Continuous casting slab and method for producing same

By controlling the original austenite particle size and microstructure structure, combined with the three-stage cooling process, the problems of seasonal cracking and opening failure during rolling of high-strength steel slabs are solved, and the high toughness and finishing rate of slabs are achieved Improvement.

CN119095996APending Publication Date: 2024-12-06JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036466.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-09
Filing Date
2023-03-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art cannot effectively suppress the seasonal cracking of high-strength steel slabs during cooling, and avoid opening failures during rolling, resulting in a decrease in yield.

Method used

By controlling the average original austenite particle size of the continuous cast slab within the range of 0.5 mm to 2.0 mm, and ensuring that the total area ratios of ferrite and pearlite are more than 90% and the area ratio of ferrite is in the microstructure. Less than 5% or 10%, three-stage cooling process is adopted: the first stage of 1200℃~1450℃ retention time is less than 130 seconds, the second stage of 700℃~850℃ average cooling speed does not exceed 20℃/hr, and the third stage The average cooling rate of 500℃~700℃ shall not exceed 10℃/hr.

Benefits of technology

It effectively suppresses the occurrence of seasonal cracks of the slabs, and prevents hole failures during the rolling process, thereby improving the yield rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095996A_ABST
    Figure CN119095996A_ABST
Patent Text Reader

Abstract

The present invention provides a continuously cast slab and a method for manufacturing the same, in which even if the slab is a continuously cast slab having low toughness, seasonal cracking does not occur during cooling of the continuously cast slab. A continuously cast slab for high-strength steel, which is characterized in that the average prior austenite particle size at a position 10 mm from the surface layer of the continuously cast slab is 0.5-2.0 mm, the total of the area ratio of ferrite and the area ratio of pearlite in the microstructure is 90% or more, and the area ratio of ferrite is less than 5% or 10% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a continuous casting slab that prevents cracks during cooling and a method for manufacturing the same. More specifically, the present invention relates to a continuous casting slab for high-strength steel that can effectively prevent season cracks and does not cause hole opening failure during rolling and a method for manufacturing the same. Background Art

[0002] In recent years, in the automotive field, in order to achieve both further thinning of the vehicle body and ensuring collision safety, the strength of high-strength steel has been further increased and high alloying has been carried out for this purpose. However, high alloying will significantly reduce the toughness of the slab.

[0003] As the toughness of the slab due to high alloying decreases, cracks during cooling of the slab, so-called seasonal cracks, frequently occur. If seasonal cracks occur, there is a risk that the slab will break during transportation and the slab cannot be supplied to hot rolling. In addition, even if the slab does not break, there is a risk that cracks will open during hot rolling of the slab and the hot-rolled steel sheet will break. Alternatively, even if the cracks in the slab are small, they will appear as surface defects such as peeling and streaks on the steel sheet after hot rolling, cold rolling, annealing or plating. Usually, cracks on the surface of the slab are removed by a grinder. However, due to the high alloying, the toughness of the slab is reduced, so the cracks in the slab expand due to the stress of the grinder, and sometimes the cracks in the slab cannot be completely removed. On the other hand, small cracks in the slab are sometimes ignored and appear as surface defects on the steel sheet after hot rolling, cold rolling, annealing or plating. Therefore, it is necessary to suppress cracks in the slab.

[0004] Figure 1 This is an enlarged photograph of a cross section of a high-strength steel slab that broke due to seasonal cracking, taken using a scanning electron microscope (SEM). Figure 1 It can also be seen that the cross section of the cracked portion of the slab appears to be a grain boundary cross section along the original austenite grain boundary. Figure 2 The cross section of the slab crack is shown in the microstructure photo. The depth of the slab crack is mainly about 20 mm from the surface of the slab. The slab crack propagates near the original austenite grain boundary, and there is grain boundary ferrite at the front end of the slab crack. In addition, pearlite or pearlite and bainite are observed in the original austenite grains.

[0005] Grain boundary fracture occurs when the original austenite grains are coarse and the grain boundaries are embrittled. It is easier to generate precipitates and ferrite at the grain boundaries than in the grains. The precipitates at the grain boundaries become the main reason for reducing the grain boundary strength and reducing the toughness of the slab. If the original austenite grains are coarse, the proportion of the grain boundaries decreases, the precipitate density increases, and the grain boundaries become further embrittled. In addition, when grain boundary ferrite is generated, due to the strength difference with the pearlite and bainite in the grains, stress concentration occurs in the grain boundary ferrite part with low strength, and even with a lower stress, it expands into a crack in the slab. Similarly, if the original austenite grains are coarse, the grain boundary ferrite extending in a straight line and thinly precipitates, so it is impossible to prevent the expansion of the slab cracks, and the damage caused by the cracks of the slab is expanded. On the other hand, when the slab is cooled, stress caused by the difference in thermal contraction and phase change expansion between the surface and the inside of the slab is generated. If this stress is large, the slab cracks occur when the slab is cooled to room temperature. In recent years, high-alloy high-strength steel has low slab toughness, so deep cracks in the slab generated in this way are difficult to remove by processing such as grinding, which has caused a problem of significantly reducing the yield of the slab.

[0006] From this point of view, a method for suppressing the occurrence of seasonal cracks in high-tensile steel slabs has been proposed. For example, Patent Document 1 proposes the following method: by slowly cooling the temperature range of 700-500°C from austenite to ferrite, the bainite / martensite phase transformation is suppressed, and the stress generated by the phase transformation expansion is reduced. That is, Patent Document 1 discloses a method for suppressing the occurrence of seasonal cracks even in steel types that are prone to seasonal cracks in high-tensile steel. Specifically, the cooling method for high-tensile steel slabs disclosed in Patent Document 1 is based on the understanding that the internal stress of high-tensile steel depends on its cooling rate, and the cooling rate of the slab is controlled according to the length of the internal cracks generated in the high-tensile steel, thereby suppressing the occurrence of seasonal cracks.

[0007] In addition, Patent Document 2 proposes the following method: slow cooling starts immediately after the casting of the slab, lasts for more than 10 hours at a temperature of 700°C or more, and further slow cooling is performed to a temperature of 700-500°C, thereby reducing the temperature difference and stress during phase transformation. That is, Patent Document 2 discloses a cooling method for a slab for high-strength steel plate, which not only does not cause slab cracks during cooling of the slab, but also does not cause quality defects such as peeling during hot rolling, even for a slab containing Si. Specifically, the cooling method for a slab for high-strength steel plate disclosed in Patent Document 2 sets the average cooling rate of 500-700°C of a continuously cast slab of a high-strength hot-rolled steel plate with limited contents of chemical components such as C, Si, and Mn to less than 20°C / hr.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2020-139209

[0011] Patent Document 2: Japanese Patent Application Publication No. 2019-167560 Summary of the invention

[0012] However, the above-mentioned prior art has the following problems. The method of cooling a high-tensile steel slab after casting described in Patent Document 1 only focuses on the temperature range from 700°C to 500°C when the slab is cooled after casting, and controls the internal stress generated in the slab to be reduced. However, in recent years, since the toughness of the slab is low in highly alloyed high-strength steel, the state of the original austenite grain boundary where the seasonal crack propagates has become very important. In the method described in Patent Document 1, since the original austenite grain size and grain boundary ferrite are not controlled, even if the method for cooling a high-tensile steel slab described in Patent Document 1 is used to manufacture a slab with an increased carbon content, the occurrence of seasonal cracks in the slab cannot be fully suppressed.

[0013] Furthermore, the cooling method for a high-strength steel plate described in Patent Document 2 is based on the knowledge that the cause of slab cracks is the thermal stress generated by the addition of Si to steel and the temperature unevenness in the slab, and focuses on reducing the thermal stress to suppress the cracks in the slab. However, the cooling method for a high-strength steel plate described in Patent Document 2 does not limit the microstructure of the slab. Therefore, even if the slab is manufactured using the cooling method for a high-strength steel plate described in Patent Document 2, the occurrence of seasonal cracks in the slab cannot be fully suppressed.

