Preparation method of silicon quantum dot loaded nitrogen-doped porous carbon lithium battery negative electrode material
Through the preparation of silicon quantum doped porous carbon materials with nitrogen loading, the problems of volume expansion and SEI rupture of silicon anode material in lithium-ion batteries are solved, the specific capacity and cycle stability of lithium-ion batteries are improved, and the conductive performance is improved .
Patent Information
- Application Number
- CN202411206397.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
As an anode material for lithium-ion batteries, silicon has problems such as volume expansion and contraction, resulting in electrical contact loss, SEI rupture, electrolyte consumption and low Coulomb efficiency, and the energy density and cycle life of traditional graphite materials are insufficient.
The preparation method of silicon quantum doped nitrogen-doped porous carbon material is adopted, and nano-silicon-carbon composite structure is formed through Tris buffer and dopamine hydrochloride precipitation, nano-microsphere grinding and magnesium powder heat treatment, thereby improving mechanical and electrochemical properties.
It significantly improves the specific capacity and cycle stability of the material, improves the conductivity and battery performance, solves the crushing problem caused by volume expansion, and achieves efficient electrochemical performance improvement.
Smart Images

Figure HDA0005019145910000011 
Figure HDA0005019145910000012 
Figure HDA0005019145910000013
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, in particular to the field of IPC H01M4, and more specifically to a method for preparing a silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material. Background Art
[0002] At present, lithium-ion batteries have been widely used in various fields of the national economy, such as new energy vehicles and electronic information. This has put forward higher energy density and higher safety requirements for lithium-ion batteries. The mainstream electrode materials with lithium iron phosphate and lithium cobalt oxide as positive electrodes and graphite as negative electrodes can no longer meet the requirements of high-performance lithium-ion batteries. The graphite materials in the traditional market have low capacity (372mAh·g -1 Alloy anodes (Si, Ge, Sn, Al, Sb, etc.) have higher lithium storage capacity than the intercalation graphite anodes currently used in lithium-ion batteries. Among them, silicon has a high theoretical specific capacity (4200mAh g -1 ) and abundant sources make it an attractive negative electrode material for lithium batteries. However, silicon as a battery anode material still inevitably has the following problems: (1) The alloy anode undergoes significant volume expansion and contraction during the insertion / extraction of lithium. This volume change (Si ~ 360%) will lead to the pulverization of the initial particle morphology and cause the loss of electrical contact between the active material and the electrode framework; (2) During lithiation, due to the change in volume during the cycle, the SEI will break, resulting in the electrode surface being periodically exposed to the electrolyte. This leads to the continuous formation of a very thick SEI film, resulting in the continuous consumption of the electrolyte during the cycle; (3) Excessive growth of SEI leads to low Coulombic efficiency, high ion transport resistance, low electronic conductivity, and reduced silicon capacity.
[0003] There are currently two solutions to this problem: (1) Compounding the material with carbon to improve conductivity and electrochemical performance. (2) One-dimensionalizing silicon materials to synthesize nanostructures. Through carbon doping, a carbon-silicon structure is achieved, which spontaneously absorbs the expansion stress and improves battery performance, Coulomb efficiency and electronic conductivity. Studies have shown that nanoscale Si particles can significantly alleviate the mechanical strain caused by volume changes, maintain the structural integrity of Si-based anodes, and thus improve the cycle stability of Si.
