Photovoltaic device and method of manufacture
By introducing an improved carrier extraction layer into thin-film cadmium telluride solar cells, and optimizing the band alignment of the absorber and the p-type contact layer using thiol-based molecular materials, the problem of ohmic contact difficulties in the prior art is solved. Improves the efficiency and stability of photovoltaic devices.
Patent Information
- Application Number
- CN202380036803.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-28
- Publication Date
- 2024-12-06
AI Technical Summary
In thin-film cadmium telluride solar cells, the lack of high work function materials with good band alignment makes it difficult to form ohmic contact with p-type CdTe and other II-VI semiconductor alloys, thereby affecting the efficiency of photovoltaic devices.
Using an improved carrier extraction (ICE) layer, thiol-based molecular materials such as 2-aminoethyl thiol (AET) and 4-fluorophenylthiophenyl (4-FTP) form the ICE layer to optimize interface complexation and carrier transport.
It realizes efficient hole conduction and electron reflection, reduces interface recombination, improves the current collection efficiency and open circuit voltage of photovoltaic devices, and enhances the stability and photoluminescence intensity of the device.
Smart Images

Figure CN119096372A_ABST
Abstract
Description
Technical Field
[0001] The present description relates generally to layers for photovoltaic devices and, more particularly, to using specific combinations of materials and layer formation parameters to improve the efficiency of photovoltaic devices. Background Art
[0002] Photovoltaic devices generate electricity by converting light into electricity using semiconductor materials that exhibit the photovoltaic effect. P-type contacts with low contact resistivity and low recombination losses have been a persistent challenge in the development of thin-film cadmium telluride-based solar cells. The lack of high work function materials with good band alignment makes it difficult to form ohmic contacts with p-type CdTe and other II-VI semiconductor alloys. It is desirable to use material layers to improve the efficiency of photovoltaic devices.
[0003] Therefore, there is a need for alternative layer structures and compositions for use in photovoltaic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] The embodiments illustrated in the drawings are schematic and exemplary in nature and are not intended to limit the subject matter defined by the claims. The following detailed description of the exemplary embodiments can be understood when read in conjunction with the following drawings, in which like reference numerals designate like or corresponding parts throughout the views.
[0005] Figure 1 A photovoltaic device according to one or more embodiments shown and described herein is schematically depicted.
[0006] Figure 2 Schematically depicts a schematic diagram of a system according to one or more embodiments shown and described herein. Figure 1 Cross-sectional view of a portion of a photovoltaic device.
[0007] Figure 3A-3B Schematically depicted is a cross-sectional view of a portion of a photovoltaic device according to embodiments shown and described herein.
[0008] Figure 4 Schematically depicted is a cross-sectional view of the formation of a self-assembled monolayer according to one or more embodiments shown and described herein.
[0009] Figure 5A-5B Shown is a shift in the valence band offset of a device according to the embodiments shown and described herein.
[0010] Figure 6A-6B Shown is an energy band diagram of a device according to embodiments shown and described herein.
[0011] Figure 7A-7B Shown is an energy band diagram of a device according to embodiments shown and described herein.
[0012] Figures 8A-8B Shown is a comparison of performance characteristics of photoluminescence intensity versus peak wavelength for a control device and devices according to embodiments shown and described herein.
[0013] Fig. 9 Shown is a comparison of performance characteristics of devices according to embodiments shown and described herein.
[0014] Figures 10A-10E Comparative performance characteristics of a control device and devices according to embodiments shown and described herein are shown. DETAILED DESCRIPTION
[0015] Photovoltaic devices can be formed by stacks of functional layers formed on a substrate. One or more functional layers can include a thin film of material, i.e., the photovoltaic device can be a thin film photovoltaic device. A thin film photovoltaic device can include an absorber layer for converting light into charge carriers and a conductive layer for collecting the charge carriers. When charge carriers are generated, an electric potential is generated by the separation of the charges. Positive and negative charge carriers, holes and electrons move in opposite directions toward the p-type region and the n-type region on the opposite side of the absorber, respectively.