[0014] In addition, the inventors of the present invention conducted intensive research and found that in the slabs containing a large amount of C, Si, and Mn in the prior art, the toughness is quite low, the seasonal crack cannot be completely suppressed, and the opening failure occurs during rolling.

[0015] The present invention is completed in view of the above situation, and its purpose is to provide a continuous casting slab and a manufacturing method thereof, wherein even if the continuous casting slab has low toughness, seasonal cracks of the slab will not occur during the cooling of the slab, and no hole opening failure will occur during rolling.

[0016] The inventors have repeatedly conducted in-depth research to achieve the above-mentioned purpose. As a result, after analyzing the fracture morphology of the slab crack, it was found that the cross section has at least one of the grain boundary cross section along the original austenite grain boundary and the intragranular cross section (cleavage cross section) across the original austenite grain boundary. Furthermore, the inventors have repeatedly conducted detailed research and clarified that the seasonal cracking of the slab cannot be suppressed only by controlling the cooling rate and reducing the stress reduction caused by temperature unevenness, and the morphology of the microstructure also has a great influence. Specifically, it was found that by controlling the average original austenite grain size and microstructure of the continuously cast slab to improve its toughness, the seasonal cracking of the slab during the cooling process of the continuously cast slab can be suppressed and the hole opening failure can be avoided during rolling, thereby completing the present invention.

[0017] That is, the continuous casting slab of the present invention which advantageously solves the above-mentioned problem is a continuous casting slab for high-strength steel, characterized in that the average original austenite grain size at a position 10 mm away from the surface of the continuous casting slab is 0.5 mm to 2.0 mm, and in the microstructure, the total of the area ratio of ferrite and the area ratio of pearlite is more than 90%, and the area ratio of the above-mentioned ferrite is less than 5% or is more than 10%.

[0018] It should be noted that the continuous cast slab (a) of the present invention contains, by mass%, C: 0.10% to 1.00%, Si: 0.10% to 2.50%, Mn: 0.40% to 5.00%, etc., which may become a more preferable solution.

[0019] Furthermore, the method for producing a continuously cast slab of the present invention is a method for producing a continuously cast slab for high-strength steel in which seasonal cracks of the slab caused by cooling are suppressed, and is characterized by comprising:

[0020] In a first cooling step, the continuously cast slab having the composition described in (a) is cooled at a cooling temperature of 1200° C. to 1450° C. at a position 10 mm from the surface of the continuously cast slab and at a center in the width direction of the continuously cast slab, and the residence time of the continuously cast slab is 130 seconds or less;

[0021] A second cooling step is performed under cooling conditions in which the surface temperature of the center of the continuous cast slab in the width direction is 700°C to 850°C and the average cooling rate is 20°C / hr or less; and

[0022] The third cooling step is performed under cooling conditions in which the surface temperature of the center of the continuous cast slab in the width direction is 500°C to 700°C and the average cooling rate is 10°C / hr or less.

[0023] According to the present invention, it is possible to provide a continuously cast slab which does not cause seasonal cracking during cooling and does not cause hole opening failure during rolling even if it is a composition system of a continuously cast slab for high-strength steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The photograph was taken using a scanning electron microscope (SEM) of a cross section of a cracked portion of a high-strength steel continuous cast slab that was fractured due to seasonal cracking.

[0025] Figure 2 This is a cross-sectional microstructure photograph of the above-mentioned crack.

[0026] Figure 3 This is an enlarged photograph of a continuously cast slab produced in the invention example (test No. D-9) of the continuously cast slab according to the embodiment of the present invention observed with an optical microscope. DETAILED DESCRIPTION

[0027] The following is a detailed description of the embodiments of the present invention. It should be noted that the drawings are schematic and sometimes different from the actual ones. In addition, the following embodiments illustrate the devices and methods for implementing the technical ideas of the present invention, and do not define the composition as the following. That is, the technical ideas of the present invention can be modified in various ways within the technical scope described in the scope of the patent claim.

[0028] [First embodiment]

[0029] The continuous casting slab of the first embodiment is described. The continuous casting slab of the present embodiment is a continuous casting slab for high-strength steel, characterized in that (i) the average original austenite grain size at a position 10 mm from the surface of the continuous casting slab is 0.5 mm to 2.0 mm, (ii) in the microstructure, the total area ratio of ferrite and the area ratio of pearlite is 90% or more, and (iii) the area ratio of the above ferrite is less than 5% or 10% or more. That is, according to the invention of the present embodiment, by having at least the above characteristics (i) to (iii), a continuous casting slab for high-strength steel can be provided, which does not cause slab seasonal cracking during cooling, can prevent hole opening failures during rolling, and has a good yield rate even if the continuous casting slab has very low toughness.

[0030] First, the appropriate range and reasons for limiting the microstructure of the continuously cast slab are described. It should be noted that in the following description, unless otherwise specified, the "%" indicating the composition ratio of the microstructure means "area %". In addition, the observation of the microstructure of the continuously cast slab is carried out at room temperature.

[0031] As described above, the fracture morphology of the cross section of the cracked part of the high-strength steel continuous casting slab that broke due to seasonal cracking was observed, and it was determined that most of the fractures had extended to about 20 mm below the surface of the slab, and were in the form of "grain boundary fracture" in which the cracks extended to the original austenite grain boundaries. That is, in the high-strength steel continuous casting slab, the main cause of seasonal cracking caused by the fracture of the grain boundaries is the coarse original austenite grain size and the presence of the grain boundary ferrite structure that becomes a factor that makes the grain boundaries embrittled. In high-alloy high-strength steel plates, the toughness of the continuous casting slab is originally very low. In addition, when these embrittlement factors exist, even if the slab is slowly cooled to reduce the stress, seasonal cracking cannot be suppressed. Therefore, in this embodiment, as a necessary condition for the high-strength steel continuous casting slab that does not cause seasonal cracking during the cooling process, attention is paid to the two phenomena consisting of (i) the average original austenite grain size at a predetermined position from the surface of the continuous casting slab and (ii) to (iii) the microstructure of the above-mentioned continuous casting slab.

[0032] <About (i) Average prior austenite grain size>

[0033] The high-strength steel continuous casting slab of the present embodiment is a high-strength steel continuous casting slab in which the seasonal cracking caused by cooling is suppressed, characterized in that (i) the average original austenite grain size at a position 10 mm from the surface of the continuous casting slab is 0.5 mm to 2.0 mm. Here, the average original austenite grain size is a factor that determines the fracture unit of the slab. Since the solute component is easily enriched at the grain boundary, it has the characteristic that the precipitate is easily concentrated. That is, the larger the average original austenite grain size, the smaller the grain boundary ratio per unit volume, so the precipitate density increases, thereby reducing the toughness of the continuous casting slab. Here, the average original austenite grain size refers to the value obtained by averaging the values ​​of multiple original austenite grain sizes calculated based on the original austenite grain sizes measured in multiple fields of view.

[0034] In the previous continuous casting slab, the average original austenite grain size is several mm in size, which is very large. Therefore, the toughness of the continuous casting slab is greatly reduced. In the previous low alloy steel, since the toughness of the original continuous casting slab is also high, the average original austenite grain size is not a problem, but in high alloy high strength steel, the average original austenite grain size may become a very serious problem. Therefore, the continuous casting slab of the present embodiment sets the average original austenite grain size at a position of 10mm from the surface of the continuous casting slab to less than 2.0mm. If the average original austenite grain size is less than 2.0mm, the precipitates concentrated on the original austenite grain boundaries can be dispersed, and the toughness of the continuous casting slab is not reduced, so it is preferred.

