High-compaction lithium manganese iron phosphate positive electrode material
Through the two calcination preparation process, the conductivity and compaction performance of lithium manganese iron phosphate positive electrode material is improved, and the problems of poor conductivity and reduced compaction are solved, and efficient electrochemical performance and charging capacity are achieved.
Patent Information
- Application Number
- CN202411267305.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
The conductivity of lithium manganese iron phosphate cathode material is poor, resulting in poor capacity and rate performance. At the same time, the small particle size leads to excessive specific surface area and reduced powder compaction.
Two-time calcination preparation process is adopted. During the first calcination, carbon source is added to calcinate under air atmosphere to generate carbon dioxide and reduce trivalent Fe to divalent Fe; during the second calcination, composite iron salts of FeNO3 and Fe(C5H5)2 are introduced. , improve the degree of graphitization and electron conductivity of carbon, and form a material with a large and small particle grade by calcining through an inert atmosphere.
Effectively improve the conductivity and compaction performance of lithium manganese iron phosphate positive electrode material, and achieve a balance between the improvement of conductivity and specific surface area and compaction. The charging capacity of 0.1C reaches 163.28mAh/g and the conductivity is 1.02E -01S/cm, compaction density is 2.45g/cm3.
Smart Images

Figure CN119092688A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium iron manganese phosphate cathode materials, and particularly relates to a high tap density lithium iron manganese phosphate cathode material. Background Art
[0002] LiMn x Fe 1-x PO4(0 < x < 1) (LMFP) is a solid solution of LiFePO4 (LFP) and LiMnPO4 (LMP). The Mn element raises the voltage plateau, thereby increasing the energy density of the lithium iron system. LMFP maintains the stable olivine structure of LFP and introduces LMP (4.1V) with a high voltage plateau, thus increasing the energy density of the lithium iron system.
[0003] However, the conductivity of the manganese element is relatively weak. Lithium iron phosphate has semiconductor properties, with an electronic conductivity of 10 -9 S / cm, while lithium iron manganese phosphate is an insulator with an electronic conductivity of 10 -13 S / cm. The transition energy gap of electrons in lithium iron manganese phosphate is as high as 2 eV (the transition energy gap of lithium iron phosphate is 0.3 eV), showing an order-of-magnitude difference compared with lithium iron phosphate materials, and having the disadvantages of low conductivity and low ion mobility, which affect its capacity performance and rate performance. Therefore, grain nanocrystallization, carbon coating, and ion doping have become the mainstream methods to improve the problems of low conductivity and low ion mobility.
[0004] Reducing the particle size and carbon coating can effectively improve the problems of low conductivity and low ion mobility. However, too small a primary particle size will lead to too high a specific surface area of lithium iron manganese phosphate, an increase in powder impedance, and a decrease in powder tap density; compared with lithium iron phosphate, lithium iron manganese phosphate has a higher carbon coating amount and a lower calcination temperature, resulting in a lower degree of graphitization. Ordinary carbon sources exist in the form of amorphous flocculent carbon after carbonization, also leading to too high a specific surface area of lithium iron manganese phosphate and a decrease in powder tap density.
[0005] Based on this, there is an urgent need to study a lithium iron manganese phosphate cathode material that can effectively solve the problem of poor conductivity of lithium iron manganese phosphate and further avoid the problems of increased specific surface area and decreased tap density. Summary of the Invention
[0006] Object of the Invention: The technical problem to be solved by the present invention is to provide a lithium iron manganese phosphate cathode material that can effectively solve the problem of poor conductivity of lithium iron manganese phosphate, further avoid the problems of increased specific surface area and decreased tap density, and has a high tap density.
[0007] Technical Solution: The high tap density lithium iron manganese phosphate cathode material of the present invention is prepared by the following steps:
[0008] (1) placing a manganese source, an iron source, a phosphorus source, a lithium source and a carbon source in deionized water, stirring, grinding and drying to obtain a lithium iron manganese phosphate precursor powder;
[0009] (2) calcining the lithium iron manganese phosphate precursor powder at 400-600° C. in an air atmosphere for 4-15 hours to obtain lithium iron manganese phosphate pre-calcined material I;
[0010] (3) After crushing the lithium iron manganese phosphate pre-burned material I, adding a carbon source and a composite iron salt, placing it in deionized water, stirring, grinding, and drying, to obtain the lithium iron manganese phosphate pre-burned material II; the composite iron salt is a mixture of FeNO3 and Fe(C5H5)2;
[0011] (4) calcining the lithium manganese iron phosphate pre-sintered material II at 610-800° C. in an inert atmosphere for 10-25 h, and then naturally cooling to obtain the lithium manganese iron phosphate positive electrode material.
