Negative active material, negative slurry and negative plate

By using the grading and carbon coating of silicon particles and carbon particles in the negative electrode material of lithium-ion batteries, the structural stress problem caused by silicon expansion is solved, the cycle performance and safety of the battery are improved, and the efficient and stable battery is achieved Sex and safety.

CN119092656APending Publication Date: 2024-12-06JIANGSU RELIANCE ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410662534.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The expansion of silicon in the negative electrode material of lithium-ion batteries leads to increased structural stress, which may cause problems such as plating shedding, interface instability, by-product generation and reduced battery safety performance.

Method used

By using grading of silicon particles and carbon particles in the negative electrode active material and combining carbon coating treatment, the conductivity and stability of silicon particles are optimized, grain expansion caused by lithium ion embedding is reduced, and the film formation integrity of SEI film is improved. .

Benefits of technology

It significantly reduces stress, prevents silicon expansion from damage to the battery, improves the cycle performance and safety of the battery, and ensures the battery's capacity retention rate and thermal test after 600 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092656A_ABST
    Figure CN119092656A_ABST
Patent Text Reader

Abstract

The first aspect of the invention provides a negative electrode active material which comprises the following components in percentage by weight: 2-30% of silicon particles and the balance of carbon particles, wherein the average particle size of the silicon particles is D1, the average particle size of the carbon particles is D2, and the ratio a of D1 to D2 is more than 0.5 and less than or equal to 0.95; the silicon particles are subjected to carbon coating treatment, and the material used in the carbon coating treatment is amorphous carbon and / or carbon nanotubes; wherein the ID / IG of the amorphous carbon is not greater than 1.0, and the length-diameter ratio b of the carbon nanotube is greater than or equal to 120 and less than or equal to 13000. Based on the negative electrode active material, a second aspect and a third aspect of the invention respectively provide a negative electrode slurry and a negative electrode plate. By forming grading between the silicon particles and the carbon particles, concentrated stress generated on the periphery by volume change of the silicon particles is effectively avoided, and further damage to the battery caused by silicon expansion is prevented; by coating the silicon particles, the conductivity and the stability of the silicon particles are improved, and the performance and the safety of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a negative electrode active material, a negative electrode slurry and a negative electrode sheet. Background Art

[0002] According to the packaging form, lithium batteries can be divided into three forms: square, cylindrical and soft pack. Among them, cylindrical lithium batteries have gradually become a hot spot in lithium battery research due to their good consistency, high production efficiency, and strong heat dissipation capacity at the system level. Cylindrical batteries are usually packaged in a cylindrical steel shell, and the cap is located on the top of the battery. The inside of the steel shell is used to accommodate the battery core, which is formed by winding the positive electrode sheet, the negative electrode sheet and the separator between the two. The negative electrode sheet includes a coated area and an uncoated area. The coated area is coated with negative electrode slurry, and the uncoated area is the negative electrode ear.

[0003] It is common to introduce silicon materials into the negative electrode slurry currently used. Silicon has a high theoretical specific capacity and specific energy density. Therefore, when silicon is used as the electrode material of the battery, it can achieve a higher ability to embed and de-embed lithium ions, thereby improving the energy storage capacity of the battery. However, when silicon embeds lithium ions, the grains will expand. This is because the lithium ions enter the silicon lattice, causing the volume of silicon to increase. If the volume change is too large, it may have an adverse effect on the structure and performance of the battery. First, the interior of the cylindrical battery will be subjected to great stress. Under the action of stress, the steel shell will deform to a certain extent, causing its structure to become unstable, especially the inner surface layer, which is easy to cause the coating to fall off, thereby causing iron dissolution. In addition, the expansion of silicon is easy to cause interface instability, thereby increasing the decomposition of the electrolyte and increasing the generation of by-products. Some of these processes will also be accompanied by an increase in the acidity of the electrolyte, thereby indirectly increasing the interface side reactions of the positive electrode and causing the dissolution of transition elements in the positive electrode. A large amount of iron elements and transition metals of the positive electrode are dissolved and deposited on various parts of the cylindrical battery, such as pole pieces, diaphragms, etc. Among them, the deposition at the negative electrode will further damage the SEI film of the negative electrode and reduce the safety performance of the battery cell, such as thermal storage, overcharging, etc. In addition, some elements will be reduced at the negative electrode to form metal particles or even dendrites, which will pierce the diaphragm and cause the battery cell to short-circuit. Summary of the invention

[0004] To solve the above problems, the first aspect of the present invention provides a negative electrode active material, which includes 2-30% silicon particles and the rest carbon particles by weight percentage; wherein the average particle size of the silicon particles is D1, the average particle size of the carbon particles is D2, and the ratio a of D1 to D2 satisfies, 0.5<a≤0.95; preferably, the silicon particles are carbon-coated, and the materials used for the carbon coating are amorphous carbon and carbon nanotubes; wherein the ID / IG of the amorphous carbon is not greater than 1.0, and the aspect ratio b of the carbon nanotubes satisfies, 120≤b≤13000.