[0016] In the development of thin film cadmium telluride based solar cells, producing p-type contacts with low contact resistivity and low recombination losses has been an ongoing challenge. The lack of high work function materials with good band alignment makes it difficult to form ohmic contacts with p-type CdTe, its alloys and other II-VI semiconductor alloys. Interface engineering using the described materials and methods provides an improved carrier extraction (ICE) layer between the absorber and the p-type contact layer to produce a structure with high hole conductivity, low electron affinity, chemical passivation and controlled band alignment. Therefore, when p-type majority carriers (holes) reach the contact interface, the ICE layer efficiently transports holes from the absorber to the p-type contact layer and minimizes interfacial recombination.
[0017] The ICE layer is combined with a p-type contact layer to provide a good back contact for a solar cell having an absorber containing a II-VI type semiconductor alloy, including alloys of cadmium and tellurium, including binary, ternary and quaternary alloys. The ICE layer remains chemically passivated at the surface of the absorber layer and provides control over the alignment of the work function band. The p-type contact layer has a low hole transport barrier and a high electron barrier for electron reflection. Ideally, the p-type contact layer has minimal interface defects, good passivation and high conductivity. The p-type contact layer may have a high doping to obtain a deep Fermi level and a high hole mobility. In some cases, the ICE layer and the p-type contact layer may be formed relative to the absorber layer toward the back side of the module. In some cases, the ICE layer and the p-type contact layer may be formulated to be substantially transparent. The embodiments provided herein relate to a p-type contact layer and a photovoltaic device including the same. The disclosed layer can improve the efficiency of the current collecting portion of the photovoltaic device.
[0018] Reference now Figure 1 , which schematically depicts one embodiment of a photovoltaic device 100. The photovoltaic device 100 can be configured to receive light and convert the light into electrical energy, for example, photons can be absorbed from the light and converted into electric current via the photovoltaic effect. Therefore, for the sake of discussion and clarity, the photovoltaic device 100 can define a front side 102 that is configured to face a primary light source (e.g., the sun). In addition, the photovoltaic device 100 can also define a back side 104 that is offset from the front side 102, for example, by multiple material functional layers. It should be noted that the term "light" can refer to various wavelengths of the electromagnetic spectrum, such as, but not limited to, wavelengths in the ultraviolet (UV), infrared (IR), and visible portions of the electromagnetic spectrum. As used herein, "sunlight" refers to light emitted by the sun.
[0019] Photovoltaic device 100 may include multiple layers disposed between front side 102 and back side 104. As used herein, the term "layer" refers to a material of a certain thickness disposed on a surface. Each layer may cover all or part of an adjacent surface. In some embodiments, the layers of photovoltaic device 100 may be divided into arrays of photovoltaic cells 200. For example, photovoltaic device 100 may be scribed according to multiple serial scribe lines 202 and multiple parallel scribe lines 204. Serial scribe lines 202 may extend along the length Y of photovoltaic device 100 and define the boundaries of photovoltaic cell 200 along the length Y of photovoltaic device 100. Adjacent cells of photovoltaic cell 200 may be connected in series along the width X of photovoltaic device 100. In other words, monolithic interconnections of adjacent cells 200 may be formed, i.e., adjacent to serial scribe lines 202. Parallel scribe lines 204 may extend along the width X of photovoltaic device 100 and define the boundaries of photovoltaic cell 200 along the width X of photovoltaic device 100. In operation, current 205 can flow primarily along width X through photovoltaic cells 200 connected in series by serial scribe lines 202. In operation, parallel scribe lines 204 can limit the ability of current 205 to flow along length Y. Parallel scribe lines 204 are optional and can be configured to separate serially connected photovoltaic cells 200 into groups 206 arranged along length Y.