[0035] On the other hand, the lower limit of the average original austenite grain size is not strictly limited, but in order to make the average original austenite grain size smaller than 0.5 mm, for example, strong cooling is required at the initial stage of solidification. In this case, there is a risk of uneven solidification and breakout. Therefore, the lower limit of the average original austenite grain size is preferably 0.5 mm or more. It should be noted that the lower limit of the average original austenite grain size is preferably 0.8 mm or more, and more preferably 1.0 mm or more.

[0036] The average original austenite grain size is the grain size of the crystal grains constituting the original austenite structure at a position 10 mm from the surface of the continuous casting slab. Here, when setting the average original austenite grain size, the reason why it is set as the position 10 mm from the surface of the continuous casting slab is that most of the seasonal cracks of the slab have extended to about 20 mm below the surface of the slab, so it is considered that the position 10 mm from the surface of the continuous casting slab is the necessary position to suppress the seasonal cracks of the slab.

[0037] On the other hand, the area less than 5 mm from the surface of the continuous casting slab is directly quenched by the mold or the water sprayer directly below the mold. Therefore, the γ grain size of the continuous casting slab is a fine structure, the toughness of the slab is high, and it is difficult to generate the starting point of the season crack from this area. Therefore, the area less than 5 mm from the surface of the continuous casting slab can be excluded from the position where the slab structure needs to be controlled. Therefore, the position where the continuous casting slab structure needs to be controlled is the position of 10 mm depth in the thickness direction of the slab, for example, based on the position of 10 mm from the surface of the continuous casting slab, for example, it can also be 5 to 20 mm deep from the surface of the continuous casting slab.

[0038] In the continuous casting slab of the present embodiment, the factor that determines the average original austenite grain size is the temperature when the continuous casting slab is cooled. The temperature of cooling the continuous casting slab is particularly in the range of 1450°C to 1200°C, and its residence time will have an impact. Furthermore, the longer the residence time of the continuous casting slab, the coarser the average original austenite grain size. That is, in order for the continuous casting slab of the present embodiment to satisfy (i) the condition that the average original austenite grain size at a position 10mm from the surface of the continuous casting slab is 0.5mm to 2.0mm, it is important to control the residence time of the continuous casting slab at 1450°C to 1200°C. Specifically, it is preferred that the residence time of the continuous casting slab at a position of 10mm from the surface of the slab in the thickness direction at 1450°C to 1200°C is less than 130s.

[0039] If the residence time of the continuously cast slab at 1450°C to 1200°C is less than 130s, the average original austenite grain size can be made less than 2.0mm. By controlling the average original austenite grain size to be small, the precipitates and grain boundary ferrite can be dispersed, the toughness of the slab can be improved, and the seasonal cracking of the slab can be suppressed, so it is preferred.

[0040] Furthermore, from such a viewpoint, the residence time of the continuously cast slab is preferably 120 s or less, more preferably 110 s or less, and even more preferably 100 s or less.

[0041] In addition, the lower limit of the residence time of the continuously cast slab is not particularly limited, but if the residence time is too short, the risk of steel breakout in continuous casting due to uneven solidification increases, so it is set to 40 seconds or more.

[0042] That is, if the residence time of the continuously cast slab at 1450°C to 1200°C is less than 40 seconds, there is a risk of cracking caused by uneven solidification and thus leakage, so it is preferably 40 seconds or more. From this point of view, the residence time of the continuously cast slab at 1450°C to 1200°C is more preferably 60 seconds or more, and even more preferably 70 seconds or more.

[0043] The residence time of the continuously cast slab can be controlled by adjusting the cooling conditions in the initial stage of slab casting. For example, in the continuous casting of steel, molten steel with adjusted composition is first injected into a water-cooled copper mold to form an initial solidified shell. Then drawing begins, and cooling using a water sprayer is implemented after it comes out of the water-cooled copper mold. The surface temperature of the slab in the above range is greatly affected by the cooling in the mold and directly below the mold, so for example, the thermal conductivity of the protective slag used for lubrication in the mold can be increased, or it can be controlled by increasing the flow rate of the water sprayer directly below the mold.

[0044] By controlling these cooling conditions, the average original austenite grain size 10 mm below the surface of the continuous casting slab can be controlled. It is difficult to measure the cooling temperature of the continuous casting slab. Therefore, the temperature history at the position 10 mm below the surface of the continuous casting slab in the slab thickness direction can be calculated by heat transfer analysis, taking the area from the depth of 5 mm to the depth of 20 mm from the surface of the continuous casting slab in the slab thickness direction as a representative, and estimating the cooling temperature of the continuous casting slab. In the interior of the continuous casting slab, in order to maximize the residence time in the above-mentioned temperature range, the heat transfer analysis position can be set at the center of the above-mentioned continuous casting slab width.

[0045] <For (ii) to (iii) Microstructure of Continuously Cast Slab>

[0046] The continuous casting slab of the present embodiment is characterized in that (ii) in the microstructure, the total area ratio of ferrite and the area ratio of pearlite is 90% or more, and (iii) the area ratio of ferrite is less than 5% or 10% or more. That is, it is known that in addition to the average original austenite grain size of 2.0 mm or less at a position 10 mm from the surface of the continuous casting slab, the ratio of internal structures such as bainite and ferrite is also a factor that determines the fracture unit, and the toughness of the slab is improved by an appropriate ratio. Therefore, the inventors found that by controlling the cooling rate, (ii) the total area ratio of ferrite and the area ratio of pearlite in the microstructure is 90% or more, and (iii) the area ratio of ferrite is less than 5% or 10% or more, the toughness of the slab is improved. It should be noted that the area ratio of ferrite and the area ratio of pearlite can be calculated based on the observation results of the microstructure of the continuous casting slab using an optical microscope or other observation means. In addition, the ferrite and pearlite contained in the microstructure of the continuous casting slab can be identified using an optical microscope or other observation means.

[0047] According to the identification results of the microstructure of the continuous casting slab, the area S of the microstructure of the continuous casting slab is calculated. total , and the area S of ferrite ferrite and the area of ​​pearlite S pearlite The total area S (ferrite+pearlite) Then, the area S of ferrite ferrite and the area of ​​pearlite S pearlite The total area S (ferrite+pearlite) Relative to the area S of the microstructure of the continuous casting slab total The ratio is defined as the area ratio (%) and calculated.

[0048] The continuous casting slab of the present embodiment is characterized in that (ii) in the microstructure, the total area ratio of ferrite and the area ratio of pearlite is 90% or more. That is, in the continuous casting slab of the present embodiment, (ii) if the area ratio of ferrite S ferrite and the area of ​​pearlite S pearlite The total area S (ferrite+pearlite) Relative to the area S of the microstructure of the continuous casting slab total When the area ratio (%) of the ratio is 90% or more, the thermal stress and phase transformation stress caused by the bainite-martensite phase transformation during the slow cooling of the slab can be reduced. In addition, these generated stresses are also dispersed in the ferrite-pearlite that exists sufficiently in the microstructure, which can improve the toughness of the continuously cast slab, so it is preferred. On the other hand, if the above area ratio is less than 90%, the toughness of the continuously cast slab decreases, so it is not preferred.

[0049] Furthermore, the continuous casting slab of the present embodiment is characterized in that (iii) the area ratio of ferrite is less than 5% or is greater than 10%. That is, in the continuous casting slab of the present embodiment, when the area ratio of ferrite is greater than 5% and less than 10%, there is a state in which thin ferrite exists at the grain boundary, stress is concentrated in the soft ferrite part, and cracks propagate, so it is not preferred. If the area ratio of ferrite is less than 5%, even if cracks propagate, they stop immediately, so it is preferred. When the area ratio of ferrite is greater than 10%, stress is not easily concentrated in the ferrite part, and cracks do not propagate, so it is preferred.