[0005] In some embodiments, the silicon particles include at least first silicon particles with an average particle size of D3 and second silicon particles with an average particle size of D4, D3≤5μm≤D4, the ratio c of D4 to D3 satisfies, 1.2≤c≤3, and the weight ratio of the first silicon particles to the second silicon particles is (0.2-3):1.

[0006] In some embodiments, a, b, and c satisfy 0.4<1000a*c / (b)≤15.

[0007] In some embodiments, the silicon particles are elemental silicon and / or silicon oxide; the carbon particles are selected from a mixture of one or more of artificial graphite, natural graphite, hard carbon, and soft carbon.

[0008] In some embodiments, the carbon coating process comprises the following steps:

[0009] a. Raise the temperature of silicon particles to 400-800°C in a nitrogen atmosphere, then introduce acetylene gas at 0.1-1L / hour for 4-8h;

[0010] b. Continue to introduce propylene gas at 0.1-1L / hour and react for 12-36h;

[0011] c. Stop passing acetylene and propylene gas, turn off heating, maintain nitrogen atmosphere and cool to below 30°C, take out the material, and obtain amorphous carbon-coated silicon particles;

[0012] d. adding 0.01-0.1% of the mass of amorphous carbon-coated silicon particles to carbon nanotubes and mixing to obtain a mixture;

[0013] e. Add 0.3-1L ethanol and 0.01-0.1kg cellulose to each 1kg mixture and mix to obtain a slurry;

[0014] f. Drying, grinding and sieving the slurry to obtain amorphous carbon and carbon nanotube-coated silicon particles.

[0015] In some preferred embodiments, in the silicon particles coated with amorphous carbon and carbon nanotubes, the weight ratio of amorphous carbon to carbon nanotubes is (0.2-5):1.

[0016] The second aspect of the present invention provides a negative electrode slurry, in which the solid matter of the negative electrode slurry includes at least 0.5-2% conductive agent, 0.5-2% thickener, 0.5-2% binder, and the rest is the above-mentioned negative electrode active material; the above-mentioned solid matter is dispersed in deionized water to form a negative electrode slurry with a solid content of 30-50%.

[0017] The third aspect of the present invention provides a negative electrode sheet, comprising a negative electrode current collector, at least one surface of which is coated with the negative electrode slurry, and the coating area is 80-98% of the total area of ​​the negative electrode current collector.

[0018] The fourth aspect of the present invention provides a battery roll core, comprising a positive electrode sheet, the above-mentioned negative electrode sheet and a separator located therebetween; the battery roll core is formed by winding the positive electrode sheet, the negative electrode sheet and the separator; the diameter of the battery roll core is 20-60mm, the height is 60-200mm, and the ratio of height to diameter is greater than 1.7.

[0019] A fifth aspect of the present invention provides a cylindrical battery, comprising the above-mentioned battery roll core, a cap and a steel shell; the interior of the steel shell accommodates the battery roll core, and the top is sealed with a cap.

[0020] The present application effectively improves the uniformity of the negative electrode active material by forming a gradation between silicon particles and carbon particles and between silicon particles of different specifications, significantly reduces and disperses stress, avoids the volume change of silicon particles causing concentrated stress on the surrounding area, and prevents silicon expansion from causing further damage to the battery. The present application also improves the conductivity and stability of silicon particles by coating the silicon particles, enhances the film integrity of the SEI film, reduces the possibility of deposited metal forming dendrites on its surface, and improves battery performance and safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the description of the present application will be briefly introduced below.

[0022] Figure 1 It is a schematic diagram of the structure of the cylindrical battery in this application;

[0023] Figure 2 It is a schematic diagram of the structure of the battery roll core in this application;

[0024] Figure 3 It is a schematic diagram of the structure of the negative electrode sheet in this application.

[0025] Figure numerals: 1-cap, 2-steel shell, 21-battery roll core, 3-negative electrode sheet, 4-diaphragm, 5-positive electrode sheet, 6-coating area, 7-uncoated area. DETAILED DESCRIPTION

[0026] Examples of the present embodiment are described in detail below. The examples are only used to explain the present embodiment and are not to be construed as limiting the present embodiment.

[0027] In the description of this embodiment, "several" means one or more, "more" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0028] See also Figure 1 and Figure 2 The cylindrical battery is packaged in a cylindrical steel shell 2, and the cap 1 is located on the top of the battery. The interior of the steel shell 2 is used to accommodate a battery core 21, which is formed by winding a positive electrode sheet 5, a negative electrode sheet 3 and a separator 4. Figure 3 The negative electrode sheet includes a coating area 6 and an uncoating area 7. The coating area 6 is coated with negative electrode slurry, and the uncoating area 7 is a negative electrode ear.