[0012] The present invention adopts two calcinations in steps to prepare the lithium manganese iron phosphate positive electrode material, and a carbon source is added during the first sintering and calcined in an air atmosphere, so that the carbon source directly reacts with oxygen to generate carbon dioxide for removal, thereby avoiding residual carbon from inhibiting the growth of secondary particles by coating, and reducing trivalent Fe to generate divalent Fe; and during the second sintering, a composite iron salt composed of FeNO3 and Fe(C5H5)2 is introduced. The introduction of the iron salt is beneficial to improving the graphitization degree of carbon, reducing the amorphous flocculent carbon on the surface of LMFP, and making the surface coating C layer thinner and the carbon coating more uniform; on the other hand, during calcination, N and C in the carbon source, FeNO3 and Fe(C5H5)2 can be combined to form pyridine N, pyridine N and pyridine C. The structure of graphite N and graphite N can produce active defect sites, accelerate the migration of lithium ions, and is beneficial to improving the electronic conductivity and diffusion rate of lithium ions; furthermore, by introducing the composite iron salt composed of FeNO3 and Fe(C5H5)2, based on the secondary calcination nucleation method of the present invention, a lithium iron manganese phosphate positive electrode material with large and small particle grading can be formed, thereby improving the compaction performance and electrical properties of the positive electrode material, that is, the large-particle lithium iron manganese phosphate positive electrode material is formed by a primary sintering and then grown by a secondary sintering to form a large-particle lithium iron manganese phosphate, and the small-particle lithium iron manganese phosphate is formed by directly performing a secondary sintering using the iron in the composite iron salt as the iron source of the lithium iron manganese phosphate, thereby improving the electrical properties of the positive electrode material with small-particle lithium iron manganese phosphate.
[0013] Therefore, the present invention is based on the preparation process conditions of secondary sintering, and uses direct air atmosphere sintering of the carbon source during the first sintering, and the secondary sintering uses a combination of sintering of the carbon source and the composite iron salt under an inert atmosphere. This preparation method can not only effectively solve the problem of poor conductivity of lithium manganese iron phosphate, but also avoid the problem of increased specific surface and reduced compaction, thereby achieving a balance between the two.
[0014] Furthermore, the molar ratio of the manganese source, iron source, phosphorus source and lithium source used in the lithium manganese iron phosphate positive electrode material is x:(1-x):y:z, wherein 0.05≤x≤0.95; 1≤y≤1.05; 1≤z≤1.08.
[0015] Furthermore, the manganese source used in the lithium iron manganese phosphate positive electrode material can be manganese carbonate, manganese tetraoxide, manganese iron oxide or manganese iron precursor; the iron source can be iron phosphate, iron tetraoxide, manganese iron oxide, manganese iron precursor; the phosphorus source can be phosphoric acid, diammonium phosphate, lithium phosphate or monoammonium phosphate; the lithium source can be lithium carbonate, lithium hydroxide, lithium sulfate, lithium nitrate or lithium chloride precursor.
[0016] Furthermore, the amount of carbon source added in step (1) of preparing the lithium manganese iron phosphate positive electrode material is 8-20% of the theoretical mass of the generated lithium manganese iron phosphate, and the amount of carbon source added in step (3) is 5-15% of the theoretical mass of the generated lithium manganese iron phosphate.
[0017] Furthermore, the carbon source used in the lithium manganese iron phosphate positive electrode material can be glucose, sucrose, starch, cellulose, polyvinyl alcohol, soluble starch, cellulose, ascorbic acid or phenolic resin.
[0018] Furthermore, in step (1) and step (3) of preparing the lithium manganese iron phosphate positive electrode material, the stirring is carried out at a stirring temperature of 0-25° C. and a frequency of 20-50 Hz, and the stirring reaction is carried out for 0.5-2 hours.
[0019] Furthermore, in step (1) and step (3) of preparing the lithium manganese iron phosphate positive electrode material, the grinding time is 0.5-6 hours and the drying temperature is 150-250°C.