[0050] Here, grain boundary ferrite is a factor that determines the grain boundary strength. If grain boundary ferrite is generated, the toughness of the continuous casting slab is reduced. In addition, ferrite is lower in strength than austenite, pearlite, and bainite, so when stress is applied, there is also a problem that stress is easily concentrated on the grain boundary ferrite. Based on this viewpoint, the inventors of the present invention have repeatedly conducted investigations and found that for the type of microstructure of the continuous casting slab of the present embodiment, even in the structure of the pearlite main body, by suppressing the generation of grain boundary ferrite, the toughness of the continuous casting slab can be greatly improved.

[0051] It should be noted that ferrite contains iron containing up to 0.02% carbon by mass, and is a structure close to pure iron. Ferrite is a ferromagnetic body from room temperature to 780°C, and is the softest and most ductile of steel structures. Pearlite is a structure obtained by slowly cooling austenite. Pearlite is composed of ferrite layers and cementite layers, and is formed by alternating these layers.

[0052] The cooling rate of the ferrite transformation zone has a great influence on the precipitation of grain boundary ferrite. When the cooling rate is slower than the critical rate, ferrite precipitation occurs, so it is necessary to control the cooling rate of 850°C to 700°C. When the cooling rate of the ferrite transformation zone is slower than the critical rate but sufficient precipitation time cannot be ensured, ferrite is preferentially precipitated at the grain boundaries where precipitation is likely to occur. Therefore, the stress during the subsequent pearlite, bainite and martensite transformation is concentrated in the soft ferrite part, causing slab quarter cracking, so it is not suitable. As a countermeasure, by reducing the cooling rate of the ferrite transformation zone and ensuring sufficient precipitation time for ferrite, the ferrite precipitated from the grain boundary can be grown to become polygonal ferrite. In the case of polygonal ferrite, the toughness of the slab can be improved by suppressing excessive stress concentration.

[0053] In addition, in terms of suppressing slab seasonal cracking, it is important not only to suppress the embrittlement of the original austenite grain boundaries, but also to reduce the stress during phase transformation. Therefore, by variously controlling the cooling rate in the pearlite phase transformation region (700°C to 500°C), the microstructure of the continuously cast slab can be controlled.

[0054] It should be noted that the cooling of the continuously cast slab after leaving the continuous casting machine can be controlled by changing the slab temperature at the outlet side of the continuous casting machine, the time until a plurality of slabs are stacked, the number of stacked slabs, the presence or absence of a heat preservation cover, water toughening treatment and other conditions. The cooling rate can be measured using a thermocouple. For example, it can be measured by setting a thermocouple in the center of the upper surface of the wide side (long side) of the slab after the slab comes out of the continuous casting machine.

[0055] As described above, according to the invention of the first embodiment, it is possible to obtain high-strength steel continuously cast slabs with good yield, which do not cause slab seasonal cracking during the cooling process and can prevent hole opening failures during rolling, even in recent years' high-strength steel continuously cast slabs where the toughness of the continuously cast slabs is very low.

[0056] [Second embodiment]

[0057] The continuously cast slab of the second embodiment will be described. The continuously cast slab of the present embodiment is the continuous cast slab of the above embodiment, and contains, by mass%, C: 0.10% to 1.00%, Si: 0.10% to 2.50%, and Mn: 1.50% to 5.00%.

[0058] In the following description, "%" indicating the content of component elements in steel means "mass %" unless otherwise specified.

[0059] <C: 0.10% to 1.00%>

[0060] In the continuous casting slab of the present embodiment, the reason for limiting each chemical component contained in the continuous casting slab is explained. It should be noted that the content of each chemical component contained in the continuous casting slab is mass %. The reason for setting the content of C contained in the continuous casting slab to 0.10% to 1.00% is as follows. The C contained in the continuous casting slab for high-strength steel is an element necessary to improve the strength of the high-strength steel plate using the continuous casting slab as a raw material. If the content of C is less than 0.10%, the required strength of the high-strength steel plate cannot be obtained, so the lower limit of the content of C is 0.10%. On the other hand, if the content of C exceeds 1.00%, the weldability and processability of the above-mentioned high-strength steel plate become insufficient, so it is not preferred.

[0061] Therefore, from such a viewpoint, in the continuously cast slab of the present embodiment, the C content in the continuously cast slab is preferably 0.10% to 1.00%, more preferably 0.12% to 0.40%, and particularly preferably 0.15% to 0.40%.

[0062] <Si: 0.10% to 2.50%>

[0063] Next, the reason for setting the content of Si contained in the continuous casting slab for high-strength steel to 0.10% to 2.50% is as follows. The Si contained in the continuous casting slab is an element necessary to ensure retained austenite in the high-strength steel plate in the annealing process of the continuous casting slab as a raw material. In addition, the Si contained in the continuous casting slab is an additional element necessary to contribute to the high strength of the high-strength steel plate through solid solution strengthening. If the content of Si is less than 0.10%, the strength required for the high-strength steel plate cannot be obtained, so the lower limit of the content of Si is 0.10%.

[0064] On the other hand, if the Si content exceeds 2.50%, the effect of obtaining the strength required for the high-strength steel sheet is saturated, and a strong scale is generated in the hot-rolled sheet before being processed into the high-strength steel sheet. As a result, the appearance and pickling properties of the high-strength steel sheet are deteriorated, so the upper limit of the Si content is 2.50%.

[0065] Therefore, from such a viewpoint, in the continuously cast slab of the present embodiment, the content of Si contained in the continuously cast slab is preferably 0.10% to 2.50%, more preferably 0.50% to 2.00%, and even more preferably 1.00% to 1.80%.

[0066] <Mn: 0.40% to 5.00%>

[0067] Furthermore, the reason for setting the content of Mn contained in the continuous casting slab to 0.40% to 5.00% is as follows. The Mn contained in the continuous casting slab is an element necessary to further improve the strength of the high-strength steel plate. Specifically, Mn is an element added in the hot rolling process of the continuous casting slab in order to control the strength of the high-strength steel plate by controlling its phase change. If the content of Mn is less than 0.40%, the high-strength steel plate cannot be fully strengthened, so the lower limit of the content of Mn is 0.40%. On the other hand, if the content of Mn exceeds 5.00%, the degree of sufficient strengthening of the high-strength steel plate is saturated, and the manufacturing cost of the high-strength steel plate increases, which is not preferred from an economic point of view.

[0068] Therefore, from such a viewpoint, in the continuously cast slab of the present embodiment, the Mn content contained in the continuously cast slab is preferably 0.40% to 5.00%, more preferably 1.20% to 4.50%, and even more preferably 1.40% to 4.00%.

[0069] The continuous casting slab of the present embodiment has the above-mentioned composition, and the remainder is composed of Fe and inevitable impurities, and has an average original austenite grain size and microstructure of appropriate composition. Under this premise, it is also possible to consider other characteristics and contain less than 0.100% of P, less than 0.0200% of S, less than 0.0100% of N, less than 0.100% of Al and less than 0.0100% of O. Here, as inevitable impurities, Zn, Pb and As can be cited. The total of these inevitable impurities is allowed to contain less than 0.100%.

[0070] P segregates at the original austenite grain boundary and makes the grain boundary embrittled, so slab seasonal cracking sometimes occurs. Therefore, the P content is preferably 0.100% or less. It should be noted that the lower limit of the P content is not particularly specified, but since P is a solid solution strengthening element and can improve the strength of the steel plate, it is preferably 0.001% or more. Therefore, the P content is preferably 0.100% or less. Preferably 0.001% or more. More preferably 0.070% or less.