[0029] In order to avoid the adverse effects of silicon expansion on the battery, the first aspect of the present invention provides a negative electrode active material, which includes 2-30% silicon particles and the rest carbon particles by weight; preferably, the weight percentage of silicon particles is 5-20%. By strictly controlling the amount of silicon particles added to the negative electrode active material, the grain expansion caused by lithium ions embedded in the silicon material is limited as a whole, and the battery capacity is increased as much as possible. When the proportion of silicon particles is too high, the silicon expansion phenomenon is difficult to be effectively controlled. Conversely, when the proportion of silicon particles is too low, the energy storage capacity of the battery decreases and cannot meet the use requirements.

[0030] In some embodiments, the silicon particles are elemental silicon and / or silicon oxide. Silicon has a high theoretical specific capacity and specific energy density, and can achieve a higher ability to embed and de-embed lithium ions, thereby improving the energy storage capacity of the battery. Embedding causes volume expansion, and de-embedding causes volume contraction. The elemental silicon in the present application can be a mixture of one or more of single crystal silicon, polycrystalline silicon, and amorphous silicon, and silicon oxide can be a commercially available silicon oxide product (SiO x , 0 <x≤2)。

[0031] In some embodiments, the carbon particles are selected from a mixture of one or more of artificial graphite, natural graphite, hard carbon, and soft carbon. In the selection of carbon particles, the principle is to meet the requirements of conductivity, stability, etc., and artificial graphite is preferred from the perspective of performance balance. Artificial graphite in this application refers to a graphite material manufactured by an artificial synthesis method, such as obtained by high temperature and high pressure treatment of carbon materials (such as graphite ore, coke, etc.) or chemical synthesis methods, with strong consistency in morphology and particle size distribution, and the structure can be in various forms, such as block, fibrous or powdered. Natural graphite in this application refers to graphite formed naturally in nature, mainly in the form of ores such as graphite schist, graphite gneiss, graphite-containing schist and metamorphic shale. Compared with natural graphite, artificial graphite has higher uniformity. Hard carbon in this application refers to carbon that is difficult to graphitize, which is usually obtained by thermal decomposition of high molecular polymers, such as resin carbon, organic polymer pyrolytic carbon and carbon black. The soft carbon in the present application refers to easily graphitized carbon, that is, amorphous carbon that can be graphitized at a high temperature above 2500° C. Common soft carbons include petroleum coke, needle coke, carbon fiber, carbon microspheres, and the like.

[0032] In some embodiments, the average particle size of the silicon particles is D1, the average particle size of the carbon particles is D2, and the ratio a of D1 to D2 satisfies 0.5<a≤0.95; preferably, 2μm≤D1≤9μm, 6μm≤D2≤18μm. The lithium ion diffusion coefficient of silicon particles is smaller than that of carbon particles, and the conductivity is poor. Appropriately reducing the particle size of silicon particles can effectively balance the impedance and form a more balanced performance. In addition, the presence of a certain particle size difference between silicon particles and carbon particles helps the two to mix more evenly, reduces the gap between particles, helps to reduce and disperse stress, and avoids excessive concentration of stress caused by volume expansion and further damage. When the particle size ratio of silicon particles to carbon particles is below 0.95, good cycle and safety performance are exhibited; when the ratio is too large, the carbon particles are too small to disperse stress for the silicon particles, thereby deteriorating the cycle and safety, and also reducing the conductivity of the negative electrode sheet and increasing the internal resistance of the battery.

[0033] In some embodiments, the silicon particles include at least first silicon particles with an average particle size of D3 and second silicon particles with an average particle size of D4, D3≤5μm≤D4, and the weight ratio of the first silicon particles to the second silicon particles is (0.2-3):1; preferably, the ratio c of D4 to D3 satisfies 1.2≤c≤3. When the ratio of silicon particles of two particle sizes is at a suitable level, the filling effect of the particles can be further optimized, and their expansion stress can be scientifically dispersed to obtain better performance. On the basis of mixing silicon particles and carbon particles of different particle sizes, the grading of silicon particles is introduced, and at least three levels of grading can be formed in the negative electrode active material, which greatly improves the uniformity of the negative electrode active material and helps to balance the various performances of the battery. However, when some particles are too small or too large, the cycle and safety performance will be deteriorated. Excessive grading can also cause a decrease in battery performance. This is because the gaps between the particles will be reduced due to the grading, resulting in insufficient penetration and infiltration of the electrolyte, which in turn damages the dynamic performance of the battery. It can be understood that, based on actual needs, the first silicon particles and the second silicon particles can be the same type of silicon particles, such as both elemental silicon or both silicon oxide, or they can be different types of silicon particles, such as elemental silicon particles and silicon oxide particles, respectively. The "first" and "second" here are only descriptions for distinguishing silicon particles of different particle sizes.

