Composite solid electrolyte material introduced with ion filler, preparation method and application

By introducing inorganic fillers into polymer electrolytes and forming composites, the problem of weak interface interactions in composite electrolyte materials is solved, the lithium ion conductivity and battery performance are significantly improved, and the stable circulation of all solid-state batteries is achieved.

CN119092808AActive Publication Date: 2024-12-06SOUTH CHINA UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411182012.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The interface interaction between fillers and polymers in existing composite polymer electrolyte materials is weak, resulting in a large impedance between the interface between the electrolyte and the electrode, affecting the performance of lithium-ion batteries, and lacking the regulation of microstructure and rapid ion transfer channels. Design limits its performance in practical applications.

Method used

Before the polymer matrix is ​​formed, inorganic filler particles are introduced, polymer-inorganic composite is formed by heat-induced polymerization, and dissolved into film to build a fast lithium ion transmission channel, improve lithium ion transmission efficiency, and significantly improve the ion conductance of polymer electrolytes Rate.

Benefits of technology

It has achieved the replacement of the separator and electrolyte in traditional batteries at room temperature, significantly improving the lithium ion transmission efficiency and the cycling stability of the battery, and is suitable for the application of all-solid-state batteries at wide temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092808A_ABST
    Figure CN119092808A_ABST
Patent Text Reader

Abstract

The invention discloses an ionic filler introduced composite solid electrolyte material, a preparation method and application, preparation raw materials comprise a polymer electrolyte, a lithium salt, a filler and a solvent, and the preparation method comprises the following steps: (1) uniformly mixing the filler and a monomer, and adding a free radical polymerization initiator azodiisobutyronitrile to obtain a compound; (2) uniformly mixing the compound with a lithium salt in a solvent to obtain a mixture; and (3) drying the mixture to form a film to obtain the composite solid electrolyte material. According to the invention, before a polymer matrix is formed, inorganic filler particles are preferentially introduced and uniformly mixed, then thermal initiation polymerization is performed to form a polymer-inorganic compound, and then the polymer-inorganic compound is dissolved to form a film, so that a rapid lithium ion transmission channel is constructed, the lithium ion transmission efficiency is improved, and the ionic conductivity of the polymer electrolyte is remarkably improved; and the diaphragm and electrolyte in the traditional battery can be replaced at room temperature, so that the circulation of the all-solid-state battery at a wide temperature range is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid electrolyte materials, and in particular relates to a composite solid electrolyte material introduced with ion fillers, a preparation method and an application thereof. Background Art

[0002] At present, as a key component of energy storage and conversion, the development of electrochemical energy storage devices has attracted much attention. As a key component responsible for ion transmission in energy devices, the performance of electrolytes directly affects the performance of devices such as batteries and capacitors. Traditional lithium-ion batteries use carbonate electrolytes, which are flammable, volatile and leaking at high temperatures, and are highly corrosive, which limits the development of carbonate electrolytes in some important application areas. Therefore, more stable and safer electrolytes are needed to replace electrolytes. Solid electrolytes show great potential in energy storage devices such as batteries because of their excellent chemical stability, thermal stability and mechanical stability.

[0003] Polymer electrolytes are soft and easy to bend, and can maintain good interface contact with electrodes. Compared with inorganic electrolytes, polymer electrolytes have better processing performance, which makes them have the potential for industrial production. Organic-inorganic composite solid electrolytes have become one of the current research hotspots. By rationally combining organic and inorganic materials, the advantages of both can be fully utilized to obtain solid electrolytes with excellent performance. By regulating the morphology and structure of the organic-inorganic interface, the ion transport performance of the solid electrolyte is enhanced, and the interface stability with the electrode is improved. Organic-inorganic composite solid electrolytes not only help to improve the cycle life and safety of the device, but also provide new solutions for the development of high energy density and high power density energy storage devices.

[0004] However, the common composite electrolytes currently have the problem of weak interface interaction between fillers and polymers, and the impedance of the electrolyte and electrode interface is still large, which makes the filler's improvement on the electrochemical performance of the polymer electrolyte not obvious. On the other hand, the existing composite polymer electrolyte materials lack the regulation of microstructure and the design of ion fast transfer channels for the composite filler. These factors lead to poor performance of organic-inorganic composite polymer electrolytes in practical applications. Therefore, it is necessary to propose a new type of composite solid electrolyte material. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a composite solid electrolyte material, preparation method and application of ion fillers. Before the formation of the polymer matrix, inorganic filler particles are preferentially introduced and mixed evenly, then thermally initiated to polymerize to form a polymer-inorganic composite, and then dissolved to form a film, thereby constructing a rapid lithium ion transmission channel, improving the lithium ion transmission efficiency, and significantly improving the ionic conductivity of the polymer electrolyte itself. It can replace the separator and electrolyte in traditional batteries at room temperature, and realize the circulation of all-solid-state batteries under a wide temperature range.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0007] In the first aspect of the present invention, the present invention provides a method for preparing a composite solid electrolyte material introducing an ion filler, wherein the raw materials include a polymer electrolyte, a lithium salt, a filler and a solvent, wherein the polymer electrolyte is polyvinylene carbonate or polyacrylonitrile, and the filler is a sulfide solid electrolyte Li 10 SnP2S 12 , the solvent is N,N-dimethylformamide and / or dimethyl sulfoxide; the steps are as follows:

[0008] (1) Filler Li 10 SnP2S 12 Mix well with the monomer, add azobisisobutyronitrile as a free radical polymerization initiator, and react at 60-80°C for 1-24h to obtain a polymer electrolyte / Li 10 SnP2S 12 Complex;

[0009] (2) Polymer electrolyte / Li 10 SnP2S 12 The complex and the lithium salt are uniformly mixed in a solvent to obtain a mixture;

[0010] (3) Drying the mixture into a film to obtain a composite solid electrolyte material.

[0011] Preferably, in step (1), the mass ratio of the free radical polymerization initiator azobisisobutyronitrile to the monomer is 1:(271-1355).

[0012] Preferably, in step (1), in the polymer electrolyte / Li 10 SnP2S 12 In the composite, filler Li 10 SnP2S 12 The mass of polymer electrolyte / Li 10 SnP2S 12 0.05-0.5% of the total mass of the composite.

[0013] Preferably, in step (2), the polymer electrolyte / Li 10 SnP2S 12 The mass ratio of the complex to the lithium salt is 1:(0.5-2).

[0014] Preferably, in step (2), the solvent and the polymer electrolyte / Li 10 SnP2S 12 The mass ratio of the complex is (15-20 ml):1 g.

[0015] Preferably, the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium bis(fluorosulfonyl)imide salt, lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate, and lithium dioxalatoborate.

[0016] Preferably, in step (3), the mixture is poured onto a polypropylene plate and dried in a water-free and oxygen-free environment.

[0017] More preferably, in step (3), the drying temperature is 60 to 100° C. and the drying time is 6 to 24 hours.

[0018] In a second aspect of the present invention, the present invention provides a composite solid electrolyte material introduced with ion fillers, which is prepared by the above-mentioned preparation method.

[0019] Preferably, the composite solid electrolyte material is in a film shape with a thickness of 50 to 400 μm.

[0020] In a third aspect of the present invention, the present invention provides an application of a composite solid electrolyte material introduced with ion fillers, and the composite solid electrolyte material is applied in the field of ion conductors or lithium ion batteries.

[0021] Beneficial effects:

[0022] The present invention first mixes the filler with vinylene carbonate monomer to form a composite, the polymer electrolyte / Li 10 SnP2S 12 The composite is based on a polymer electrolyte, and then the filler-containing composite and lithium salt are innovatively dissolved in DMF to make the filler Li 10 SnP2S 12 React with the solvent to partially convert the original solid filler into Sn in the polymer electrolyte. 4+ , S 2- PO4 3- There are various forms of ions. After the lithium salt is dissolved, Sn 4+Ions can anchor more anions, allowing more lithium ions to participate in ion transport, introducing the appearance of ions, and producing more lithium ion fast transfer areas with the polymer electrolyte matrix and residual solvents, forming a lithium ion fast transfer network, which promotes the transmission of lithium ions and replaces the separators and electrolytes in traditional batteries at room temperature, realizing the circulation of all-solid-state batteries under a wide temperature range. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The surface and cross-section scanning electron microscope photos of the composite polymer solid electrolyte material prepared in Example 1;

[0024] Figure 2 The graph is a relationship between the conductivity of the composite polymer solid electrolytes obtained under different conditions and the temperature in Examples 1, 2, 3, 4 and Comparative Examples 1 and 2;

[0025] Figure 3 Schematic diagram of ionic conductivity of composite polymer solid electrolytes with different filler contents at 30° C. prepared in Examples 1, 5, 6, 7, 8 and Comparative Example 1;

[0026] Figure 4 Schematic diagram of ionic conductivity of different composite polymer solid electrolytes prepared in Comparative Examples 2, 3, 4, 5, 6, 7, and 8 at 30°C;

[0027] Figure 5 The cycle performance diagram of an all-solid-state lithium metal battery assembled using the composite polymer solid electrolyte prepared in Example 1, a lithium iron phosphate positive electrode and a lithium metal negative electrode at 30°C;

[0028] Figure 6 This is a charge and discharge cycle performance diagram of a lithium symmetric battery using the composite polymer solid electrolyte prepared in Example 1. DETAILED DESCRIPTION

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the specific implementation methods of the present invention will be described below with reference to the accompanying drawings. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.

[0030] The present invention provides a composite solid electrolyte material with an ion filler, wherein the raw materials include a polymer electrolyte, a lithium salt, a filler and a solvent, wherein the polymer electrolyte is polyvinyl carbonate or polyacrylonitrile (PAN), the lithium salt includes one or more of bistrifluoromethanesulfonyl imide lithium, lithium trifluoromethanesulfonate (LiOTf), bisfluorosulfonyl imide lithium salt (LiFSI), lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium difluorooxalatoborate (LiODFB), and lithium dioxalatoborate (LiBOB), and the filler is a sulfide solid electrolyte Li 10 SnP2S 12 , the solvent is N,N-dimethylformamide (DMF) and / or dimethyl sulfoxide (DMSO).