[0020] Still reference Figure 1 , parallel scribe lines 204 can electrically isolate groups 206 of series-connected photovoltaic cells 200. In some embodiments, groups 206 of photovoltaic cells 200 can be connected in parallel, for example, via an electrical bus. Optionally, the number of parallel scribe lines 204 can be configured to limit the maximum current generated by each group 206 of photovoltaic cells 200. In some embodiments, the maximum current generated by each group 206 can be less than or equal to about 200 milliamperes (mA), for example, less than or equal to about 100 mA in one embodiment, less than or equal to about 75 mA in another embodiment, or less than or equal to about 50 mA in yet another embodiment.
[0021] Reference now Figure 2 , the layers of the photovoltaic device 100 may include a thin film stack disposed on a substrate 110. The substrate 110 may be configured to facilitate transmission of light into the photovoltaic device 100. The substrate 110 may be disposed at a front side 102 of the photovoltaic device 100. The substrate 110 may have a first surface 112 that generally faces the front side 102 of the photovoltaic device 100 and a second surface 114 that generally faces the back side 104 of the photovoltaic device 100. One or more layers may be disposed between the first surface 112 and the second surface 114 of the substrate 110.
[0022] The substrate 110 may include a transparent layer. The transparent layer may be a substantially transparent material (e.g., glass). Suitable glass may include soda-lime glass or glass with a reduced iron content. The transparent layer may have a transmittance range, for example, including visible light and near-ultraviolet and / or infrared ranges. In some embodiments, the transmittance range may include a wavelength of 250nm to 1,300nm or a subset within the range. The transparent layer may also be characterized by a transmittance percentage, including, for example, greater than about 50% in one embodiment, greater than about 60% in another embodiment, greater than about 70% in yet another embodiment, greater than about 80% in yet another embodiment, or greater than about 85% in yet another embodiment. In one embodiment, the transparent layer may include glass with a transmittance of about 90% or more. Optionally, the substrate 110 may include a coating at the first surface 112. The coating may be configured to interact with light or improve the durability of the substrate 110, such as, but not limited to, an anti-reflective coating, an anti-fouling coating, or a combination thereof.
[0023] Reference again Figure 2 , the photovoltaic device 100 may include a barrier layer 130 configured to mitigate diffusion of contaminants (e.g., sodium) from the substrate 110, which may cause degradation or delamination of other layers of the photovoltaic stack. The barrier layer 130 may have a first surface 132 that generally faces the front side 102 of the photovoltaic device 100 and a second surface 134 that generally faces the back side 104 of the photovoltaic device 100. In some embodiments, the barrier layer 130 may be disposed adjacent to the substrate 110. For example, the first surface 132 of the barrier layer 130 may be disposed above the second surface 114 of the substrate 100. As used herein, the expression "adjacent to" means that two layers are disposed adjacently and there is no intervening material between at least a portion of the layers.
[0024] Typically, barrier layer 130 can be substantially transparent, thermally stable, have a reduced number of pinholes, and have high sodium blocking capabilities and good adhesion properties. Alternatively or in addition, barrier layer 130 can be configured to apply color suppression to light. Barrier layer 130 can include one or more material layers, including but not limited to tin oxide, silicon dioxide, aluminum-doped silicon oxide, silicon oxide, silicon nitride, or aluminum oxide. Barrier layer 130 can have a thickness defined by first surface 132 and second surface 134, including, for example, greater than 10.0 nm in one embodiment, greater than about 15.0 nm in one embodiment, less than about 80.0 nm or less than about 20.0 nm in another embodiment.