[0020] Furthermore, the amount of the composite iron salt used in the lithium manganese iron phosphate positive electrode material is 0.1-5% of the mass of the theoretically generated lithium manganese iron phosphate. Preferably, the mass ratio of FeNO3 and Fe(C5H5)2 in the composite iron salt used in the lithium manganese iron phosphate positive electrode material is (0.01-1):1.
[0021] Beneficial effects: Compared with the prior art, the significant advantages of the present invention are: the lithium manganese iron phosphate positive electrode material not only effectively solves the problem of poor conductivity of lithium manganese iron phosphate, but also avoids the problem of increased specific surface and reduced compaction; its 0.1C charging capacity can reach more than 163.28mAh / g, 0.1C discharge capacity can reach more than 162.78mAh / g, and the specific surface area is 13.58m 2 / g, the conductivity is 1.02E-01S / cm, and the compaction density can reach 2.45g / cm 3 . BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a SEM image of the lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present invention;
[0023] Figure 2 This is a particle size distribution diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present invention;
[0024] Figure 3 This is a SEM image of the lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention;
[0025] Figure 4 This is a SEM image of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention;
[0026] Figure 5 This is a SEM image of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 3 of the present invention;
[0027] Figure 6 This is a SEM image of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be noted that the raw materials used in the present invention can all be purchased from the market.
[0029] Example 1
[0030] The high-density lithium manganese iron phosphate positive electrode material of Example 1 is prepared by the following steps:
[0031] (1) manganese carbonate, iron phosphate, ammonium dihydrogen phosphate and lithium carbonate in a molar ratio of 0.6:0.4:0.6:1, and glucose accounting for 10% of the mass of the theoretically generated lithium manganese iron phosphate, are placed in deionized water, and stirred at a temperature of 25° C. and a frequency of 20 Hz for 0.5 h to obtain a mixed slurry I;
[0032] (2) grinding the mixed slurry I for 2 hours to obtain lithium manganese iron phosphate precursor slurry I;
[0033] (3) drying the lithium iron manganese phosphate precursor slurry I at 150° C. to obtain lithium iron manganese phosphate precursor powder I;
[0034] (4) calcining the lithium iron manganese phosphate precursor powder I at 500° C. in an air atmosphere for 10 h, and naturally cooling to obtain the lithium iron manganese phosphate pre-calcined material I;
[0035] (5) The pre-burned lithium manganese iron phosphate material I was crushed and placed in excess deionized water with 10% of the theoretical mass of the generated lithium manganese iron phosphate in glucose and 3% of the theoretical mass of the generated lithium manganese iron phosphate in a composite iron salt. The mixture was stirred at 25°C and 20 Hz for 0.5 h to obtain a uniform mixed slurry II. The mass ratio of FeNO3 to Fe(C5H5)2 in the composite iron salt was 0.5:1.
[0036] (6) grinding the mixed slurry II for 2 hours to obtain lithium manganese iron phosphate pre-sintered material slurry II;
[0037] (7) drying the lithium iron manganese phosphate pre-calcined material slurry II at 150° C. to obtain the lithium iron manganese phosphate pre-calcined material II;
[0038] (8) The lithium manganese iron phosphate pre-fired material II is calcined at 700° C. in a nitrogen atmosphere for 14 h, and then naturally cooled to obtain the lithium manganese iron phosphate positive electrode material.