[0034] In some embodiments, the silicon particles are carbon-coated silicon particles, and the material used for carbon coating is amorphous carbon and / or carbon nanotubes; wherein the ID / IG of amorphous carbon is not greater than 1.0, and the aspect ratio b of the carbon nanotubes satisfies 120≤b≤13000. In the present application, the ID / IG of amorphous carbon refers to the intensity ratio of the D-peak and the G-peak in the Raman spectrum, wherein I represents the intensity, and the D-peak represents the defects of the lattice. The larger the ID / IG value, the more defects there are in the carbon atom crystal. When a reasonable ID / IG carbon coating is used, a certain proportion of defects can ensure the conduction of electrons and ions; but when the ID / IG is too large, indicating that there are too many surface defects, it will induce too many side reactions, increase the ionic conductivity of the interface, and deteriorate the cycle performance. When the aspect ratio of carbon nanotubes is relatively large, they can provide better electronic conduction, improve circulation and safety. If they are too long, the coating effect will be poor. However, when the aspect ratio of carbon nanotubes is too low, they cannot provide effective bridging, and the conductive network will fail after the silicon particles expand, causing the circulation to deteriorate.

[0035] In some preferred embodiments, a, b, and c satisfy 0.4<1000a*c / (b)≤15. Within the range of satisfying this formula, the electrochemical performance of the negative electrode active material reaches a relatively good state, the expansion effect of the silicon material obtained by simultaneously coating the amorphous carbon and the carbon nanotubes can be greatly suppressed, and the lithium-ion cylindrical battery can achieve a longer cycle life and higher safety performance.

[0036] In some embodiments, the carbon coating process comprises the following steps:

[0037] a. Raise the temperature of silicon particles to 400-800°C in a nitrogen atmosphere, then introduce acetylene gas at 0.1-1L / hour for 4-8h;

[0038] b. Continue to introduce propylene gas at 0.1-1L / hour and react for 12-36h;

[0039] c. Stop passing acetylene and propylene gases, turn off heating, maintain nitrogen atmosphere and cool to below 30°C, take out the material, and obtain amorphous carbon-coated silicon particles.

[0040] Acetylene and propylene are two different coating gas sources. The amorphous carbon formed by them has different ID / IG. By controlling the coating ratio of the two gases, ID / IG can be adjusted. In addition, the gas concentration, coating temperature and time will cause changes in ID / IG.

[0041] Preferably, the carbon coating process further comprises the following steps:

[0042] d. adding 0.01-0.1% of the mass of amorphous carbon-coated silicon particles to carbon nanotubes and mixing to obtain a mixture;

[0043] e. Add 0.3-1L ethanol and 0.01-0.1kg cellulose to each 1kg mixture, and mix to obtain a slurry; wherein the cellulose includes but is not limited to methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose;

[0044] f. Drying, grinding and sieving the slurry to obtain amorphous carbon and carbon nanotube-coated silicon particles.

[0045] The coating optimization of silicon particles can further improve the interface stability and conductivity of silicon particles, thereby improving the film integrity of SEI film (Solid Electrolyte Interface, a passivation layer covering the surface of electrode materials formed during the first charge and discharge process of lithium-ion batteries), reducing the possibility of deposited metals being reduced on their surface to form dendrites, and improving the cycle and safety performance of the battery cell.

[0046] In some embodiments, in the silicon particles coated with amorphous carbon and carbon nanotubes, the weight ratio of amorphous carbon and carbon nanotubes is (0.2-5):1. The coating amount is generally obtained in two ways, one is to calculate based on the coating efficiency of the gas; the other is to measure the coated particles using a carbon-sulfur analyzer. Coating the surface of silicon particles with different forms of carbon can not only ensure that the surface of the material has excellent electronic conductivity, but also form a protective effect on the surface of the material. The conductivity of amorphous carbon is worse than that of carbon nanotubes, but it can better form a comprehensive wrapping of the surface, thereby improving the uniformity of the coating and further ensuring the protective effect. When there is too much amorphous carbon, the conductivity of the interface will be reduced, and the electronic conductivity of the material surface cannot be guaranteed. However, when there are too many carbon nanotubes, it is difficult to completely wrap the surface due to their tubular and bundle-like structures, which makes it easy for silicon to be exposed on the surface. The silicon particle raw materials will react with moisture and oxygen in the air during storage. After being prepared into batteries, the silicon particles will also have side reactions with the electrolyte. In other words, improper carbon coating treatment will have a serious negative impact on battery performance.

[0047] The second aspect of the present invention provides a negative electrode slurry, in which the solid matter of the negative electrode slurry includes at least 0.5-2% conductive agent, 0.5-2% thickener, 0.5-2% binder, and the rest is the negative electrode active material as described above; the above solid matter is dispersed in deionized water to form a negative electrode slurry with a solid content of 30-50%.