[0025] Still reference Figure 2, the photovoltaic device 100 may include an n-type contact layer 140 configured to provide an electrical contact to transfer charge carriers generated by the photovoltaic device 100. The n-type contact layer may be a transparent conductive oxide (TCO) layer 140. The n-type contact layer 140 may have a first surface 142 that generally faces the front side 102 of the photovoltaic device 100 and a second surface 144 that generally faces the back side 104 of the photovoltaic device 100. In some embodiments, the n-type contact layer 140 may be disposed adjacent to the barrier layer 130. For example, the first surface 142 of the n-type contact layer 140 may be disposed above the second surface 134 of the barrier layer 130. Generally, the n-type contact layer 140 may include one or more layers of an n-type semiconductor material that is generally transparent and has a wide bandgap. Specifically, the wide bandgap may have a larger energy value compared to the photon energy of the light, which may mitigate undesirable light absorption. The n-type contact layer 140 may include one or more material layers, including but not limited to tin dioxide, doped tin dioxide (e.g., F-SnO2), indium tin oxide, or cadmium tin oxide, including cadmium stannate (Cd2SnO4). In embodiments where the n-type contact layer 140 includes cadmium stannate, the cadmium stannate may be provided in a crystalline form. For example, the cadmium stannate may be deposited as a film and then subjected to an annealing process, which converts the thin film into a crystalline film.
[0026] The photovoltaic device 100 may include a buffer layer 150 configured to provide an insulating layer between the n-type contact layer 140 and the semiconductor layer. The buffer layer 150 may have a first surface 152 that generally faces the front side 102 of the photovoltaic device 100 and a second surface 154 that generally faces the back side 104 of the photovoltaic device 100. In some embodiments, the buffer layer 150 may be disposed adjacent to the n-type contact layer 140. For example, the first surface 152 of the buffer layer 150 may be disposed above the second surface 144 of the n-type contact layer 140. The buffer layer 150 may include a material having a higher resistivity than the n-type contact layer 140, including but not limited to intrinsic tin dioxide, zinc magnesium oxide (e.g., ZnO), and the like. 1-x Mg x 0), silicon dioxide (SiO2), aluminum oxide (Al2O3), aluminum nitride (AlN), zinc tin oxide, zinc oxide, tin silicon oxide, or any combination thereof. In some embodiments, the material of the buffer layer 150 can be configured to substantially match the band gap of an adjacent semiconductor layer (e.g., an absorber). The buffer layer 150 can have a thickness between the first surface 152 and the second surface 154, including, for example, greater than about 10.0 nm in one embodiment, between 10.0 nm and 120.0 nm in one embodiment, between 10.0 nm and 80.0 nm, or between 15.0 nm and 60.0 nm in another embodiment.
[0027] Still reference Figure 2 , the photovoltaic device 100 may include an absorber layer 160 configured to cooperate with another layer and form a pn junction within the photovoltaic device 100. Accordingly, absorbed photons of light may release electron-hole pairs and generate a carrier flow, thereby generating electrical energy.
[0028] The partially formed device, including the substrate 110 , the n-type layer including the TCO layer 140 and / or the buffer layer 150 , and the layers therebetween, may be referred to as a substrate stack 113 . An absorber layer 160 may be formed over the substrate stack 113 .
[0029] The absorber layer 160 may have a first surface 162 that generally faces the front side 102 of the photovoltaic device 100 and a second surface 164 that generally faces the back side 104 of the photovoltaic device 100. The thickness of the absorber layer 160 may be defined between the first surface 162 and the second surface 164. The thickness of the absorber layer 160 may be between about 500 nm and about 10,000 nm, for example, between about 1,000 nm and about 7,000 nm in one embodiment, or between about 1,500 nm and about 4,000 nm in another embodiment.
[0030] Absorber layer 160 may include a p-type semiconductor material having an excess of positive charge carriers (i.e., holes or acceptors). Absorber layer 160 may include a p-type semiconductor material such as a II-VI semiconductor, for example, cadmium and tellurium. Further examples include, but are not limited to, semiconductor materials comprising cadmium, zinc, tellurium, selenium, or any combination thereof. In some embodiments, absorber layer 160 may include a ternary compound of cadmium, selenium, and tellurium (e.g., CdSe x Te 1-x ), or a compound containing cadmium, selenium, tellurium and one or more additional elements (e.g., Cd y Zn 1-y Se x Te 1-x ). The absorber layer 160 may also include one or more dopants. The photovoltaic device 100 provided herein may include a variety of absorber materials.