[0031] Preferably, the composite solid electrolyte material is in a film shape with a thickness of 50 to 400 μm.

[0032] The present invention also provides a preparation method for preparing the composite solid electrolyte material, the steps are as follows:

[0033] (1) Filler Li 10 SnP2S 12 Mix well with the monomer, add azobisisobutyronitrile as a free radical polymerization initiator, and react at 60-80°C for 1-24h to obtain a polymer electrolyte / Li 10 SnP2S 12 Complex;

[0034] (2) Polymer electrolyte / Li 10 SnP2S 12 The complex and the lithium salt are uniformly mixed in a solvent to obtain a mixture;

[0035] (3) Drying the mixture into a film to obtain a composite solid electrolyte material.

[0036] Taking vinylene carbonate as a polymer electrolyte, the present invention first mixes the filler with the vinylene carbonate monomer solution, and then forms a new composite by thermal initiation polymerization. 10 SnP2S 12 The composite matrix and lithium salt are dissolved in the solvent to make the filler Li 10 SnP2S 12 Further reaction with solvent (such as DMF) to form Sn 4+ , S 2- PO4 3- Then the solvent is dried out on a heating table. However, it is worth noting that DMF will not be completely dried due to the complex structure of DMF and lithium ions. After the electrolyte membrane is formed, on the one hand, Sn 4+Ions can anchor the anions in the original lithium salt, causing more free lithium ions to appear in the electrolyte membrane. On the other hand, the filler Li 10 SnP2S 12 After reacting with the solvent, some free lithium ions will also appear. These factors lead to more lithium ions participating in ion transport. During the transmission process in the electrolyte membrane, lithium ions are complexed with the C=O matrix of the polymer matrix and the C=O group in DMF. 2- PO4 3- In the subsequent electrochemical cycle, it combines with lithium ions to promote the formation of SEI film containing substances such as Li2S and Li3P, thereby improving the stability of the electrolyte membrane on the lithium metal side. The present invention introduces ions through the reaction of fillers and solvents, generates more free lithium ions with the polyvinyl carbonate matrix and residual solvent, forms a lithium ion fast transmission area and fast transmission network, and promotes the transmission of lithium ions.

[0037] During the preparation process, the filler is evenly mixed with polyvinyl carbonate, and in the subsequent mixing process with the solvent, it reacts with DMF to form a variety of ion fillers evenly dispersed in the polyvinyl carbonate matrix. The introduced ions are evenly dispersed in the composite solid electrolyte material, and together with the residual solvent, form an ion fast transmission area, which has a significant effect on improving the ion conductivity in lithium-ion batteries.

[0038] In existing composite electrolyte materials, inorganic filler particles are generally evenly dispersed in polymer electrolytes, and the fast transfer area at the interface between polymer electrolytes and inorganic fillers is used to promote the improvement of ionic conductivity. The present invention dissolves the inorganic filler and uses the residual solvent in the composite solid electrolyte material and the reaction between the solvent and the filler to form an ionic filler. The introduction of ionic fillers constructs a lithium ion fast transfer channel, improves the lithium ion transfer efficiency, and significantly improves the ionic conductivity of the polymer electrolyte itself, so that the composite solid electrolyte material prepared by the present invention can replace the diaphragm and electrolyte in traditional batteries at room temperature, and realize the circulation of all-solid-state batteries at a wide temperature. Since there is no liquid electrolyte in the battery, the battery does not need to be equipped with an additional temperature control system.

[0039] In step (1), the reaction temperature and reaction time are preferably 12 to 24 hours at 60°C and 1 to 12 hours at 80°C.

[0040] In a preferred embodiment, in step (1), the mass ratio of the free radical polymerization initiator azobisisobutyronitrile to the monomer is 1:(271-1355), preferably 1:500.

[0041] In a preferred embodiment, in step (1), in the polymer electrolyte / Li 10 SnP2S 12In the composite, filler Li 10 SnP2S 12 The mass of polymer electrolyte / Li 10 SnP2S 12 0.05-0.5% of the total mass of the composite, more preferably, the filler Li 10 SnP2S 12 The mass of polymer electrolyte / Li 10 SnP2S 12 0.1-0.5% of the total mass of the composite.

[0042] In a preferred embodiment, in step (2), the polymer electrolyte / Li 10 SnP2S 12 The mass ratio of the complex to the lithium salt is 1:(0.5-2).

[0043] In a preferred embodiment, in step (2), the solvent and the polymer electrolyte / Li 10 SnP2S 12 The mass ratio of the complex is (12-20 ml):1 g.

[0044] In a preferred embodiment, in step (3), the mixture is poured onto a polypropylene plate, and the mixture is dried in a water-free and oxygen-free environment at a temperature of 60 to 100° C. for 6 to 24 hours.