[0071] S is an element that exists in the form of sulfide and causes slab embrittlement. Therefore, the S content is preferably 0.0200% or less. It should be noted that the lower limit of the S content is not particularly specified, but considering the limitations of production technology, it is preferably 0.0001% or more. Therefore, the S content is preferably 0.0200% or less. Preferably, it is 0.0001% or more. More preferably, it is 0.0050% or less.

[0072] Al is an element that affects the fraction of retained austenite in the slab by inhibiting the formation of carbides during slab cooling and promoting the formation of retained austenite. In addition, for deoxidation, it is preferably added at least 0.005%. If the Al content exceeds 0.100%, there is a risk of causing slab embrittlement. Therefore, the Al content is preferably 0.100% or less. More preferably, it is 0.010% or more. More preferably, it is 0.080% or less.

[0073] N is an element that exists in the form of nitride and causes embrittlement of the slab. Therefore, the N content is preferably 0.0100% or less. It should be noted that there is no particular lower limit for the N content, but from the perspective of production technology, the N content is preferably 0.0001% or more. Therefore, the N content is preferably 0.0100% or less. Preferably, it is 0.0001% or more. More preferably, it is 0.0050% or less.

[0074] O is an element that exists in the form of oxides and causes slab embrittlement. Therefore, the content of O is preferably 0.0100% or less. It should be noted that there is no particular lower limit for the content of O, but from the perspective of production technology, the content of O is preferably 0.0001% or more. Therefore, the content of O is preferably 0.0100% or less. Preferably, it is 0.0001% or more. More preferably, it is 0.0050% or less.

[0075] The continuously cast slab of this embodiment is used as a high-strength steel plate, and in addition to the above-mentioned component composition, it can further contain at least one element selected from Ti: less than 0.200%, Nb: less than 0.200%, V: less than 0.200%, Ta: less than 0.10%, W: less than 0.10%, Cr: less than 2.00%, Mo: less than 2.00%, Ni: less than 2.00%, Cu: less than 2.00%, and B: less than 0.0100%, or a combination of two or more elements.

[0076] If the contents of Ti, Nb and V are respectively less than 0.200%, coarse precipitates and inclusions will not be generated in large quantities, and the toughness of the slab will not be reduced. Therefore, the contents of Ti, Nb and V are preferably less than 0.200%. It should be noted that there is no particular lower limit for the contents of Ti, Nb and V, but since the strength of the steel sheet is improved by forming fine carbides, nitrides or carbonitrides during hot rolling of the continuously cast slab or during continuous annealing, the contents of Ti, Nb and V are more preferably more than 0.001%. Therefore, when Ti, Nb and V are contained, their contents are respectively less than 0.200%. More preferably, they are more than 0.001%. More preferably, they are less than 0.100%.

[0077] If the contents of Ta and W are respectively less than 0.10%, coarse precipitates and inclusions will not be generated in large quantities, and the toughness of the slab will not be reduced. Therefore, the contents of Ta and W are preferably respectively less than 0.10%. It should be noted that there is no particular lower limit for the contents of Ta and W, but since the strength of the steel sheet is improved by forming fine carbides, nitrides or carbonitrides during hot rolling of the continuously cast slab or during continuous annealing, the contents of Ta and W are more preferably respectively more than 0.01%. Therefore, when Ta and W are contained, their contents are respectively less than 0.10%. More preferably, they are more than 0.01%. More preferably, they are less than 0.08%.

[0078] The continuous casting slab of the present embodiment may contain at least one selected from Cr, Mo, Ni and Cu as required within the range not impairing the purpose of the present invention. Cr, Mo, Ni and Cu bring about the effect of high strength of the steel plate produced by organizational control in the hot rolling of the continuous casting slab. This effect becomes significant by adding 0.01% or more of Cr, Mo, Ni and Cu, respectively, one or more of them, so it is preferred to add 0.01% or more. If the amount of each element exceeds the upper limit of each element, the weldability, hot workability, etc. of the steel plate deteriorate, so the upper limit of the amount of each element of Cr, Mo, Ni and Cu is 1.00%. Therefore, when the continuous casting slab contains Cr, Mo, Ni and Cu, each content is less than 1.00%. Preferably more than 0.01%. More preferably less than 0.80%.

[0079] B controls the microstructure phase transformation during hot rolling and annealing of the continuous casting slab, and therefore affects the strength through microstructure strengthening, so it can be added. If B is less than 0.0100%, it does not affect the toughness of the slab. Therefore, the content of B is preferably less than 0.0100%. It should be noted that there is no particular lower limit for the content of B, but since it is an element that segregates at the austenite grain boundary during hot rolling and annealing of the continuous casting slab to improve hardenability, the content of B is more preferably more than 0.0003%. Therefore, when B is contained, its content is less than 0.0100%. More preferably, it is more than 0.0003%. More preferably, it is less than 0.0080%.

[0080] If Co is 1.00% or less, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the content of Co is preferably 1.00% or less. It should be noted that there is no particular lower limit for the content of Co, but since it is an element that improves hardenability, the content of Co is more preferably 0.001% or more. Therefore, when Co is contained, its content is 1.00% or less. More preferably, it is 0.001% or more. More preferably, it is 0.80% or less.

[0081] If Cu is 1.00% or less, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the Cu content is preferably 1.00% or less. It should be noted that there is no particular lower limit for the Cu content, but since it is an element that improves hardenability, the Cu content is more preferably 0.01% or more. Therefore, when Cu is contained, its content is 1.00% or less. More preferably, it is 0.01% or more. More preferably, it is 0.80% or less.

[0082] If Sn is 0.200% or less, the toughness of the slab is not affected. Therefore, the content of Sn is preferably 0.200% or less. It should be noted that the lower limit of the content of Sn is not particularly specified, but since Sn is an element that improves hardenability, the content of Sn is more preferably 0.001% or more. Therefore, when Sn is contained, its content is 0.200% or less. More preferably, it is 0.001% or more. More preferably, it is 0.100% or less.

[0083] If Sb is 0.200% or less, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the Sb content is preferably 0.200% or less. It should be noted that the lower limit of the Sb content is not particularly specified, but since it is an element that suppresses decarburization and can adjust the strength of the steel sheet, the Sb content is more preferably 0.001% or more. Therefore, when Sb is contained, its content is 0.200% or less. More preferably, it is 0.001% or more. More preferably, it is 0.100% or less.

[0084] If Ca, Mg and REM are 0.0100% or less, respectively, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the content of each of Ca, Mg and REM is preferably 0.0100% or less. It should be noted that the lower limit of each content of Ca, Mg and REM is not particularly specified, but since they are elements that spheroidize the shape of nitrides and sulfides and improve the toughness of the slab, the content of Ca, Mg and REM is more preferably 0.0005% or more. Therefore, when Ca, Mg and REM are contained, their contents are each 0.0100% or less. More preferably, they are 0.0005% or more. More preferably, they are 0.0050% or less.

[0085] If Zr and Te are respectively less than 0.100%, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the content of each Zr and Te is preferably less than 0.100%. It should be noted that the lower limit of each content of Zr and Te is not particularly specified, but since Zr and Te are elements that spheroidize the shape of nitrides and sulfides and improve the toughness of the slab, the content of Zr and Te is more preferably more than 0.001%. Therefore, when Zr and Te are contained, their contents are respectively less than 0.100%. More preferably, they are more than 0.001%. More preferably, they are less than 0.080%.

[0086] If Hf is 0.10% or less, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the Hf content is preferably 0.10% or less. It should be noted that the lower limit of the Hf content is not particularly specified, but since it is an element that spheroidizes the shape of nitrides and sulfides and improves the ultimate deformation capacity of the steel sheet, the Hf content is more preferably 0.01% or more. Therefore, when Hf is contained, its content is 0.10% or less. More preferably, it is 0.01% or more. More preferably, it is 0.08% or less.