[0031] Alternatively, in some embodiments, the absorber layer 160 can include an n-type semiconductor material having an excess of negative charge carriers (i.e., electrons or donors). The absorber layer 160 can include n-type semiconductor materials, including II-VI semiconductors, such as cadmium and selenium. In some embodiments, the absorber layer 160 is an n-type cadmium selenide; in some embodiments, the absorber layer can include a ternary compound of cadmium, selenium, and tellurium, such as CdSe. x Te 1-x , wherein x is greater than 0.5; or a compound comprising cadmium, selenium, tellurium and one or more additional elements.
[0032] In embodiments where the absorber layer 160 is p-type and comprises tellurium and cadmium, the average atomic percentage of tellurium in the absorber layer 160 can be greater than or equal to about 25 atomic percent and less than or equal to about 50 atomic percent, for example, greater than about 30 atomic percent and less than about 50 atomic percent in one embodiment, greater than about 40 atomic percent and less than about 50 atomic percent in another embodiment, or greater than about 47 atomic percent and less than about 50 atomic percent in yet another embodiment. Alternatively or in addition, the average atomic percentage of tellurium in the absorber layer 160 can be greater than about 45 atomic percent, for example, greater than about 49% in one embodiment. It should be noted that the average atomic percentages described herein represent the entire absorber layer 160, and the atomic percentage of material at a particular location within the absorber layer 160 can be gradient across the thickness compared to the overall composition of the absorber layer 160. For example, the absorber layer 160 can have a gradient composition.
[0033] In embodiments where absorber layer 160 is p-type and comprises selenium and tellurium, the average atomic percentage of selenium in absorber layer 160 may be greater than 0 atomic percentage and less than or equal to about 25 atomic percentage, for example, greater than about 1 atomic percentage and less than about 20 atomic percentage in one embodiment, greater than about 1 atomic percentage and less than about 15 atomic percentage in another embodiment, or greater than about 1 atomic percentage and less than about 8 atomic percentage in yet another embodiment. It should be noted that the concentration of tellurium, selenium, or both may be gradient throughout the thickness of absorber layer 160. For example, when absorber layer 160 comprises a compound (Se) comprising selenium at a mole fraction x and tellurium at a mole fraction 1-x, the average atomic percentage of selenium in absorber layer 160 may be greater than 0 atomic percentage and less than about 25 atomic percentage, for example, greater than about 1 atomic percentage and less than about 20 atomic percentage in one embodiment, greater than about 1 atomic percentage and less than about 15 atomic percentage in another embodiment, or greater than about 1 atomic percentage and less than about 8 atomic percentage in yet another embodiment. x Te 1-x ), x in the absorption layer 160 may vary with the distance from the first surface 162 of the absorption layer 160. x Te 1-x In an example absorber layer, the molar fraction of selenium can be such that x is greater than 0 and less than 0.40; in some embodiments, x is less than 0.30. In some embodiments, the absorber layer comprises CdSe x Te 1-x And the average value of x in the absorbing layer is less than 0.16.
[0034] Still reference Figure 2 , the absorption layer 160 can be doped with a dopant configured to manipulate the charge carrier concentration. In some embodiments, the absorption layer 160 can be p-type doped with a group V dopant such as arsenic, phosphorus, antimony, or a combination thereof. Alternatively or in addition, the absorption layer 160 can be doped with a group IB dopant such as copper, silver, gold, or a combination thereof. The total density of the dopant within the absorption layer 160 can be controlled. In addition, the amount of the dopant can vary with the distance from the first surface 162 of the absorption layer 160.