[0048] The third aspect of the present invention provides a negative electrode sheet, including a negative electrode current collector, wherein the negative electrode slurry is coated on at least one surface of the negative electrode current collector, and the coating area is 80-98% of the total area of ​​the negative electrode current collector. The negative electrode current collector is, for example, copper foil. In the present application, when one surface of the negative electrode current collector is coated with the negative electrode slurry, its total area is the single-sided area; when the two surfaces of the negative electrode current collector are coated with the negative electrode slurry, its total area is the double-sided area.

[0049] The fourth aspect of the present invention provides a battery roll core, comprising a positive electrode sheet, the above-mentioned negative electrode sheet and a separator located therebetween, wherein the battery roll core is formed by winding the positive electrode sheet, the negative electrode sheet and the separator. Preferably, the diameter of the roll core is 20-60 mm, the height is 60-200 mm, and the ratio of the height to the diameter is greater than 1.7.

[0050] The fifth aspect of the present invention provides a cylindrical battery, comprising the battery core, a cap and a steel shell, wherein the battery core is contained inside the steel shell and the top is sealed with a cap. The negative electrode active material is prepared into a negative electrode sheet, and the negative electrode sheet is assembled into a battery core, and finally assembled into a cylindrical battery. The preparation method is as follows:

[0051] (1) Making a positive electrode sheet: taking lithium nickel cobalt manganese oxide, a conductive agent, a binder and N-methyl-2-pyrrolidone (NMP solvent), mixing them evenly in a homogenizer, coating the slurry on the surface of an aluminum foil, and drying to obtain a positive electrode sheet;

[0052] (2) Making a negative electrode sheet: taking the above-mentioned negative electrode active material, conductive agent, thickener, binder and deionized water, mixing them evenly in a homogenizer, coating the slurry on the surface of copper foil, and drying to obtain a negative electrode sheet;

[0053] (3) preparing an electrolyte: dissolving a lithium salt in an organic solvent to prepare an electrolyte;

[0054] (4) Assembly: The positive electrode sheet and the negative electrode sheet are rolled separately, cut and die-cut according to size requirements, and then wound together with the separator to obtain a cylindrical battery core. The battery core tabs are welded to the electrical connecting sheet, loaded into the shell, and the electrolyte is injected, sealed, and formed to obtain a cylindrical battery.

[0055] The present invention will be further explained with reference to the following examples.

[0056] Example 1

[0057] Embodiment 1 provides a negative electrode active material, which includes 10% elemental silicon and the rest is artificial graphite by weight percentage. The average particle size D1 of the elemental silicon is 6.5 μm, and the elemental silicon is a combination of a first elemental silicon and a second elemental silicon in a weight ratio of 7:10, the average particle size D3 of the first elemental silicon is 3.5 μm, and the average particle size of the second elemental silicon is 9.3 μm; the average particle size of the artificial graphite is 9.7 μm. The elemental silicon and the artificial graphite are uniformly mixed to obtain the negative electrode active material.

[0058] The above-mentioned elemental silicon is subjected to carbon coating treatment as follows:

[0059] (1) Place the elemental silicon in a rotary furnace and bake it under vacuum for 24 hours;

[0060] (2) After baking, N2 was introduced, and the temperature was raised to 600°C at 5°C / min, and then acetylene gas was introduced at 0.5L / hour for 6h;

[0061] (3) Continue to introduce propylene gas at 0.5 L / h and react for 24 h;

[0062] (4) Stop the acetylene and propylene gases, turn off the heating, keep N2 gas flowing and cool down to below 30°C;

[0063] (5) taking out the material, adding carbon nanotubes according to 0.05% of the material weight, and mixing;

[0064] (6) adding 0.5 L of ethanol and 0.05 kg of carboxymethyl cellulose to every 1 kg of the above mixture, stirring and mixing to obtain a slurry;

[0065] (7) The slurry is taken out, dried, ground, and sieved to obtain coated elemental silicon.

[0066] By introducing acetylene and propylene gases, amorphous carbon is coated on the surface of elemental silicon, and the ID / IG of the amorphous carbon is 0.9. The aspect ratio of the carbon nanotubes used in the coating process is 2100. After the above carbon coating process, the weight ratio of the amorphous carbon and the carbon nanotubes coated on the surface of elemental silicon is 3:1.

[0067] Example 2

[0068] Example 2 provides a negative electrode active material, which differs from Example 1 in that the weight ratio of amorphous carbon and carbon nanotubes coated on the surface of elemental silicon is 5:1.

[0069] Example 3

[0070] Example 3 provides a negative electrode active material, which is different from Example 1 in that the weight ratio of amorphous carbon and carbon nanotubes coated on the surface of elemental silicon is 1:5.

[0071] Example 4

[0072] Example 4 provides a negative electrode active material, which is different from Example 1 in that the average particle size of the artificial graphite is 6.9 μm.

[0073] Example 5

[0074] Example 5 provides a negative electrode active material, which is different from Example 1 in that the average particle size of the artificial graphite is 7.9 μm.