[0087] If Bi is 0.200% or less, coarse precipitates and inclusions do not increase, and the toughness of the slab does not decrease. Therefore, the Bi content is preferably 0.200% or less. It should be noted that the lower limit of the Bi content is not particularly specified, but since it is an element that reduces segregation, the Bi content is more preferably 0.001% or more. Therefore, when Bi is contained, its content is 0.200% or less. More preferably, it is 0.001% or more. More preferably, it is 0.100% or less.

[0088] It should be noted that for the above-mentioned Ti, Nb, V, Ta, W, B, Cr, Mo, Ni, Co, Cu, Sn, Sb, Ca, Mg, REM, Zr, Te, Hf and Bi, the effects of the present invention are not impaired when the content thereof is less than the preferred lower limit value, and therefore they are included as unavoidable impurities.

[0089] As described above, according to the invention of the second embodiment, the strength required for high-strength steel can be obtained, and further, a continuously cast slab excellent in weldability, workability, and appearance of high-strength steel can be obtained.

[0090] [Third Embodiment]

[0091] The method for producing a continuously cast slab according to the third embodiment is described below. The method for producing a continuously cast slab according to the present embodiment is a method for producing a continuously cast slab for high-strength steel in which seasonal cracks of the slab caused by cooling are suppressed, and includes:

[0092] In a first cooling step, the continuously cast slab having the composition of the continuously cast slab described in the above embodiment is cooled under cooling conditions that the cooling temperature of the continuously cast slab at the center in the width direction of the continuously cast slab and 10 mm away from the surface of the continuously cast slab is 1200° C. to 1450° C. and the residence time of the continuously cast slab is 130 seconds or less;

[0093] A second cooling step is performed under cooling conditions in which the surface temperature of the center of the continuous cast slab in the width direction is 700°C to 850°C and the average cooling rate is 20°C / hr or less; and

[0094] The third cooling step is performed under cooling conditions in which the surface temperature of the center of the continuous cast slab in the width direction is 500°C to 700°C and the average cooling rate is 10°C / hr or less.

[0095] Here, the lower limit of the average cooling rate in the second cooling process and the third cooling process is not specifically specified. When a plurality of slabs are stacked and a heat preservation cover is used, the average cooling rates of 700°C to 850°C and 500°C to 700°C are at least 2°C / hr and 1°C / hr, respectively. In the second cooling process and the third cooling process, cooling at an average cooling rate slower than these average cooling rates requires, for example, placing the slab in a heating furnace and heating it, which requires equipment and is therefore not preferred from an economic point of view. Therefore, in the second cooling process, the lower limit of the average cooling rate of 700°C to 850°C is 2°C / hr, and in the third cooling process, the lower limit of the average cooling rate of 500°C to 700°C is 1°C / hr.

[0096] It should be noted that the method for manufacturing a slab for a high-strength steel sheet of the present embodiment may sometimes cause transfer depending on various conditions of the manufacturing process. When transfer occurs, the cooling rate of the slab may temporarily exceed the predetermined cooling rate. However, since the time required for phase transformation is more than 10 hours, which is very slow, if the operation time is the transfer degree (maximum 1 to 2 hours), season cracking will not occur. Therefore, in the present invention, the average cooling rate is specified instead of the maximum cooling rate.

[0097] Hereinafter, each step included in the method for producing a continuously cast slab according to the present embodiment will be described.

[0098] (First Cooling Step)

[0099] The method for manufacturing a continuous cast slab of the present embodiment is a method for manufacturing a continuous cast slab for high-strength steel in which seasonal cracking of the slab caused by cooling is suppressed, comprising a first cooling step, wherein a continuous cast slab having the component composition of the continuous cast slab described in the above embodiment is cooled under cooling conditions in which a cooling temperature of the continuous cast slab at the center in the width direction of the continuous cast slab and 10 mm away from the surface of the continuous cast slab is 1200°C to 1450°C and a residence time of the continuous cast slab is less than 130s.

[0100] The first cooling step is a step for controlling the average prior austenite grain size contained in the continuous casting slab of the above embodiment to be less than 2.0 mm at a predetermined position. By controlling the average prior austenite grain size to be less than 2.0 mm, the density of precipitates precipitated at the prior austenite grain boundaries can be reduced, the precipitation of harmful grain boundary ferrite can be suppressed, and the slab toughness can be improved.

[0101] In the method for manufacturing a continuously cast slab of the present embodiment, the factor determining the average original austenite grain size is the temperature when the slab is cooled. In the first cooling step, the temperature of cooling the continuously cast slab is in the range of 1450°C to 1200°C. Thus, the method for manufacturing a continuously cast slab of the present embodiment focuses on the cooling temperature of the continuously cast slab in the range of 1450°C to 1200°C, which is the factor determining the average original austenite grain size, and controls the temperature.

[0102] Furthermore, in the first cooling step, the residence time of the continuously cast slab within the above temperature range of the continuously cast slab is 130 seconds or less. If the residence time of the continuously cast slab at the above temperature is 130 seconds or less, the average original austenite grain size can be made less than 2.0 mm, and the seasonal cracking of the slab can be suppressed, so it is preferred. It should be noted that there is no particular lower limit for the residence time of the continuously cast slab at 1200°C to 1450°C, but if the residence time is too short, the risk of steel leakage in continuous casting caused by uneven solidification becomes high, so it is preferably 40 seconds or more, more preferably 60 seconds or more, and even more preferably 70 seconds or more.

[0103] (Second Cooling Step)

[0104] Next, the method for manufacturing the continuous casting slab of the present embodiment includes a second cooling step, wherein the continuous casting slab is cooled according to a cooling condition in which the surface temperature at the center in the width direction of the continuous casting slab is 700°C to 850°C and the average cooling rate is 20°C / hr or less. The second cooling step is a step for suppressing the precipitation of grain boundary ferrite contained in the microstructure of the continuous casting slab of the above embodiment and making the area ratio of ferrite less than 5% or more than 10%.

[0105] In the second cooling step, the temperature of the continuously cast slab is further cooled to 700° C. to 850° C. As described above, the method for producing a continuously cast slab according to the present embodiment focuses on the cooling rate in the temperature range of the ferrite transformation region where precipitation of ferrite can be controlled, and controls the temperature.

[0106] In the second cooling step, within the above-mentioned temperature range for cooling the continuously cast slab, the average cooling rate of the continuously cast slab is 20°C / hr or less. When the average cooling rate exceeds 20°C / hr, ferrite is only thinly precipitated at the original austenite grain boundaries, making the grain boundaries embrittled, so it is not suitable. If the average cooling rate of the continuously cast slab is 20°C / hr or less, the residence time of the continuously cast slab in the ferrite transformation temperature range can be fully ensured, the grain boundary ferrite grows into polygonal ferrite, and the stress concentration on the grain boundary ferrite can be suppressed, so it is preferred.

[0107] The lower limit of the average cooling rate is not strictly limited, but is preferably 2°C / hr or more because an energy source is required to control the cooling rate. More preferably, the average cooling rate is 5°C / hr to 18°C / hr.

[0108] (Third Cooling Step)

[0109] Furthermore, the method for producing a continuously cast slab of the present embodiment includes a third cooling step of cooling the continuously cast slab under cooling conditions in which the surface temperature at the center in the width direction of the slab is 500°C to 700°C and the average cooling rate is 10°C / hr or less.

[0110] The third cooling step is a step for making the microstructure of the continuous casting slab of the above embodiment a pearlite-based structure and reducing the internal stress. Specifically, the third cooling step is a step for making the area S of ferrite ferrite and the area of ​​pearlite S pearlite The total area S (ferrite+pearlite) Relative to the area S of the microstructure of the continuous casting slab total A process in which the area ratio (%) of the ratio is 90% or more.