[0045] The composite solid electrolyte material prepared by the present invention has a thermal conductivity of 1.5×10 -3 S cm -1 The ionic conductivity and electrochemical window of about 4.6V can be applied in the field of ion conductors or lithium-ion batteries.

[0046] Taking the application of the present invention in the field of lithium-ion batteries as an example, the composite solid electrolyte material prepared by the present invention is used as a solid electrolyte and is located between the positive electrode and the negative electrode.

[0047] The technical solution of the present invention is described in detail below with specific embodiments.

[0048] The raw materials used in the following Examples 1-8 are as follows:

[0049] Organic monomer solution: vinylene carbonate, purchased from Aladdin Company.

[0050] Initiator: Azobisisobutyronitrile (AIBN), purchased from Aladdin.

[0051] Lithium salt: Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), purchased from Aladdin.

[0052] Organic solvent: N,N-dimethylformamide (DMF), with anhydrous grade purity of 99.8%, purchased from Aladdin Company.

[0053] Inorganic filler Li 10 SnP2S 12 Preparation:

[0054] Under the protection of argon atmosphere, Li2S, P2S5, SnS2 powders of corresponding weight were weighed according to the molar mass ratio of Li2S: P2S5: SnS2 = 5: 1: 1. In order to ensure the full progress of the reaction and reduce the impurity phase, 2% of Li2S powder was additionally added.

[0055] In order to make the powders mixed evenly and further improve the purity of the product, the above powders were added to a zirconia planetary ball mill, and vacuum ball milling was used to evenly mix and refine the powders, wherein the mass ratio of grinding balls to mixed powders was 40:1, the ball milling time was 4 hours, and the rotation speed was 400 rpm.

[0056] About 0.5g of the powder obtained after ball milling is evenly poured into the cold press mold, and the pressure is maintained at 5t for 1min. Then the obtained block sample is crushed and placed in a quartz tube for vacuum sealing. Finally, the preparation is completed by heat treatment. The heat treatment process is: heating to 600℃ at 0.5℃ / min, keeping warm for 24h, and then cooling with the furnace.

[0057] Example 1

[0058] (1) 5 ml (i.e. 6.775 g) of vinyl carbonate monomer was weighed and mixed with 0.01 g of Li 10 SnP2S 12 After the powders were mixed evenly, 0.005 g of initiator azobisisobutyronitrile was added and the mixture was kept at 80 °C for 3 h to polymerize vinylene carbonate into polyvinylene carbonate by thermal polymerization, thus obtaining polymer electrolyte / Li 10 SnP2S 12 Complex.

[0059] (2) Weigh 1 g of polymer electrolyte / Li 10 SnP2S 12 The complex and 2 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 20 mL (ie, 18.96 g) of N,N-dimethylformamide (DMF) and stirred at room temperature for 12 h to obtain a mixture.

[0060] (3) The mixture was poured onto a clean polypropylene plate and then dried at 60 °C for 12 h under an argon atmosphere to obtain a Li-containing 10 SnP2S 12 Polyvinylene carbonate-based composite solid electrolyte with filler.

[0061] The surface and cross-sectional morphology of the composite solid electrolyte prepared in Example 1 are as follows: Figure 1 shown.

[0062] The composite solid electrolyte prepared in Example 1 was sandwiched between two polished stainless steel substrates to form a blocking electrode. The composite solid electrolyte in the blocking electrode was subjected to AC impedance analysis at different temperatures in a constant temperature box using an electrochemical workstation, and the corresponding ionic conductivity at different temperatures was obtained. The relationship between the conductivity and temperature of the composite polymer electrolyte prepared in Example 1 in a wide temperature range is shown in Figure 2. Figure 2 shown.

[0063] The composite solid electrolyte prepared in Example 1 was assembled with lithium iron phosphate as the positive electrode and lithium metal as the negative electrode into an all-solid-state lithium metal battery. The cycle performance of the battery at 30°C and 2C was as follows: Figure 5 As shown. After 5000 cycles, the discharge capacity is 90.8 mAh g -1 , with about 73% capacity remaining.

[0064] The composite polymer electrolyte prepared in Example 1 was assembled with lithium metal into a lithium symmetric battery. -2 Cyclic performance under conditions such as Figure 6 As shown, it can run stably for 1000h.

[0065] Example 2

[0066] (1) The same as step (1) of Example 1, to obtain a polymer electrolyte / Li 10 SnP2S 12 Complex.

[0067] (2) Weigh 1g polymer electrolyte / Li 10 SnP2S 12 The complex and 1.5 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 18 mL (ie, 17.04 g) of N,N-dimethylformamide (DMF) and stirred at room temperature for 12 h to obtain a mixture.

[0068] (3) The mixture was cast on a clean polypropylene plate and then dried at 60° C. for 12 h under an argon atmosphere to obtain the composite solid electrolyte of Example 2.

[0069] The method for testing the ionic conductivity versus temperature curve in Example 1 is the same as that in Example 1. The relationship between the conductivity and temperature of the composite solid electrolyte prepared in Example 2 in a wide temperature range is as follows: Figure 2 shown.