[0004] CN112980436B discloses a carbon quantum dot-derived carbon nanosheet composite silicon dioxide negative electrode material and a preparation method thereof. In the carbon quantum dot-derived carbon nanosheet composite nano silicon dioxide negative electrode material, the carbon quantum dot-derived carbon nanosheet has a thickness of ≤2nm, contains 0.8-.3% sulfur by mass, the silicon dioxide has a spherical shape, an amorphous crystal structure, and an average particle size of about 150nm. The carbon quantum dots and the sulfur doping agent are mixed and calcined to prepare sulfur-doped carbon quantum dot-derived carbon nanosheets, the carbon quantum dot-derived carbon nanosheets are ultrasonically dispersed in anhydrous ethanol, ammonia water, ethyl orthosilicate and deionized water are added and mixed, and the sulfur-doped carbon quantum dot-derived carbon nanosheet composite silicon dioxide negative electrode material is prepared by sol-gel method and freeze drying. The invention has a simple preparation process and low energy consumption, but the electrochemical performance is still not excellent enough. Summary of the invention
[0005] The present invention provides a method for preparing a silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material, comprising the following steps:
[0006] S1, dissolving Tris buffer in aqueous solvent A, mixing, adding dopamine hydrochloride, mixing, and drying the precipitate to obtain nanoparticles A;
[0007] S2, dissolving nano-microspheres A in aqueous solvent B, mixing, adding ammonia water, mixing to obtain a dispersion, dropping tetraethyl orthosilicate into the dispersion, washing with aqueous solvent C, filtering to obtain a precipitate, and drying to obtain nano-microspheres B;
[0008] S3, grinding the nano-microspheres B and magnesium powder uniformly, performing heat treatment in an inert atmosphere, washing with an aqueous solvent C, and drying to obtain.
[0009] The applicant has found that in step S3, the nano-microspheres B and magnesium powder are evenly ground and heat-treated with magnesium, which improves the specific capacity and mechanical properties of the material. A large amount of silicon oxide is reduced to elemental silicon, which improves the specific capacity of the material to a certain extent; the polydopamine matrix is carbonized at high temperature, and part of the nitrogen element therein is thermally decomposed to react with the elemental silicon of the outer layer to produce silicon nitride, which improves the mechanical properties of the material to a certain extent.
[0010] The mixing method in steps S1 and S2 is stirring or ultrasound, and the ultrasound time is 30-60 minutes.
[0011] The aqueous solvent A, aqueous solvent B, aqueous solvent C and aqueous solvent D are all selected from at least one of alcohols, aldehydes, ketones, ethers and deionized water.
[0012] Preferably, the aqueous solvent A and the aqueous solvent C include deionized water.
[0013] The weight ratio of Tris buffer to dopamine hydrochloride in step S1 is (0.5-0.8): (0.4-0.9).
[0014] Preferably, in step S1, the weight ratio of Tris buffer to dopamine hydrochloride is (0.5-0.6): (0.4-0.4).
[0015] In the step S1, the weight-to-volume ratio of the Tris buffer and the aqueous solvent A is (0.5-0.8) g / mL: (200-400).
[0016] Preferably, in step S1, the weight-to-volume ratio of Tris buffer to aqueous solvent A is (0.5-0.6) g / mL: (200-300).
[0017] The volume ratio of the aqueous solvent B, ammonia water and tetraethyl orthosilicate is (30-120): (1-4): (2-8).
[0018] Preferably, the volume ratio of the aqueous solvent B, ammonia water and tetraethyl orthosilicate is (30-80):(1-2):(2-5).
[0019] The aqueous solvent B includes a mixed solution of deionized water and anhydrous ethanol.
[0020] Preferably, the volume ratio of the deionized water to anhydrous ethanol is 1:(2-3).
[0021] The weight-to-volume ratio of the nanospheres A to the aqueous solvent B is (0.1-0.3) g / mL: (30-120).
[0022] Preferably, the weight-to-volume ratio of the nanospheres A to the aqueous solvent B is (0.1-0.3) g / mL: (30-80).
[0023] The weight ratio of the nano-microspheres B to the magnesium powder is 1:(1-3).
[0024] Preferably, the weight ratio of the nano-microspheres B to the magnesium powder is 1:(1-2).
[0025] The heat treatment step includes: heating to 800-1000° C. at a heating rate of 1-10° C. / min and maintaining the temperature for 1-3 hours.
[0026] Preferably, the heat treatment step comprises: heating to 800-1000° C. at a heating rate of 3-8° C. / min and maintaining the temperature for 1-2 hours.
[0027] The aqueous solvent D includes deionized water and hydrochloric acid.
[0028] Beneficial Effects
[0029] 1. The present invention utilizes polydopamine (PDA) as an alkaline nitrogen and carbon source to promote the hydrolysis of TEOS into silicate monomers, inducing a large number of SiO2 quantum dots to evenly cover the surface of the carbon matrix, which helps to increase the silicon content in subsequent materials.