[0111] In the third cooling step, the temperature of the continuously cast slab is further cooled to 500° C. to 700° C. As described above, the method for producing a continuously cast slab according to the present embodiment focuses on the cooling rate in the temperature range in the pearlite transformation region and controls the temperature.

[0112] In the third cooling step, within the above temperature range for cooling the continuously cast slab, the average cooling rate of the continuously cast slab is 10°C / hr or less. If the average cooling rate of the continuously cast slab exceeds 10°C / hr, bainite and martensite precipitate relative to the microstructure of the pearlite main body, thereby generating large stress, which is not suitable. Bainite and martensite have a lower phase transformation temperature than pearlite, and their phase transformation stress is applied to the pearlite part that has completed the phase transformation, which becomes the main cause of promoting cracking.

[0113] From such a viewpoint, if the average cooling rate of the continuously cast slab is 10° C. / hr or less, the internal stress can be reduced by suppressing bainite transformation and obtaining a structure mainly composed of pearlite, which is preferred.

[0114] The lower limit of the average cooling rate is not strictly limited, but is preferably 1° C. / hr or more, and more preferably 5° C. / hr or more, because an energy source required for controlling the cooling rate is separately required.

[0115] In this way, the manufacturing method of the continuous casting slab of this embodiment adopts a three-stage cooling process as the cooling process of the continuous casting slab to accurately control the average original austenite grain size and the microstructure of the continuous casting slab, thereby providing a high-strength steel continuous casting slab in which the seasonal cracking of the slab caused by cooling is suppressed and hole opening failures during rolling can be prevented.

[0116] As described above, according to the manufacturing method of the continuous casting slab of the third embodiment, even if the composition system of the continuous casting slab for high-strength steel is the continuous casting slab, by dividing the cooling process into three stages to accurately control each cooling process, it is possible to provide a continuous casting slab for high-strength steel that does not cause seasonal cracking during the cooling process and can prevent hole opening failures during rolling.

[0117] [Other embodiments]

[0118] The present invention has been described above with reference to the embodiments, but the present invention is not limited to the above embodiments. Various changes that can be understood by those skilled in the art can be made to the composition and details of the present invention within the technical scope of the present invention. In addition, systems or devices obtained by arbitrarily combining the various features included in the various embodiments are also included in the technical scope of the present invention.

[0119] Example

[0120] Hereinafter, the effects of the present invention will be specifically described based on the examples, but the present invention is not limited to these examples. That is, in order to confirm the effects of the present invention, the inventors used various steel types as raw materials in the comparative examples (test No. A-1 to A-4, test No. B-1 to B-8, test No. C-1 to C-3) and the inventive examples (test No. D-1 to D-24) to produce continuous casting slabs. Table 1 shows the steel types A to I used as raw materials for the continuous casting slabs in the comparative examples (test No. A-1 to A-4, test No. B-1 to B-8, test No. C-1 to C-3) and the inventive examples (test No. D-1 to D-24).

[0121] [Table 1]

[0122]

[0123] Among them, the cooling conditions of the continuously cast slab adopt a three-stage cooling process consisting of (I) a residence time [s] of 1200℃~1450℃, (II) an average cooling rate [℃ / hr] of 700℃~850℃ and (III) an average cooling rate [℃ / hr] of 500℃~700℃, and cooling is carried out by appropriately changing the conditions of each stage.

[0124] Tables 2 to 4 show the cooling conditions (I) to (III) of the continuously cast slab, the microstructure of the obtained continuously cast slab, and the evaluation of the slab seasonal crack.

[0125] The measurement of the average prior austenite grain size in the continuously cast slabs produced in the comparative examples and the inventive examples, the calculation of the ferrite and pearlite area ratios, and the evaluation of the season cracking of the continuously cast slabs were performed as follows.

[0126] <Measurement of average prior austenite grain size>

[0127] Here, the method for measuring the average prior austenite grain size is as follows. A sample is cut from the width center of the cooled slab so that the slab thickness section parallel to the slab width direction becomes the observation surface. Next, the observation surface is mirror-polished using diamond paste, and then fine-polished using colloidal silica, and then 3 vo 1.% nitric acid alcohol etching solution was used to etch the surface to reveal the structure. Using an optical microscope, 5 fields of view were observed at a magnification of 10 times at a position 10 mm below the surface of the slab to obtain the microstructure image of the continuously cast slab. The obtained microstructure image was used by the cutting method according to JIS G 0551:2020 to obtain the original austenite grain size obtained by observing the 5 fields of view, and their average value was calculated as the average original austenite grain size.

[0128] <Method for measuring ferrite area ratio>

[0129] The method for determining the ferrite area ratio is the same as the method for determining the average prior austenite grain size described above. The observation surface of the slab is prepared in the same manner. Next, the observation surface is mirror-polished using diamond paste, and then fine-polished using colloidal silica, and then etched using 3 vol.% nitric acid alcohol etching solution to reveal the structure. Under the condition of an accelerating voltage of 15 kV, a SEM (Scanning Electron Microscope) is used to observe 10 fields of view at a magnification of 50 times at a position 10 mm below the surface of the slab. The microstructure image of the continuously cast slab obtained is used with Adobe's PHOTOSHOP (registered trademark) to calculate the area ratio of ferrite in 10 fields of view, and these values ​​are averaged and obtained as the area ratio of ferrite. It should be noted that ferrite has a larger grain size than other structures (pearlite, bainite, tempered martensite, quenched martensite, and retained austenite), and has a smooth surface and dark contrast, so it can be easily distinguished at a magnification of 50 times.

[0130] <Method for measuring the area ratio of pearlite>

[0131] The method for determining the area ratio of the pearlite structure is the same as the method for determining the ferrite described above. The structure is visualized on the observation surface of the slab. Under the condition of an accelerating voltage of 15 kV, the ferrite is removed from the field of view at a position 10 mm below the surface of the slab using a SEM, and 10 fields of view are observed at a magnification of 10,000 times. The microstructure image of the continuously cast slab obtained is used with Adobe's PHOTOSHOP (registered trademark) to calculate the area ratio of pearlite and the area ratio of bainite in 10 fields of view. These values ​​are averaged and calculated in such a way that the sum of the area ratio of ferrite determined by the above method is 100%, and the area ratio of each structure is obtained. Pearlite is a eutectic crystal of ferrite and cementite, and is a structure in which the thin flaky layers of the two have a pearl-like luster when observed using the above scanning electron microscope.

[0132] The microstructure of the continuous casting slab of the present invention is a structure in which pearlite is the main component and there is no grain boundary ferrite. However, it is difficult to strictly classify grain boundary ferrite and polygonal ferrite. Therefore, the present inventors conducted an in-depth investigation on slabs in which slab season cracking occurred, and found that when the area ratio of ferrite is greater than 5% and less than 10%, a large amount of ferrite exists at the grain boundary. That is, it is a structure in which the area ratio of ferrite + pearlite is greater than 90% and the area ratio of ferrite is less than 5% or greater than 10%.

[0133] <Seasonal crack evaluation of slab>

[0134] The evaluation method for slab quarter cracks is based on the penetrant flaw detection test specified in JIS Z 2343: 2017, and the presence or absence of cracks on the wide and narrow surfaces of the slab is evaluated. After applying the developer, the exposure of the penetrant is visually observed to visually inspect the quarter cracks of the slab on the surface.

[0135] It should be noted that when cracks with a length of 50 mm or more exist, there is a high risk of slab breakage in the heating furnace during slab operation. In addition, there is a high possibility of hole opening failure during rolling. Therefore, the evaluation criteria for seasonal cracks in slabs are as follows.