[0070] Example 3

[0071] (1) The same as step (1) of Example 1, to obtain a polymer electrolyte / Li 10 SnP2S 12 Complex.

[0072] (2) Weigh 1g polymer electrolyte / Li 10 SnP2S 12 The complex and 1 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 15 mL (ie, 14.22 g) of N,N-dimethylformamide (DMF) and stirred at room temperature for 12 h to obtain a mixture.

[0073] (3) The mixture was cast on a clean polypropylene plate and then dried at 60° C. for 12 h under an argon atmosphere to obtain the composite solid electrolyte of Example 3.

[0074] The method for testing the ionic conductivity versus temperature curve in Example 1 is the same as that in Example 1. The relationship between the conductivity and temperature of the composite solid electrolyte prepared in Example 3 under a wide temperature range is as follows: Figure 2 shown.

[0075] The composite solid electrolyte prepared in Example 3 was assembled with lithium iron phosphate as the positive electrode and lithium metal as the negative electrode into an all-solid-state lithium metal battery. After 500 cycles at 30°C and 1C, the battery still had a capacity of 138.3 mAh·g -1 The discharge capacity.

[0076] Example 4

[0077] (1) The same as step (1) of Example 1, to obtain a polymer electrolyte / Li 10 SnP2S 12 Complex.

[0078] (2) Weigh 1g polymer electrolyte / Li 10 SnP2S 12 The complex and 0.5 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 12 mL (ie, 11.376 g) of N,N-dimethylformamide (DMF) and stirred at room temperature for 12 h to obtain a mixture.

[0079] (3) The mixture was cast on a clean polypropylene plate and then dried at 60° C. for 12 h under an argon atmosphere to obtain the composite solid electrolyte of Example 4.

[0080] The method for testing the ionic conductivity versus temperature curve in Example 1 is the same as that in Example 1. The relationship between the conductivity and temperature of the composite solid electrolyte prepared in Example 4 in a wide temperature range is as follows: Figure 2 shown.

[0081] Example 5

[0082] (1) 5 ml (i.e. 6.775 g) of vinyl carbonate monomer was weighed and mixed with 0.005 g of Li 10 SnP2S 12 After the powders are mixed evenly, 0.005 g of initiator azobisisobutyronitrile is added. The mixture is kept at 80°C for 3 h to polymerize vinylene carbonate into polyvinylene carbonate by thermal polymerization, thus obtaining polymer electrolyte / Li 10 SnP2S 12 Complex.

[0083] (2) Weigh 1g polymer electrolyte / Li 10 SnP2S 12 The complex and 2 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 20 mL (i.e., 18.96 g) of N,N-dimethylformamide (DMF) and stirred at room temperature for 12 h to obtain a mixture.

[0084] (3) The mixture was poured onto a clean polypropylene plate. Then, it was dried at 60°C for 12 h under an argon atmosphere to obtain a Li 10 SnP2S 12 Polyvinylene carbonate-based composite solid electrolyte with filler.

[0085] The method for testing ionic conductivity is the same as that in Example 1. The relationship between the conductivity and temperature of the composite solid electrolyte prepared in Example 5 under a wide temperature range is as follows: Figure 3 shown.

[0086] Example 6

[0087] 5 ml (6.775 g) of vinyl carbonate monomer was weighed and mixed with 0.015 g of Li 10 SnP2S 12 After the powders are mixed evenly, 0.005 g of initiator azobisisobutyronitrile is added. The mixture is kept at 80°C for 3 h to polymerize vinylene carbonate into polyvinylene carbonate by thermal polymerization, thus obtaining polymer electrolyte / Li 10 SnP2S 12 Complex.

[0088] The subsequent steps are the same as those in Example 1 to obtain a composite solid electrolyte.

[0089] The method for testing ionic conductivity is the same as that in Example 1. The relationship between the conductivity and temperature of the composite polymer electrolyte prepared in Example 6 under a wide temperature range is shown in FIG. Figure 3 shown.

[0090] Example 7

[0091] 5 ml (i.e. 6.775 g) of vinyl carbonate monomer was measured and mixed with 0.02 g of Li 10 SnP2S 12 After the powders are mixed evenly, 0.005 g of initiator azobisisobutyronitrile is added. The mixture is kept at 80°C for 3 h to polymerize vinylene carbonate into polyvinylene carbonate by thermal polymerization, thus obtaining polymer electrolyte / Li 10 SnP2S 12 Complex.

[0092] The subsequent steps are the same as those in Example 1 to obtain a composite solid electrolyte.

[0093] The method for testing ionic conductivity is the same as that in Example 1. The relationship between the conductivity and temperature of the composite solid electrolyte prepared in Example 7 under a wide temperature range is as follows: Figure 3 shown.

[0094] Example 8

[0095] 5 ml (6.775 g) of vinyl carbonate monomer was weighed and mixed with 0.025 g of Li 10 SnP2S 12 After the powders are mixed evenly, 0.005 g of initiator azobisisobutyronitrile is added. The mixture is kept at 80°C for 3 h to polymerize vinylene carbonate into polyvinylene carbonate by thermal polymerization, thus obtaining polymer electrolyte / Li 10 SnP2S 12 Complex.