[0039] Example 2
[0040] The high-density lithium iron manganese phosphate positive electrode material of Example 2 is prepared by the following steps:
[0041] (1) manganese carbonate, iron phosphate, ammonium dihydrogen phosphate and lithium carbonate in a molar ratio of 0.65:0.35:0.651:1.03, and glucose accounting for 11% of the mass of the theoretically generated manganese iron lithium phosphate, are placed in deionized water, and stirred at a temperature of 20° C. and a frequency of 30 Hz for 1 hour to obtain a mixed uniform slurry I;
[0042] (2) grinding the mixed slurry for 1.5 hours to obtain lithium manganese iron phosphate precursor slurry I;
[0043] (3) drying the lithium iron manganese phosphate precursor slurry I at 150° C. to obtain lithium iron manganese phosphate precursor powder I;
[0044] (4) calcining the lithium iron manganese phosphate precursor powder I at 450° C. in an air atmosphere for 12 h, and naturally cooling to obtain the lithium iron manganese phosphate pre-calcined material I;
[0045] (5) crushing the pre-calcined lithium manganese iron phosphate material I, placing it in deionized water with glucose accounting for 8% of the theoretical mass of lithium manganese iron phosphate and composite iron salt accounting for 4% of the theoretical mass of lithium manganese iron phosphate, stirring at a temperature of 20° C. and a frequency of 30 Hz, reacting for 1 hour to obtain a mixed uniform slurry II;
[0046] (6) grinding the mixed slurry II for 2 hours to obtain lithium manganese iron phosphate pre-sintered material slurry II;
[0047] (7) drying the lithium iron manganese phosphate pre-calcined material slurry II at 150° C. to obtain the lithium iron manganese phosphate pre-calcined material II;
[0048] (8) The lithium manganese iron phosphate pre-fired material II is calcined at 750° C. in a nitrogen atmosphere for 10 h, and then naturally cooled to obtain the lithium manganese iron phosphate positive electrode material.
[0049] The structure of the lithium manganese iron phosphate positive electrode materials prepared in Example 1 and Example 2 was analyzed, and the results obtained are as follows: Figures 1 to 3 As shown. Figures 1 to 3 It can be seen that the lithium iron manganese phosphate positive electrode materials prepared in Example 1 and Example 2 both form a morphology of large and small particle gradation. This proves that the preparation process of the present invention can form a lithium iron manganese phosphate positive electrode material with large and small particle gradation, thereby improving the compaction performance and electrical performance of the positive electrode material.
[0050] Comparative Example 1
[0051] The basic steps are the same as those in Example 1, except that no composite iron salt is added. The specific steps are as follows:
[0052] The high-pressure compacted lithium manganese iron phosphate positive electrode material of Comparative Example 1 is prepared by the following steps:
[0053] (1) manganese carbonate, iron phosphate, ammonium dihydrogen phosphate and lithium carbonate in a molar ratio of 0.6:0.4:0.6:1, and glucose accounting for 10% of the mass of the theoretically generated lithium manganese iron phosphate, are placed in deionized water, and stirred at a temperature of 25° C. and a frequency of 20 Hz for 0.5 h to obtain a mixed slurry I;
[0054] (2) grinding the mixed slurry I for 2 hours to obtain lithium manganese iron phosphate precursor slurry I;
[0055] (3) drying the lithium iron manganese phosphate precursor slurry I at 150° C. to obtain lithium iron manganese phosphate precursor powder I;
[0056] (4) calcining the lithium iron manganese phosphate precursor powder I at 500° C. in an air atmosphere for 10 h, and naturally cooling to obtain the lithium iron manganese phosphate pre-calcined material I;
[0057] (5) crushing the lithium manganese iron phosphate pre-burned material I, and placing it in deionized water with glucose accounting for 10% of the theoretical mass of the lithium manganese iron phosphate produced, stirring at a temperature of 25° C. and a frequency of 20 Hz, reacting for 0.5 h to obtain a mixed uniform slurry II;
[0058] (6) grinding the mixed slurry II for 2 hours to obtain lithium manganese iron phosphate pre-sintered material slurry II;
[0059] (7) drying the lithium iron manganese phosphate pre-calcined material slurry II at 150° C. to obtain the lithium iron manganese phosphate pre-calcined material II;
[0060] (8) The lithium manganese iron phosphate pre-fired material II is calcined at 700° C. in a nitrogen atmosphere for 14 h, and then naturally cooled to obtain the lithium manganese iron phosphate positive electrode material.
[0061] The high-density lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 was subjected to structural analysis, and the results obtained are as follows: Figure 4 As shown. Figure 4 It can be seen that in Comparative Example 1, by not adding the composite iron salt, the positive electrode material particles prepared therein are basically uniform large particle morphology, and no morphology of large and small particle grading is formed.
[0062] Comparative Example 2
[0063] The basic steps are the same as those in Example 2, except that only Fe(C5H5)2 is used in the composite iron salt.