[0075] Example 6

[0076] Example 6 provides a negative electrode active material, which differs from Example 1 in that the elemental silicon is a combination of a first elemental silicon and a second elemental silicon in a weight ratio of 1:5, the average particle size D3 of the first elemental silicon is 3.5 μm, and the average particle size of the second elemental silicon is 7.2 μm.

[0077] Example 7

[0078] Example 7 provides a negative electrode active material, which differs from Example 1 in that the elemental silicon is a combination of a first elemental silicon and a second elemental silicon in a weight ratio of 3:1, the average particle size D3 of the first elemental silicon is 5.7 μm, and the average particle size of the second elemental silicon is 7.4 μm.

[0079] Example 8

[0080] Example 8 provides a negative electrode active material, which is different from Example 1 in that the elemental silicon is replaced by silicon oxide (SiO), wherein the average particle size D1 of the silicon oxide is 6.6 μm, and the silicon oxide is a combination of a first silicon oxide and a second silicon oxide in a weight ratio of 7:10, the average particle size D3 of the first silicon oxide is 3.8 μm, and the average particle size of the second silicon oxide is 9.2 μm.

[0081] Example 9

[0082] Example 9 provides a negative electrode active material, which differs from Example 1 in that artificial graphite is replaced by natural graphite, and the average particle size of the natural graphite is 12.2 μm.

[0083] Example 10

[0084] Example 10 provides a negative electrode active material, which differs from Example 1 in that artificial graphite is replaced by hard carbon, and the average particle size of the hard carbon is 10.4 μm.

[0085] Embodiment 11

[0086] Example 11 provides a negative electrode active material, which differs from Example 1 in that, in the carbon coating treatment of elemental silicon, the ID / IG of the amorphous carbon is 1, and the aspect ratio of the carbon nanotube is 1990.

[0087] Example 12

[0088] Example 12 provides a negative electrode active material, which is different from Example 1 in that, in the carbon coating treatment of elemental silicon, the ID / IG of the amorphous carbon is 0.87, and the aspect ratio of the carbon nanotube is 120.

[0089] Embodiment 13

[0090] Example 13 provides a negative electrode active material, which differs from Example 1 in that the weight percentage of elemental silicon is 5%.

[0091] Embodiment 14

[0092] Example 14 provides a negative electrode active material, which differs from Example 1 in that the weight percentage of elemental silicon is 20%.

[0093] Embodiment 15

[0094] Example 15 provides a negative electrode active material, which differs from Example 1 in that the weight percentage of elemental silicon is 2%.

[0095] Example 16

[0096] Example 16 provides a negative electrode active material, which is different from Example 1 in that the weight percentage of elemental silicon is 30%.

[0097] Embodiment 17

[0098] Embodiment 17 provides a negative electrode active material, which differs from Embodiment 1 in that, by weight percentage, it includes 5% elemental silicon, 5% silicon oxide (SiO), and the rest is artificial graphite. Among them, the average particle size D1 of elemental silicon is 6.5 μm, and the elemental silicon is a combination of a first elemental silicon and a second elemental silicon in a weight ratio of 7:10, the average particle size D3 of the first elemental silicon is 3.5 μm, and the average particle size of the second elemental silicon is 9.3 μm; the average particle size D1 of silicon oxide is 6.6 μm, and the silicon oxide is a combination of a first silicon oxide and a second silicon oxide in a weight ratio of 7:10, the average particle size D3 of the first silicon oxide is 3.8 μm, and the average particle size of the second silicon oxide is 9.2 μm.

[0099] Comparative Example 1

[0100] Comparative Example 1 provides a negative electrode active material, which is different from Example 1 in that the average particle size of the artificial graphite is 5.4 μm.

[0101] Comparative Example 2

[0102] Comparative Example 2 provides a negative electrode active material, which differs from Example 1 in that the elemental silicon is a combination of a first elemental silicon and a second elemental silicon in a weight ratio of 3:20, the average particle size D3 of the first elemental silicon is 1.9 μm, and the average particle size of the second elemental silicon is 6.8 μm.

[0103] Comparative Example 3

[0104] Comparative Example 3 provides a negative electrode active material, which differs from Example 1 in that the elemental silicon particles are a combination of a first elemental silicon and a second elemental silicon in a weight ratio of 4.9:1, the average particle size D3 of the first elemental silicon is 6.1 μm, and the average particle size of the second elemental silicon is 12.4 μm.

[0105] Comparative Example 4

[0106] Comparative Example 4 provides a negative electrode active material, which is different from Example 1 in that, in the coating process of single silicon, the ID / IG of the amorphous carbon is 1.3, and the aspect ratio of the carbon nanotube is 2000.

[0107] Comparative Example 5

[0108] Comparative Example 5 provides a negative electrode active material, which is different from Example 1 in that, in the coating process of single silicon, the ID / IG of the amorphous carbon is 1, and the aspect ratio of the carbon nanotube is 90.