[0096] The subsequent steps are the same as those in Example 1 to obtain a composite solid electrolyte.

[0097] The method for testing ionic conductivity is the same as that in Example 1. The relationship between the conductivity and temperature of the composite solid electrolyte prepared in Example 8 under a wide temperature range is as follows: Figure 3 shown.

[0098] Comparative Example 1

[0099] Compared with Example 1, the difference is that no inorganic filler is added in this comparative example. The details are as follows:

[0100] 5 ml of vinylene carbonate monomer was measured, and 0.005 g of azobisisobutyronitrile as an initiator was added, and the mixture was kept at 80° C. for 3 hours to polymerize the vinylene carbonate into polyvinylene carbonate by thermal initiation polymerization, thus obtaining polyvinylene carbonate.

[0101] Weigh 1g of polyvinyl carbonate and 2g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), dissolve them in 20mL (i.e. 18.96g) of N,N-dimethylformamide (DMF), stir them continuously at room temperature for 12h, and then pour them on a clean polypropylene plate. Then dry them at 60°C for 12h under argon atmosphere to obtain a solid electrolyte.

[0102] The method for testing ionic conductivity is the same as that in Example 1. The relationship between the conductivity and temperature of the solid electrolyte prepared in Comparative Example 1 under a wide temperature range is shown in FIG. Figure 2 , Figure 3 shown.

[0103] Comparative Example 2

[0104] The preparation of polyvinylene carbonate is the same as that of Comparative Example 1, except that no inorganic filler is added in this comparative example.

[0105] Weigh 1g of polyvinyl carbonate and 1g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), dissolve them in 20mL (i.e. 18.96g) of N,N-dimethylformamide (DMF), stir them continuously at room temperature for 12h, and then pour them on a clean polypropylene plate. Then dry them at 60°C for 12h under argon atmosphere to obtain a solid electrolyte.

[0106] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the solid electrolyte prepared in Comparative Example 2 at 30°C is as follows: Figure 4 shown.

[0107] Comparative Example 3

[0108] The filler used in this comparative example is tin trifluoromethanesulfonate (Sn(OTf)2), which is purchased from Aladdin.

[0109] The preparation of polyvinylene carbonate is the same as that of Comparative Example 1.

[0110] Weigh 1g of polyvinyl carbonate, 1g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 0.005g of tin(OTf)2), dissolve them in 20mL (i.e. 18.96g) of N,N-dimethylformamide (DMF) and stir them continuously at room temperature for 12h, then pour them on a clean polypropylene plate. Then dry them at 60°C for 12h under argon atmosphere to obtain a solid electrolyte.

[0111] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the solid electrolyte prepared in Comparative Example 3 at 30°C is as follows: Figure 4 shown.

[0112] Comparative Example 4

[0113] The filler used in this comparative example is tin disulfide (SnS2), which was purchased from Aladdin.

[0114] The preparation of polyvinylene carbonate is the same as that of Comparative Example 1.

[0115] Weigh 1g of polyvinyl carbonate, 1g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 0.005g of tin disulfide (SnS2), dissolve them in 20mL (i.e. 18.96g) of N,N-dimethylformamide (DMF), stir them continuously at room temperature for 12h, and then pour them on a clean polypropylene plate. Then dry them at 60°C for 12h under argon atmosphere to obtain a solid electrolyte.

[0116] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the solid electrolyte prepared in Comparative Example 4 at 30°C is as follows: Figure 4 shown.

[0117] Comparative Example 5

[0118] In this comparative example, the polymer electrolyte is polyvinylidene fluoride (PVDF), and no inorganic filler is used, and the polymer electrolyte is purchased from Aladdin Corporation.

[0119] Weigh 1g of polyvinylidene fluoride and 1g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), dissolve them in 20mL (i.e. 18.96g) of N,N-dimethylformamide (DMF), stir them continuously at room temperature for 12h, and then pour them on a clean polypropylene plate. Then dry them at 60℃ for 12h under argon atmosphere to obtain a polyvinylidene fluoride based polymer solid electrolyte.

[0120] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the solid electrolyte prepared in Comparative Example 5 at 30°C is as follows: Figure 4 shown.

[0121] Comparative Example 6

[0122] In this comparative example, the polymer electrolyte is polyvinylidene fluoride (PVDF).

[0123] Weigh 1g polyvinylidene fluoride, 0.005g inorganic filler Li 10 SnP2S 12 and 1g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), dissolved in 20mL (i.e. 18.96g) of N,N-dimethylformamide (DMF) and stirred at room temperature for 12h, then poured onto a clean polypropylene plate and dried at 60°C for 12h under an argon atmosphere to obtain a composite solid electrolyte.

[0124] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the composite solid electrolyte prepared in Comparative Example 6 at 30°C is as follows: Figure 4 shown.