[0035] A pn junction may be formed by an absorber layer and a layer of opposite charge type. In a device having a p-type absorber layer, a pn junction may be formed by disposing the absorber layer 160 sufficiently close to a portion of the photovoltaic device 100 having an excess of negative charge carriers (i.e., electrons or donors). For example, a p-type absorber layer may be disposed on an n-type TCO layer 140, optionally with an intervening buffer layer 150. In some embodiments, the absorber layer 160 may be disposed adjacent to an n-type semiconductor material. Alternatively, one or more intervening layers may be disposed between the absorber layer 160 and the n-type semiconductor material. In some embodiments, the absorber layer 160 may be disposed adjacent to the buffer layer 150. For example, a first surface 162 of the absorber layer 160 may be disposed above a second surface 154 of the buffer layer 150. In some embodiments, the absorber layer 160 may be disposed adjacent to an n-type contact layer 140. For example, a first surface 162 of the absorber layer 160 may be disposed above a second surface 144 of the n-type contact layer 140.
[0036] like Figure 3A-3B As shown in , the photovoltaic device 100 may include an improved carrier extraction (ICE) layer 170 between the absorber layer 160 and the conductive layer 190. Figure 3A In the configuration shown in FIG. 1 , an improved carrier extraction (ICE) layer 170 can be located between the absorber layer 160 and the p-type contact layer 180. The ICE layer 170 can have a first surface 172 that generally faces the front side 102 of the photovoltaic device 100 and a second surface 174 that generally faces the back side 104 of the photovoltaic device 100. The ICE layer 170 can be disposed between the p-type contact layer 180 and the absorber layer 160. In some embodiments, the ICE layer 170 can be disposed directly adjacent to one or both of the p-type contact layer 180 and the absorber layer 160. For example, as Figure 2 and Figure 3A As illustrated in FIG. 1 , the first surface 172 of the ICE layer 170 may be disposed above the second surface 164 of the absorber layer 160 , and the second surface 174 of the ICE layer 170 may be adjacent to the first surface 182 of the p-type contact layer 180 .
[0037] like Figure 3B As shown in , in an alternative configuration, the device may include a first p-type contact layer 180 a between the absorber layer 160 and the ICE layer 170 ; alternatively or additionally, the device may include a second p-type contact layer 180 b between the ICE layer 170 and the conductive layer 190 .
[0038] The thickness of the ICE layer 170 can be defined between the first surface 172 and the second surface 174. The thickness of the ICE layer 170 can be greater than about 0.2nm, for example, equal to or greater than 0.25nm, equal to or greater than 0.3nm, equal to or greater than 0.4nm, equal to or greater than 0.5nm, equal to or greater than 0.8nm, equal to or greater than 1.0nm, equal to or greater than 2.0nm, or equal to or greater than 4.0nm. The thickness of the ICE layer can be less than about 30nm, for example, equal to or less than 25.0nm, equal to or less than 20.0nm, equal to or less than 15.0nm, equal to or less than 10.0nm, equal to or less than 5.0nm, or equal to or less than 4.0nm. In one example, the thickness of the ICE layer is between 0.3nm and 6.0nm. In another example, the thickness of the ICE layer is between about 0.4nm and about 25nm in one embodiment, or between about 0.5nm and about 15nm. In some embodiments, the thickness of ICE layer 170 can be between about 0.2 nm and about 20 nm, for example, between about 0.2 nm and about 5.0 nm in one embodiment.