[0109] Comparative Example 6

[0110] Comparative Example 6 provides a negative electrode active material, which is different from Example 1 in that, in the coating process of single silicon, the ID / IG of amorphous carbon is 1.2, and the aspect ratio of carbon nanotubes is 91.

[0111] Comparative Example 7

[0112] Comparative Example 7 provides a negative electrode active material, which is different from Example 1 in that the weight percentage of elemental silicon particles is 37%.

[0113] Comparative Example 8

[0114] Comparative Example 8 provides a negative electrode active material, which is different from Example 1 in that the single silicon has only one particle size specification, and the average particle size D1 is 6.5 μm.

[0115] Comparative Example 9

[0116] Comparative Example 9 provides a negative electrode active material, which differs from Comparative Example 8 in that the average particle size D1 of elemental silicon is 9 μm, and the average particle size D2 of artificial graphite is 9 μm.

[0117] Comparative Example 10

[0118] Comparative Example 10 provides a negative electrode active material, which is different from Comparative Example 8 in that the average particle size D1 of elemental silicon is 9 μm and is not subjected to carbon coating treatment.

[0119] Comparative Example 11

[0120] Comparative Example 11 provides a negative electrode active material, which differs from Comparative Example 8 in that the carbon coating treatment of elemental silicon does not include steps (5) and (6).

[0121] The comparison of parameters of the above embodiments is shown in Table 1 and Table 2, wherein ND3 / ND4 represents the weight ratio of the first silicon particles to the second silicon particles, and C1 / C2 represents the weight ratio of the amorphous carbon and the carbon nanotubes coated on the surface of the silicon particles.

[0122] Table 1

[0123]

[0124]

[0125] Table 2

[0126]

[0127]

[0128] Performance Evaluation

[0129] The negative electrode active material provided in the above embodiment is prepared into a negative electrode sheet, and then the negative electrode sheet is assembled into a battery roll core, and finally assembled into a cylindrical battery for testing. The preparation method is as follows:

[0130] (1) Preparation of positive electrode sheet: 97% of lithium nickel cobalt manganese oxide, 0.4% of carbon nanotube conductive agent, 1.6% of conductive carbon black, and 1% of polyvinylidene fluoride (PVDF) binder were taken as the solid matter of the positive electrode slurry by weight percentage, and the solid matter was dispersed in N-methyl-2-pyrrolidone with a solid content of 60%. The mixture was mixed evenly in a homogenizer, and the slurry was coated on both sides of an aluminum foil and dried to obtain a positive electrode sheet;

[0131] (2) Preparation of negative electrode sheet: In terms of weight percentage, 96% of negative electrode active material, 1% of acetylene black conductive agent, 1% of thickener (hydroxymethyl cellulose), and 2% of polyacrylate binder are taken as the solid matter of the negative electrode slurry, the solid matter is dispersed in deionized water, and the solid content is 40%. The mixture is mixed evenly in a homogenizer, and the slurry is coated on both sides of the copper foil and dried to obtain a negative electrode sheet;

[0132] (3) preparing an electrolyte: mixing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 1:1:1 to obtain an organic solvent, and then dissolving fully dried lithium salt LiPF6 in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L;

[0133] (4) Assembly: The positive electrode sheet and the negative electrode sheet are rolled separately, cut and die-cut according to size requirements, and then wound together with the separator to obtain a cylindrical battery core. The battery core tabs are welded to the electrical connecting sheet, installed in a shell, injected with electrolyte, sealed, and formed to obtain an experimental battery.

[0134] Test 1: Cycle performance test

[0135] Take a fresh battery, place it in a 25℃ constant temperature box for more than 4 hours, and test it according to the following steps:

[0136] (1) Discharge the battery at a constant current of 0.1C to 2.5V cutoff and leave it for 5 minutes;

[0137] (2) Charge the battery at a constant current of 0.2C to a cutoff of 4.2V, and at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0138] (3) Discharge the battery at a constant current of 0.2C to a cutoff of 2.5V, and let it stand for 5 minutes. Read the capacity value C0 at this time.

[0139] (4) Charge the battery at a constant current of 1.0C to 4.2V, and charge at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0140] (5) Discharge the battery at a constant current of 2.0C to a cutoff of 2.5V and let it stand for 5 minutes;

[0141] (6) Repeat steps (4) and (5) 600 times;

[0142] (7) The cycle performance of a single battery, i.e., the capacity retention rate, is obtained by calculating the ratio of the 600th discharge capacity to the first discharge capacity in steps (4) and (5).

[0143] Test 2: Hot box test

[0144] Take a fresh battery, place it in a 25℃ constant temperature box for more than 4 hours, and test it according to the following steps:

[0145] (1) Discharge the battery at a constant current of 0.1C to 2.5V cutoff and leave it for 5 minutes;

[0146] (2) Charge the battery at a constant current of 0.2C to a cutoff of 4.2V, and at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0147] (3) Place the battery in a thermostat, set the heating rate to 5K / min, heat it to 130°C, and keep it for 1 hour, then stop heating and allow it to cool down to below 30°C by self-heating;

[0148] (4) If the battery does not catch fire or emit smoke, it is considered to have passed. Otherwise, it is considered to have failed. At least 5 batteries shall be tested and the pass rate shall be recorded.