[0125] Comparative Example 7

[0126] In this comparative example, the polymer electrolyte is polyethylene oxide (PEO), purchased from Aladdin; the solvent is anhydrous acetonitrile (AN), with an anhydrous grade purity of 99.8% H2O<0.003%, purchased from Aladdin.

[0127] 1 g of polyethylene oxide and 0.4 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed and dissolved in 20 mL of anhydrous acetonitrile (AN) and stirred at room temperature for 12 h, then poured onto a clean polypropylene plate and dried at 60 °C for 12 h under an argon atmosphere to obtain a polymer solid electrolyte.

[0128] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the polymer solid electrolyte prepared in Comparative Example 6 at 30°C is as follows: Figure 4 shown.

[0129] Comparative Example 8

[0130] In this comparative example, the polymer electrolyte is polyethylene oxide (PEO), the solvent is anhydrous acetonitrile (AN), and the inorganic filler is Li 10 SnP2S 12 .

[0131] Weigh 1g polyethylene oxide, 0.005g inorganic filler Li 10 SnP2S 12 and 0.4 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), were dissolved in 20 mL of anhydrous acetonitrile (AN) and stirred at room temperature for 12 h, then poured onto a clean polypropylene plate and dried at 60 °C for 12 h under an argon atmosphere to obtain a composite solid electrolyte.

[0132] The method for testing ionic conductivity is the same as that in Example 1. The ionic conductivity of the polymer electrolyte prepared in Comparative Example 8 at 30°C is as follows: Figure 4 shown.

[0133] Figure 2 The temperature variation curves of ionic conductivity of composite polymer solid electrolytes with different polymer electrolytes, different lithium salt contents and different preparation methods were compared.

[0134] It can be seen from the figure that the electrolyte with the ion filler has higher ion conductivity. Compared with Comparative Example 1, the ion conductivity of the composite polymer solid electrolyte in Example 1 is significantly improved at different temperatures. At 30°C, the ion conductivity in Example 1 is 2.06×10 -3 S cm -1 , compared with 1.13×10 -3 S cm -1 Improved by about 2 times.

[0135] according to Figure 2 It is shown that the ionic conductivity of Examples 3 and 4 is close to that of Comparative Example 1, but in Examples 3 and 4, the amount of lithium salt and filler (containing lithium) used is much lower than that of Comparative Example 1. In the art, an increase in the amount of lithium salt will increase the ionic conductivity of the solid electrolyte, but will increase the weight of the solid electrolyte. Examples 3 and 4 use less lithium salt and filler to achieve the effect that can only be achieved by using more lithium salt in the prior art, indicating that the present invention is conducive to the research on lightweight solid electrolytes.

[0136] Comparing Example 3 with Comparative Example 2, the ionic conductivity after adding filler increased from 0.82×10 -3 S cm -1 Increased to 1.2×10 -3 S cm -1 This indicates that the filler Li is uniformly added to the polymer polyvinylene carbonate. 10 SnP2S 12 After reacting with DMF, the lithium ion conductivity can be effectively improved, and the effect is maintained at different lithium salt contents. Such modification has a certain universality. It should be noted that the ion conductivity mentioned above refers to the attached Figure 2 The σ in the figure is treated as Logσ, and the attached figure is obtained by plotting Figure 2 .

[0137] Preferably, it can be seen from the test results of the lithium metal battery assembled in Example 1 that the composite solid electrolyte has high ionic conductivity and can achieve excellent cycle stability with a high capacity under given test conditions.

[0138] Examples 1, 5, 6, 7, 8 and Comparative Example 1 compare the ionic conductivity at 30°C corresponding to different contents of fillers. Figure 3 The filler content in Comparative Example 1 is 0, and it can be seen that Li 10 SnP2S 12 After the filler reacts with DMF, the ionic conductivity can be significantly improved.

[0139] Comparative Example 3 selected a tin-containing filler tin trifluoromethanesulfonate (Sn(OTf)2) that is soluble in DMF. Using this filler, Sn ions can be directly introduced into the polymer solid electrolyte in the electrolyte membrane. At the same time, Comparative Example 4 introduced a tin-containing filler tin disulfide that is insoluble in DMF. The effects of both on the ionic conductivity of the polymer electrolyte are shown in the figure. Figure 4 As shown. At 30°C, the ionic conductivity of the composite polymer solid electrolyte membrane with 0.5% tin trifluoromethanesulfonate added was significantly improved. At 30°C, the ionic conductivity increased from 0.82 mS·cm in Comparative Example 2 to 0.11 mS·cm in Comparative Example 3. -1 Improved to 1.15mS·cm in Comparative Example 3 -1 However, after adding tin disulfide, a filler that is insoluble in DMF, the ionic conductivity of the polymer electrolyte membrane did not increase but showed a downward trend. This shows that when Sn ions exist in the electrolyte membrane, the electrolyte membrane will promote the formation of a lithium ion fast transfer network, which will promote the improvement of ionic conductivity.