[0039] The ICE layer 170 may be formed of one or more molecules of an organic sulfur compound. The ICE layer includes thiol-based molecules or thiol derivatives, such as thiol alkanes or thiophenes. The thiol-based molecules may include, for example, one or more of the following: cysteamine, also known as 2-aminoethanethiol (AET); 4-fluorothiophenol (4-FTP); 4-aminothiophenol (4-ATP); 1,2-ethanedithiol, also known as ethylenethiol (EDT); L-cysteine, also known as (R)-2-amino-3-mercaptopropionic acid (L-Cys); thioglycolic acid, also known as thioglycolic acid (TGA); 1-octanethiol (OT); 4-fluorobenzylthiol, also known as (4-fluorophenyl) methylthiol (4-FMB); 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluoro-1-octanethiol (TDF-OT); or 4-trifluoromethylbenzylthiol (4-TFMBM). The ICE layer may be composed of thiol-based molecules that constitute the reaction product or tautomeric form of one or more other molecules, including, for example, isothioureas from the tautomerization of thiourea. The ICE layer may be composed of thiol-based molecules that are produced from salt forms, including, for example, sodium thiophenolate or sodium thioglycolate.
[0040] The photovoltaic device 100 may include a p-type contact layer 180 configured to provide electrical contact with the absorber layer 160. The p-type contact layer 180 may have a first surface 182 that generally faces the energy side 102 of the photovoltaic device 100 and a second surface 184 that generally faces the opposite side 104 of the photovoltaic device 100. The p-type contact layer 180 may be a back contact layer having a first surface 182 that generally faces the absorber layer 160. The thickness of the p-type contact layer 180 may be defined between the first surface 182 and the second surface 184. The thickness of the p-type contact layer 180 may be less than about 500 nm, for example, between about 0.5 nm and about 100 nm in one embodiment, or between about 5 nm and about 50 nm in another embodiment. In some embodiments, the thickness of the p-type contact layer 180 may be between about 5 nm and about 200 nm, for example, between about 10 nm and about 50 nm in one embodiment.
[0041] In some embodiments, the p-type contact layer 180, 180a, 180b is one or more layers comprising polymers, small molecules, or inorganic compounds. These materials can be doped to change their electrical and optical properties.
[0042] In some embodiments, the p-type contact layer comprises an inorganic compound comprising one or more of a metal, an oxide, or a nitride. In some embodiments, the p-type contact layer comprises an inorganic compound selected from the group consisting of nickel oxide (NiOx), cuprous thiocyanate (CuSCN), copper iodide (CuI), or copper oxide (Cu2O).
[0043] In some embodiments, the p-type contact layer comprises a polymer material selected from the group consisting of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly(9,9-dioctylfluorene-alt-N-(4-sec-butylphenyl)-diphenylamine) (TFB), poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(2,4-dimethylphenyl))diphenylamine)] (PF8-TAA), poly[[(2,4-dimethylphenyl) imino]-1,4-phenylene(6,12-dihydro-6,6,12,12-tetraoctylindeno[1,2-b]fluorene-2,8-diyl)-1,4-phenylene] (PIF8-TAA), poly(3-hexylthiophene-2,5-diyl) (P3HT), poly(N,N'-bis-4-butylphenyl-N,N'-biphenyl)benzidine (polyTPD), polythiophene or poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonate) (PEDOT:PSS).
[0044] In some embodiments, the p-type contact layer comprises a small molecule selected from the group consisting of: N2,N2,N2',N2',N7,N7,N7',N7'-octa(4-methoxyphenyl)-9,9'-spiro[9H-fluorene]-2,2',7,7'-tetramine (Spiro-OMeTAD), N2,N2,N2',N2',N7,N7,N7',N7'-octa(4-methoxyphenyl)-10-phenyl-10H-spiro[acridine-9,9'-fluorene]-2,2',7,7 '-tetramine (SAF-OMe), N,N'-dialkyl perylene diimide (PDI), 4,4'-bis(N-carbazolyl)-1,1'-biphenyl (CBP), tris(4-carbazolyl-9-ylphenyl)amine (TCTA), 1,3,5-tris(carbazol-9-yl)benzene (TCP), tris{N,N-bis(4-methoxyphenyl)-N-phenyl}aminequinolizineacridine (OMeTPA-FA), SGT-407, Fused-F or tetrathiafulvalene (TTF-1). In some embodiments, the p-type contact layer includes a material selected from the group consisting of α-NPD, 6,13-bis(triisopropylsilylethynyl)pentacene (TIPS-pentacene), poly[2,6-(4,4-bis-(2-ethylhexyl)-4H-cyclopenta[2,1-b;3,4-b']dithiophene)-alt-4,7(2,1,3-benzothiadiazole)] (PCPDTBT), poly[N-9'-heptadecanyl-2,7-carbazole-alt-5,5-(4',7'-di-2-thienyl-2',1',3'-benzothiadiazole)] (PCDTBT), graphene oxide, and quinolizineacridine.