[0149] The test results are shown in Table 3.

[0150] Table 3

[0151]

[0152]

[0153] This application effectively improves the uniformity of the negative electrode active material by forming a gradation between silicon particles and carbon particles, and between silicon particles of different specifications, significantly reduces and disperses stress, avoids the volume change of silicon particles from causing concentrated stress on the surrounding area, and prevents silicon expansion from causing further damage to the battery. This application also improves the conductivity and stability of silicon particles by coating the silicon particles, enhances the film integrity of the SEI film, reduces the possibility of deposited metal forming dendrites on its surface, and improves battery performance and safety. Through the above improvements, the negative electrode active material in this application enables the battery to maintain a capacity of more than 80% after 600 cycles, and the hot box test is qualified.

[0154] In the description of this specification, reference to the terms "some embodiments", "an example", or similar descriptions means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment are included in at least one embodiment or example. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0155] Although examples of the present embodiment have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present embodiment, and the scope of the present embodiment is defined by the claims and their equivalents.

Claims

1. A negative electrode active material, characterized in that: In terms of weight percentage, the silicon particles are 2-30%, and the rest are carbon particles; wherein the average particle size of the silicon particles is D1, the average particle size of the carbon particles is D2, and the ratio a of D1 to D2 satisfies 0.5<a≤0.95; The silicon particles are subjected to carbon coating treatment, and the materials used for the carbon coating treatment are amorphous carbon and carbon nanotubes; wherein the ID / IG of the amorphous carbon is not greater than 1.0, and the aspect ratio b of the carbon nanotubes satisfies 120≤b≤13000.

2. The negative electrode active material according to claim 1, characterized in that The silicon particles include at least first silicon particles with an average particle size of D3 and second silicon particles with an average particle size of D4, D3≤5μm≤D4, the ratio c of D4 to D3 satisfies, 1.2≤c≤3, and the weight ratio of the first silicon particles to the second silicon particles is (0.2-3):

1.

3. The negative electrode active material according to claim 2, characterized in that: The a, b, and c satisfy 0.4<1000a*c / (b)≤15.

4. The negative electrode active material according to claim 1, characterized in that The silicon particles are simple silicon and / or silicon oxide; the carbon particles are selected from a mixture of one or more of artificial graphite, natural graphite, hard carbon and soft carbon.

5. The negative electrode active material according to any one of claims 1 to 4, characterized in that: The carbon coating process comprises the following steps: a. The silicon particles are heated to 400-800°C in a nitrogen atmosphere, and then acetylene gas is introduced at 0.1-1 L / hour for 4-8 hours; b. Continue to introduce propylene gas at 0.1-1L / hour and react for 12-36h; c. Stop passing acetylene and propylene gas, turn off heating, maintain nitrogen atmosphere and cool to below 30°C, remove the material, and obtain the amorphous carbon-coated silicon particles; d. adding the amorphous carbon-coated silicon particles to carbon nanotubes in an amount of 0.01-0.1% by mass thereof, and mixing to obtain a mixture; e. Add 0.3-1L ethanol and 0.01-0.1kg cellulose to each 1kg mixture and mix to obtain a slurry; f. Drying, grinding and sieving the slurry to obtain the silicon particles coated with amorphous carbon and carbon nanotubes.

6. The negative electrode active material according to claim 5, characterized in that In the silicon particles coated with amorphous carbon and carbon nanotubes, the weight ratio of the amorphous carbon to the carbon nanotubes is (0.2-5):

1.

7. A negative electrode slurry, characterized in that: In terms of weight percentage, the solid matter of the negative electrode slurry includes at least 0.5-2% conductive agent, 0.5-2% thickener, 0.5-2% binder, and the rest is the negative electrode active material according to any one of claims 1-6; the solid matter is dispersed in deionized water to form the negative electrode slurry, and the solid content is 30-50%.

8. A negative electrode sheet, characterized in that: The invention comprises a negative electrode current collector, at least one surface of which is coated with the negative electrode slurry according to claim 7, and the coating area is 80-98% of the total area of ​​the negative electrode current collector.

9. A battery roll core, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet according to claim 8 and a separator located therebetween; the battery roll core is formed by winding the positive electrode sheet, the negative electrode sheet and the separator; the battery roll core has a diameter of 20-60 mm and a height of 60-200 mm, and the ratio of the height to the diameter is greater than 1.

7.

10. A cylindrical battery, characterized in that: It comprises the battery roll core, a cap and a steel shell according to claim 9; the battery roll core is accommodated inside the steel shell, and the top is sealed with the cap.