[0064] Comparative Example 3
[0065] The basic steps are the same as those in Example 1, except that a one-time sintering preparation process is used. The specific steps are as follows:
[0066] (1) manganese carbonate, iron phosphate, ammonium dihydrogen phosphate and lithium carbonate in a molar ratio of 0.6:0.4:0.6:1, glucose accounting for 14.5% of the theoretical mass of lithium manganese iron phosphate generated, and composite iron salt accounting for 3% of the theoretical mass of lithium manganese iron phosphate generated are placed in deionized water, and stirred at a temperature of 25° C. and a frequency of 20 Hz for 0.5 h to obtain a mixed uniform slurry;
[0067] (2) grinding the mixed slurry for 2 hours to obtain lithium manganese iron phosphate slurry;
[0068] (3) drying the lithium iron manganese phosphate slurry at 150° C. to obtain lithium iron manganese phosphate powder;
[0069] (4) calcining the lithium iron manganese phosphate powder at 700° C. in a nitrogen atmosphere for 10 h, and naturally cooling it to obtain a lithium iron manganese phosphate positive electrode material;
[0070] The structure of the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 3 was characterized, and the results obtained are as follows: Figure 5 As shown. Figure 5 It can be seen that compared with the two-time sintering process, the lithium manganese iron phosphate particles obtained after one sintering are evenly distributed, small in size, and have poor sphericity, and no morphology of large and small particle grading is formed.
[0071] Comparative Example 4
[0072] Comparative Example 4 is substantially the same as Example 1, except that the first sintering is performed under a nitrogen atmosphere. The specific steps are as follows:
[0073] (1) manganese carbonate, iron phosphate, ammonium dihydrogen phosphate and lithium carbonate in a molar ratio of 0.6:0.4:0.6:1, and glucose accounting for 10% of the mass of the theoretically generated lithium manganese iron phosphate, are placed in deionized water, and stirred at a temperature of 25° C. and a frequency of 20 Hz for 0.5 h to obtain a mixed slurry I;
[0074] (2) grinding the mixed slurry I for 2 hours to obtain lithium manganese iron phosphate precursor slurry I;
[0075] (3) drying the lithium iron manganese phosphate precursor slurry I at 150° C. to obtain lithium iron manganese phosphate precursor powder I;
[0076] (4) calcining the lithium iron manganese phosphate precursor powder I at 500° C. in a nitrogen atmosphere for 10 h, and naturally cooling to obtain the lithium iron manganese phosphate pre-calcined material I;
[0077] (5) After the lithium manganese iron phosphate pre-burned material I is crushed, glucose accounting for 10% of the theoretical mass of the lithium manganese iron phosphate generated and a composite iron salt accounting for 3% of the theoretical mass of the lithium manganese iron phosphate generated are placed in deionized water, and stirred at a temperature of 25° C. and a frequency of 20 Hz for 0.5 h to obtain a mixed uniform slurry II;
[0078] (6) grinding the mixed slurry II for 2 hours to obtain lithium manganese iron phosphate pre-sintered material slurry II;
[0079] (7) drying the lithium iron manganese phosphate pre-calcined material slurry II at 150° C. to obtain the lithium iron manganese phosphate pre-calcined material II;
[0080] (8) The lithium manganese iron phosphate pre-fired material II is calcined at 700° C. in a nitrogen atmosphere for 14 h, and then naturally cooled to obtain the lithium manganese iron phosphate positive electrode material.
[0081] The structure of the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 4 was characterized, and the results obtained are as follows: Figure 6 As shown. Figure 6 It can be seen that during the first sintering in a nitrogen atmosphere, the residual carbon hindered the growth of the particles in the secondary sintering stage; the particle size was small and the morphology was irregular.
[0082] Performance Testing
[0083] The lithium iron manganese phosphate positive electrode materials obtained in the above-mentioned Example 1, Example 2 and Comparative Examples 1 to 4 were prepared into button cells by the following method and the electrochemical performance was evaluated: the lithium iron manganese phosphate positive electrode material, Super P and PVDF were uniformly mixed in a NMP solution at a ratio of 8:1:1 to obtain a mixed slurry, the slurry was applied on a bright aluminum foil by hand coating, and then dried at 100°C. After the NMP was completely volatilized, the electrode sheet was punched into an electrode sheet with a diameter of 13 mm, and then the electrode sheet was placed in a vacuum oven at 105°C to dry overnight. After the electrode sheet was weighed, it was quickly transferred to a glove box, and metal lithium was used as the counter electrode, Celgard 2400 was used as the diaphragm, and the electrolyte was 1 mol / L LiPF6 was dissolved in a mixed solvent of EC / DMC / EMC (volume ratio of 1:1:1). The assembled battery was subjected to an electrochemical performance test using a Xinwei 4008 constant current test cabinet with a test voltage range of 2.0-4.35 V. The electrochemical performance results are shown in Table 1.