[0136] ·Seasonal cracks of slab 0···No cracks longer than 50 mm on the slab surface ·Seasonal cracks of slab ×···There are cracks longer than 50 mm on the slab surface

[0137]

[0138]

[0139]

[0140] <Comparative Examples (Test Nos. A-1 to A-4)>

[0141] The microstructure of the slabs satisfied by the continuously cast slabs produced in Test No. A-1 to A-4 is set as Condition A. Condition A is a condition for an example in which the average prior austenite grain size at a position 10 mm below the surface of the slab is greater than 2.0 mm. In these cases, since the density of precipitates at the prior austenite grain boundaries increases and the toughness of the prior austenite grain boundaries decreases, even if various changes are made to the conditions for slow cooling of the slab after leaving the slab continuous casting machine, the slab seasonal cracking cannot be suppressed.

[0142] <Comparative Examples (Test Nos. B-1 to B-8)>

[0143] The microstructure of the slabs satisfied by the continuously cast slabs produced in Test No. B-1 to B-8 is set as Condition B. Condition B is a condition in which the average prior austenite grain size at a position 10 mm below the surface of the slab is 2.0 mm or less, but grain boundary ferrite is precipitated at the prior austenite grain boundaries. Under these conditions, the toughness of the prior austenite grain boundaries is reduced due to the grain boundary ferrite, so even if the subsequent cooling rate is changed in various ways to change the composition of the microstructure, the slab quarter cracking cannot be suppressed.

[0144] <Comparative Examples (Test Nos. C-1 to C-3)>

[0145] The microstructure of the slabs satisfied by the continuously cast slabs produced in Test No. C-1 to C-3 is set as Condition C. Condition C is a condition in which the average prior austenite grain size is 2.0 mm or less and the precipitation of grain boundary ferrite is suppressed, but since more than 10% of bainite is precipitated, it is a condition in which cracks in the slab cannot be suppressed. Since the bainite phase transformation occurs at a lower temperature than the pearlite phase transformation, the density difference with austenite is large, and the phase transformation stress also becomes large, so it is considered that cracks in the slab cannot be suppressed.

[0146] <Invention Examples (Test Nos. D-1 to D-24)>

[0147] The microstructure of the slabs satisfied by the continuously cast slabs produced in Test No. D-1 to D-24 is set as Condition D. Condition D is the condition of the present invention example. The continuously cast slabs produced in the present invention example are microstructures with an average prior austenite grain size of 2.0 mm or less and almost no grain boundary ferrite and little bainite. That is, the prior austenite grain boundaries are controlled to be small, and in addition to improving toughness by dispersing precipitates, toughness is improved by suppressing the precipitation of grain boundary ferrite, and internal stress is reduced by suppressing the precipitation of bainite, so that the slab quarter cracking after cooling does not occur.

[0148] According to Tables 2 to 4, it can be seen that the seasonal cracking of the slab during cooling can be suppressed by (i) the average original austenite grain size at a position 10 mm away from the surface of the slab is 0.5 mm to 2.0 mm, (ii) the combined area ratio of ferrite and pearlite in the microstructure of the continuously cast slab is more than 90%, and (iii) the area ratio of the above ferrite is less than 5% or more than 10%.

[0149] That is, the continuous casting slab of the present invention can provide a high-alloy high-strength steel slab without slab cracks after casting, and can also prevent hole opening failures during rolling, etc., because the average original austenite grain size at a position 10 mm from the slab surface is 0.5 mm to 2.0 mm, and the area ratio of ferrite and pearlite in the microstructure is 90% or more, and the area ratio of ferrite is less than 5% or 10% or more. That is, according to the inventive examples and comparative examples, it is found that the average original austenite grain size at a position 10 mm from the slab surface is 0.5 mm to 2.0 mm, and the area ratio of ferrite and pearlite in the microstructure is 90% or more, and (iii) the area ratio of ferrite is less than 5% or 10% or more, so that cracks during cooling of the slab can be suppressed.

[0150] Figure 3 This is an enlarged photograph of a continuously cast slab produced in the invention example (Test No. D-9) observed with an optical microscope. Figure 3 The magnified photograph of the continuous casting slab observed by an optical microscope is shown in FIG. 1 to identify the metal structure contained in the continuous casting slab. The area S of ferrite is ferrite and the area of ​​pearlite S pearlite The total area S (ferrite+pearlite) Relative to the area S of the microstructure of the continuous casting slab total The ratio is calculated as the area ratio (%). The results show that in the continuous casting slab of the present invention, the average original austenite grain size at a position 10 mm from the surface of the slab is 0.5 mm to 2.0 mm, and the total area ratio of ferrite and pearlite in the microstructure is 90% or more. It is further shown that in the continuous casting slab of the present invention, the area ratio of ferrite satisfies less than 5% or is 10% or more.

[0151] In order to obtain such a microstructure of the continuously cast slab, for example, it is preferred to adopt the following three-stage cooling: the temperature of the slab 10 mm below the surface is 1450°C to 1200°C and the residence time is less than 130s, then, the slab is cooled so that the temperature of the central surface of the width is 850°C to 700°C and the cooling rate is less than 20°C / hr, and further, the temperature of the central surface of the width of the slab is 700°C to 500°C and the average cooling rate is less than 10°C / hr.

[0152] It should be noted that if the continuous casting slab is strongly cooled in the temperature range of 1450°C to 1200°C, there is also a risk of cracking the slab surface due to uneven solidification. In this case, for example, after the slab surface is quenched to below the BS point at a temperature of 900°C to 1200°C at the center of the slab width and 10mm below the surface of the slab, the cooling is stopped and heated again to above the AC3 point, thereby the original austenite grain size can be refined by austenite reverse transformation. Then, the cooling rate is 20°C / hr or less when the temperature of the central surface of the slab width is 850°C to 700°C, and then the average cooling rate of the central surface of the slab width is 700°C to 500°C is 10°C / hr or less, thereby obtaining a continuous casting slab having such a microstructure. In addition, the method for manufacturing a continuous casting slab having the microstructure of the above-mentioned continuous casting slab is not limited to this.

[0153] Industrial Applicability

[0154] The continuous casting slab of the present invention has an average original austenite grain size of 0.5mm to 2.0mm at a position 10mm away from the surface of the slab, and the total area ratio of ferrite and pearlite in the microstructure is more than 90%, and the area ratio of ferrite is less than 5% or more than 10%. Therefore, it is possible to provide a high-strength steel slab without slab cracks after casting, and can also prevent hole opening failures during rolling, etc., so it is useful in industry.

Claims

1. A continuous casting slab, which is a continuous casting slab for high-strength steel, characterized in that: The average original austenite grain size at a position 10 mm from the surface of the continuous casting slab is 0.5 mm to 2.0 mm. Furthermore, in the microstructure, the total of the area ratio of ferrite and the area ratio of pearlite is 90% or more, and the area ratio of ferrite is less than 5% or 10% or more.

2. The continuous casting slab according to claim 1, characterized in that: The continuously cast slab contains, by mass %, C:0.10%~1.00%、 Si: 0.10% to 2.50%, Mn: 0.40%~5.00%.

3. A method for producing a continuously cast slab, which is a method for producing a continuously cast slab for high-strength steel in which seasonal cracks of the slab caused by cooling are suppressed, characterized in that: include: In a first cooling step, the continuously cast slab having the composition of claim 2 is cooled under cooling conditions that the cooling temperature of the continuously cast slab at the center in the width direction of the continuously cast slab and 10 mm from the surface of the continuously cast slab is 1200° C. to 1450° C. and the residence time of the continuously cast slab is 130 seconds or less; The second cooling step is to cool the continuously cast slab under cooling conditions in which the surface temperature at the center of the width direction of the slab is 700°C to 850°C and the average cooling rate is 20°C / hr or less; as well as The third cooling step is performed under cooling conditions in which the surface temperature of the center in the width direction of the continuous cast slab is 500° C. to 700° C. and the average cooling rate is 10° C. / hr or less.