[0030] 2. In step S3, the nano-microspheres B and magnesium powder are evenly ground and subjected to magnesium heat high-temperature treatment, thereby improving the specific capacity and mechanical properties of the material.
[0031] 3. The present invention solves some problems in the commercial use of silicon materials as battery anodes, especially the problem of powderization caused by volume expansion during the lithiation process.
[0032] 4. The improved silicon-carbon composite of the present invention exhibits excellent electrical conductivity and improves the battery specific capacity and cycle stability.
[0033] 5. Through the synergistic effect of different elements, the electrochemical performance is improved and a composite structure formed by nano-silicon-carbon composite materials is constructed.
[0034] 6. The preparation method of the present invention has simple process and low cost, which is conducive to sustainable production. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a scanning electron microscope image of the PDA nanospheres prepared in Example 1.
[0036] Figure 2 This is a transmission electron microscope image of the PDA nanospheres prepared in Example 1.
[0037] Figure 3 This is a scanning electron microscope image of the PDA@SiO2 nanospheres prepared in Example 2.
[0038] Figure 4 This is a transmission electron microscope image of the PDA@SiO2 nanospheres prepared in Example 2.
[0039] Figure 5 This is a scanning electron microscope image of the NC@Si nanomaterial prepared in Example 3.
[0040] Figure 6 This is a transmission electron microscope image of the NC@Si nanomaterial prepared in Example 3.
[0041] Figure 7 The particle size distribution histograms of the three materials prepared in Examples 1-3.
[0042] Figure 8 X-ray diffraction patterns of PDA nanospheres and NC@Si nanomaterials prepared in Example 1 and Example 3, wherein the red curve corresponds to the NC@Si nanomaterial.
[0043] Fig. 9 Raman spectra of PDA nanospheres and NC@Si nanomaterials prepared in Example 1 and Example 3, wherein the red curve corresponds to the NC@Si nanomaterial.
[0044] Fig.10 Thermogravimetric analysis curves of PDA nanospheres and NC@Si nanomaterials prepared in Example 1 and Example 3, where the red curve corresponds to the NC@Si nanomaterial.
[0045] Fig.11 This is the oxygen element X-ray electron energy spectrum of the NC@Si nanomaterial prepared in Example 3.
[0046] Fig.12 This is the carbon element X-ray electron energy spectrum of the NC@Si nanomaterial prepared in Example 3.
[0047] Fig.13 This is the nitrogen element X-ray electron energy spectrum of the NC@Si nanomaterial prepared in Example 3.
[0048] Fig.14 This is the X-ray electron energy spectrum of the NC@Si nanomaterial prepared in Example 3.
[0049] Fig.15 Electrochemical impedance spectra of the three materials prepared in Examples 1-3 before cycling.
[0050] Fig.16 Electrochemical impedance spectra of the three materials prepared in Examples 1-3 after cycling.
[0051] Fig.17 These are the charge and discharge curves at different rates for the three materials prepared in Examples 1-3.
[0052] Fig.18 Cyclic voltammetry characteristic curves of the three materials prepared in Examples 1-3 at different scan rates.
[0053] Fig.19 The charge and discharge curves of NC@Si nanomaterials prepared in embodiment 3 at different cycle numbers.
[0054] Fig. 20 The cycling performance curve of NC@Si nanomaterials prepared in implementation 3. DETAILED DESCRIPTION
[0055] Example 1
[0056] A method for preparing silicon quantum dots loaded with nitrogen-doped porous carbon material comprises the following steps:
[0057] (1) Dissolve 0.6 g of Tris buffer in 250 mL of deionized water and stir for 30 min;
[0058] (2) adding 0.5 g of dopamine hydrochloride to the mixed solution in step 1 and allowing to react fully under stirring;
[0059] (3) After the reaction is completed, the mixed solution in step 2 is filtered to obtain a precipitate, which is dried in a vacuum drying oven overnight. After sufficient drying, a brown solid substance is obtained, and the silicon quantum dot-loaded nitrogen-doped porous carbon material is obtained, which is recorded as PDA nanospheres.