[0140] Comparative Examples 5 and 6 use different polymer matrices, namely polyvinylidene fluoride. Figure 4 It can be clearly seen that the polymer matrix of polyvinylidene fluoride has a weaker lithium ion transmission capacity than polyvinyl carbonate, and the ionic conductivity of both is significantly lower than that of polyvinyl carbonate-based polymer electrolyte at different temperatures. 10 SnP2S 12 After filling, the ionic conductivity still achieved a certain improvement. At 30°C, the ionic conductivity increased from 0.33mS·cm -1 Increased to 0.43mS·cm -1 .

[0141] Comparative Example 7 and Comparative Example 8 chose not to 10 SnP2S 12 The anhydrous acetonitrile of the reaction was used as a solvent to prepare the electrolyte membrane. The polymer matrix selected was polyethylene oxide, which is the most common polymer matrix. The difference between the polymer electrolytes in the two examples is that a small amount of Li 10 SnP2S 12 Filler. The ionic conductivity of the two at 30°C is Figure 4 The ionic conductivity of the polymer electrolyte in Comparative Example 7 is about 8.1×10 -3 mS cm -1 , while the ionic conductivity of the polymer electrolyte in Comparative Example 8 is 7.8×10 -3 mS cm -1 .Li 10 SnP2S 12It cannot react with the solvent AN, but exists in the electrolyte membrane in the form of particles. It cannot provide Sn ions to the electrolyte membrane, and the ionic conductivity is not significantly improved.

[0142] The above examples and comparative examples specifically demonstrate the universality and effectiveness of the technology for preparing polymer solid electrolytes with ion fillers in the present invention for improving the electrochemical performance of polymer-based composite solid electrolytes from four aspects, namely, different solid polymer matrices, different lithium salt contents, different filler contents, and methods for preparing composite polymer electrolytes. This is unique in achieving rapid transfer of lithium ions in the polymer matrix, and ultimately achieving improved ion conductivity and battery performance.

[0143] The embodiments provided by the present invention are described in detail above. Specific examples are used herein to describe the principles and implementation methods of the present invention, and the description of the above embodiments is only used to help understand the core idea of ​​the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a composite solid electrolyte material introducing an ion filler, characterized in that: The raw materials include polymer electrolyte, lithium salt, filler and solvent, wherein the polymer electrolyte is polyvinyl carbonate or polyacrylonitrile, and the filler is sulfide solid electrolyte Li 10 SnP2S 12 , the solvent is N,N-dimethylformamide and / or dimethyl sulfoxide; Here are the steps: (1) Filler Li 10 SnP2S 12 Mix well with the monomer, add azobisisobutyronitrile as a free radical polymerization initiator, and react at 60-80°C for 1-24h to obtain a polymer electrolyte / Li 10 SnP2S 12 Complex; (2) Polymer electrolyte / Li 10 SnP2S 12 The complex and the lithium salt are uniformly mixed in a solvent to obtain a mixture; (3) Drying the mixture into a film to obtain a composite solid electrolyte material.

2. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of the free radical polymerization initiator azobisisobutyronitrile to the monomer is 1:

500.

3. The preparation method according to claim 1, characterized in that: In step (1), in the polymer electrolyte / Li 10 SnP2S 12 In the composite, filler Li 10 SnP2S 12 The mass of polymer electrolyte / Li 10 SnP2S 12 0.05-0.5% of the total mass of the composite.

4. The preparation method according to claim 1, characterized in that: In step (2), the polymer electrolyte / Li 10 SnP2S 12 The mass ratio of the complex to the lithium salt is 1:(0.5-2).

5. The preparation method according to claim 1, characterized in that: In step (2), the solvent and the polymer electrolyte / Li 10 SnP2S 12 The mass ratio of the complex is (15-20 ml):1 g.

6. The preparation method according to claim 1, characterized in that: In step (3), the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium bis(fluorosulfonyl)imide salt, lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate, and lithium dioxalatoborate.

7. The preparation method according to claim 1, characterized in that: In step (3), the drying temperature is 60 to 100° C. and the drying time is 6 to 24 hours.

8. A composite solid electrolyte material introduced with ion fillers, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7.

9. The composite solid electrolyte material according to claim 8, characterized in that: The composite solid electrolyte material is in film form with a thickness of 50 to 400 μm.

10. An application of a composite solid electrolyte material introduced with ion fillers, characterized in that: The composite solid electrolyte material as claimed in claim 8 or 9 is applied in the field of ion conductors or lithium ion batteries.

Citation Information

Patent Citations

  • Composite solid electrolyte prepared based on in-situ thermal polymerization method and preparation method and application thereof

    CN112018430A

  • Solid-liquid mixed polymer electrolyte, battery, preparation method and application

    CN116960449A

  • In-situ cross-linked organic-inorganic composite solid electrolyte, preparation method and application thereof

    CN117613365A

  • Composite quasi-solid electrolyte as well as precursor solution, preparation method and application thereof

    CN118507813A

  • Heat / Flame-Resistant Polymer Composite-Based Solid Electrolyte Separator, Lithium Secondary Battery, and Manufacturing Method

    US20230387548A1