[0084] Table 1 Electrochemical performance characterization of materials of Example 1, Example 2 and Comparative Examples 1 to 4 (button cell)
[0085]
[0086] It can be seen from Table 1 that the lithium manganese iron phosphate positive electrode material prepared by the process of the present invention not only effectively solves the problem of poor conductivity of lithium manganese iron phosphate, but also avoids the problem of increased specific surface area and reduced compaction.
[0087] In addition to the above embodiments, in the process steps of preparing high-density manganese iron phosphate lithium positive electrode materials of the present invention, in addition to the parameters defined in Examples 1 and 2, the parameters can be adjusted in a floating range up and down to reach the parameter range defined in the claims. Therefore, this application only supports the parameter range by listing Examples 1 and 2, and the ranges defined in the claims can all achieve similar technical effects.
Claims
1. A high-density lithium manganese iron phosphate positive electrode material, It is characterized in that Prepared by the following steps: (1) placing a manganese source, an iron source, a phosphorus source, a lithium source and a carbon source in deionized water, stirring, grinding and drying to obtain a lithium iron manganese phosphate precursor powder; (2) calcining the lithium iron manganese phosphate precursor powder at 400-600° C. in an air atmosphere for 4-15 hours to obtain lithium iron manganese phosphate pre-calcined material I; (3) After the lithium manganese iron phosphate pre-burned material I is crushed, a carbon source and a composite iron salt are added, and the mixture is placed in deionized water. After stirring, grinding, and drying, the lithium manganese iron phosphate pre-burned material II is obtained; the composite iron salt is FeNO 3 and Fe(C 5 H 5 ) 2 mixture of (4) calcining the lithium manganese iron phosphate pre-sintered material II at 610-800° C. in an inert atmosphere for 10-25 h, and then naturally cooling to obtain the lithium manganese iron phosphate positive electrode material.
2. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that In step (1), the molar ratio of the manganese source, iron source, phosphorus source and lithium source is x:(1-x):y:z; wherein 0.05≤x≤0.95, 1≤y≤1.05, and 1≤z≤1.
08.
3. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that The manganese source is manganese carbonate, manganese trimanganese tetroxide, manganese iron oxide or manganese iron precursor; the iron source is iron phosphate, iron trimanganese tetroxide, manganese iron oxide or manganese iron precursor; the phosphorus source is phosphoric acid, diammonium phosphate, lithium phosphate or monoammonium phosphate; the lithium source is lithium carbonate, lithium hydroxide, lithium sulfate, lithium nitrate or lithium chloride precursor.
4. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that The amount of carbon source added in step (1) is 8-20% of the mass of the theoretically generated lithium iron manganese phosphate, and the amount of carbon source added in step (3) is 5-15% of the mass of the theoretically generated lithium iron manganese phosphate.
5. The high-density lithium iron manganese phosphate positive electrode material according to claim 4, It is characterized in that The carbon source is glucose, sucrose, starch, cellulose, polyvinyl alcohol, soluble starch, cellulose, ascorbic acid or phenolic resin.
6. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that In step (1) and step (3), the stirring is carried out at a stirring temperature of 0-25° C. and a frequency of 20-50 Hz, and the stirring reaction is carried out for 0.5-2 h.
7. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that In step (1) and step (3), the grinding time is 0.5-6h and the drying temperature is 150-250°C.
8. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that In step (3), the amount of the composite iron salt added is 0.1-5% of the mass of the theoretically generated lithium manganese iron phosphate.
9. The high-density lithium iron manganese phosphate positive electrode material according to claim 1, It is characterized in that The FeNO in the composite iron salt 3 and Fe(C 5 H 5 ) 2 The mass ratio is (0.01-1):1.
Citation Information
Cited By
Preparation method of high-compaction lithium manganese iron phosphate positive electrode material
CN119786544A
Method for preparing high-compaction lithium manganese iron phosphate positive electrode material
CN121573663A
A method for preparing a high-compaction lithium iron manganese phosphate cathode material
CN121573663B