[0060] Example 2
[0061] A method for preparing silicon quantum dots loaded with nitrogen-doped porous carbon material carbon substrate loaded with silicon oxide particles comprises the following steps:
[0062] (1) 0.2 g of the PDA nanospheres prepared in Example 1 were dispersed in a mixed solution of 18 mL of deionized water and 42 mL of anhydrous ethanol, 1.5 mL of aqueous ammonia (25 wt %) was added, and the mixture was stirred thoroughly.
[0063] (2) 3 mL of tetraethyl orthosilicate (TEOS) was slowly dripped into the solution of step 1, stirred thoroughly, and reacted for 1 h. The mixed solution was filtered and washed with deionized water for 3 times to obtain a silicon quantum dot-loaded nitrogen-doped porous carbon material carbon substrate loaded with silicon oxide particles sample, recorded as PDA@SiO2 nanospheres.
[0064] Example 3
[0065] A method for preparing a silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material comprises the following steps:
[0066] (1) The dried material obtained in Example 2 and magnesium powder were ground evenly in a ratio of 1:2 and then fed into a tube furnace. Under argon protection, the temperature was increased to 800° C. at a heating rate of 5° C. / min and kept at a constant temperature for 1 h to obtain a dark brown powder.
[0067] (2) The dark brown powder was washed three times with an acidic solution (1 M HCL aqueous solution) and then washed three times with deionized water to obtain a silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material, which was recorded as NC@Si nanomaterial.
[0068] Performance Testing Methods
[0069] The materials prepared in Examples 1-3 were subjected to the following tests:
[0070] 1. Morphology test: Use a field emission scanning electron microscope to calculate the particle size distribution. The equipment is called FEI (scanning electron microscope). The morphology test results are as follows: Figure 1-6 The particle size distribution is shown in Figure 7 shown.
[0071] 2. Spectral test: combined with X-ray diffraction pattern ( Figure 8 ) and Raman spectroscopy ( Fig. 9 ), determine the synthesis of NC@Si nanomaterials.
Claims
1. A method for preparing silicon quantum dots loaded with nitrogen-doped porous carbon lithium battery negative electrode material, It is characterized in that The following steps are involved: S1, dissolving Tris buffer in aqueous solvent A, mixing, adding dopamine hydrochloride, mixing, and drying the precipitate to obtain nanoparticles A; S2, dissolving nano-microspheres A in aqueous solvent B, mixing, adding ammonia water, mixing to obtain a dispersion, dropping tetraethyl orthosilicate into the dispersion, washing with aqueous solvent C, filtering to obtain a precipitate, and drying to obtain nano-microspheres B; S3, grinding the nano-microspheres B and magnesium powder uniformly, performing heat treatment in an inert atmosphere, washing with an aqueous solvent D, and drying to obtain.
2. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 1, It is characterized in that The mixing method in steps S1 and S2 is stirring or ultrasound, and the ultrasound time is 30-60 minutes.
3. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 2, It is characterized in that The weight ratio of Tris buffer to dopamine hydrochloride in step S1 is (0.5-0.8): (0.4~0.9)。 4. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 3, It is characterized in that In the step S1, the weight-to-volume ratio of the Tris buffer and the aqueous solvent A is (0.5-0.8) g / mL: (200-400).
5. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 1 or 4, It is characterized in that The volume ratio of the aqueous solvent B, ammonia water and tetraethyl orthosilicate is (30-120): (1~4):(2~8)。 6. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 5, It is characterized in that The aqueous solvent B includes a mixed solution of deionized water and anhydrous ethanol.
7. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 6, It is characterized in that The weight-to-volume ratio of the nanospheres A and the aqueous solvent B is (0.1-0.3) g / mL: (30~120)。 8. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 7, It is characterized in that The weight ratio of the nano-microspheres B to the magnesium powder is 1:(1-3).
9. The method for preparing the silicon quantum dot-loaded nitrogen-doped porous carbon lithium battery negative electrode material according to claim 1 or 8, It is characterized in that The heat treatment step includes: heating to 800-1000° C. at a heating rate of 1-10° C. / min and maintaining the temperature for 1-3 hours.