon wafers (1), so as to form a second poly-Si layer (5) on the back side of the molecular sieve layer (4); wherein the deposition treatment time of the second poly-Si layer (5) is 265 seconds; S53, performing a fifth vacuuming process on the reaction chamber that has completed the fourth glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

7. A method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S6 is specifically implemented, it includes: S61, under the condition that the temperature range of the reaction chamber is 435±15°C, silane with a flow rate of 3450sccm / min, hydrogen with a flow rate of 10080sccm / min and phosphine with a flow rate of 1017sccm / min are introduced into the reaction chamber that has completed the fifth vacuum treatment, and the pressure inside the reaction chamber is controlled to be 3100mTorr, and a third poly-Si layer (6) is pre-deposited on multiple N-type silicon wafers (1) using silane, hydrogen and phosphine; wherein the pre-deposition time of the third poly-Si layer (6) is 60s; S62, performing a fifth glow discharge treatment on the plurality of N-type silicon wafers (1) that have completed the pre-deposition treatment of the third poly-Si layer (6) by using a radio frequency power supply, so as to perform a deposition treatment of the third poly-Si layer (6) on the plurality of N-type silicon wafers (1), so as to form a third poly-Si layer (6) on the back side of the second poly-Si layer (5); wherein the deposition treatment time of the third poly-Si layer (6) is 212 seconds; S63, performing a sixth vacuuming process on the reaction chamber that has completed the fifth glow discharge, so as to extract the silane, hydrogen and phosphine in the reaction chamber out of the reaction chamber.

8. A method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S7 is specifically implemented, it includes: S71, under the condition that the temperature range of the reaction chamber is 435±15°C, silane with a flow rate of 1622 sccm / min and nitrous oxide with a flow rate of 7084 sccm / min are introduced into the reaction chamber that has completed the sixth vacuum treatment, and the pressure inside the reaction chamber is controlled to be 1750 mTorr, and a mask layer (7) is pre-deposited on a plurality of N-type silicon wafers (1) using silane and nitrous oxide; wherein the pre-deposition time of the mask layer (7) is 30 seconds; S72, performing a sixth glow discharge treatment on the plurality of N-type silicon wafers (1) that have completed the pre-deposition treatment of the mask layer (7) by using a radio frequency power supply, so as to perform a deposition treatment of the mask layer (7) on the plurality of N-type silicon wafers (1), so as to form a mask layer (7) on the back side of the third poly-Si layer (6); wherein the deposition treatment time of the mask layer (7) is 60 seconds; S73, performing a seventh vacuuming treatment on the reaction chamber that has completed the sixth glow discharge, so as to extract the silane and laughing gas in the reaction chamber out of the reaction chamber.

9. A method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 or 2, characterized in that: When S8 is specifically implemented, it includes: S81, introducing a purge gas into the reaction chamber that has completed the seventh vacuuming process to purge the reaction chamber, so that the gas pressure in the reaction chamber is restored to the atmospheric pressure; S82, after the purging treatment is completed, the furnace door of the PECVD reaction furnace tube is opened, the graphite boat loaded with multiple N-type silicon wafers (1) is sent out of the reaction chamber, and the furnace door is closed to obtain the passivation layer of the prepared TOPCon battery.

10. A passivation layer of a TOPCon battery, prepared by the method for preparing a passivation layer of a TOPCon battery according to any one of claims 1 to 9, characterized in that: The passivation layer of the TOPCon cell comprises: An N-type silicon wafer (1) and a tunneling oxide layer (2), a first poly-Si layer (3), a molecular sieve layer (4), a second poly-Si layer (5), a third poly-Si layer (6) and a mask layer (7) formed in sequence on the back side of the N-type silicon wafer (1); The total thickness of the first poly-Si layer (3), the molecular sieve layer (4), the second poly-Si layer (5) and the third poly-Si layer (6) is 99.5 nm ± 2 nm.