[0045] The composition of the p-type contact layer can be doped. For example, the p-type dopant of the small molecule composition can include, but is not limited to, 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanoquinodimethane (F4-TCNQ), transition metal oxides such as molybdenum trioxide (MoO3), vanadium pentoxide (V2O5) or tungsten trioxide (WO3), and tris[1,2-bis(trifluoromethyl-)ethane-1,2-dithiolene]molybdenum (Mo(tfd)3).
[0046] The thin film junction 176 can be defined as the thin film stack that primarily contributes to the photovoltaic effect. For example, in some embodiments, Figure 2 As illustrated therein, the thin film junction 176 may include an n-type contact layer 140 , a buffer layer 150 , an absorber layer 160 , an improved carrier extraction (ICE) layer 170 , and a p-type contact layer 180 . Figure 3A-3B A thin film junction 176 is shown, which includes a layer between and including the n-type contact layer 140 and the p-type contact layer 180 .
[0047] The photovoltaic device 100 may include a conductive or electrically conductive layer 190 configured to provide electrical contact with the absorber layer 160. The conductive layer 190 may have a first surface 192 that generally faces the energy side 102 of the photovoltaic device 100 and a second surface 194 that generally faces the opposite side 104 of the photovoltaic device 100. In some embodiments, the conductive layer 190 may be disposed adjacent to the p-type contact layer 180. For example, the first surface 192 of the conductive layer 190 may be disposed above the second surface 184 of the p-type contact layer 180. The conductive layer 190 may include an electrically conductive material, such as one or more layers of metals, oxides, oxynitrides, nitrides, nitrogen-containing metals, silver, nickel, copper, aluminum, titanium, palladium, chromium, molybdenum, gold, etc. Examples of nitrogen-containing metal layers may include nitrogen-doped zinc telluride, nitrogen-doped cadmium zinc telluride, nitrogen-doped zinc oxide, molybdenum nitride, molybdenum oxynitride, aluminum nitride, nickel nitride, titanium nitride, tungsten nitride, selenium nitride, tantalum nitride, or vanadium nitride. The conductive material may include one or more metallic elements. The conductive material may include metal alloys, nitrides, oxides and / or oxynitrides. The conductive material may have sub-layers of different compositions.
[0048] The photovoltaic device 100 may include a back support 196 configured to cooperate with the substrate 110 to form an enclosure of the photovoltaic device 100. The back support 196 may be disposed at the opposite side 102 of the photovoltaic device 100. For example, the back support 196 may be formed adjacent to the conductive layer 190. The back support 196 may include, for example, glass, a polymer sheet, borosilicate glass, float glass, soda-lime glass, carbon fiber, or polycarbonate.
[0049] Common Reference Figure 1 -3, the substrate stack 113 of the photovoltaic device 100 is positioned toward the front side 102 facing the light and opposite to the back side 104. The layers constituting the substrate stack 113 are substantially transparent. An absorber layer is disposed on the substrate stack 113 to form an absorber stack 115.
[0050] In some embodiments, a partially formed device including layer stack 115 can be subjected to one or more surface treatments to modify a surface region 364 of absorber layer 160 at a back interface. Surface region 364 of the absorber layer may include a portion of absorber layer 160 at second surface 164 and extending into the thickness of absorber layer 160. In one embodiment, surface region 364 includes the top surface of absorber stack 115 extending into absorber layer 160 to a depth in a range of about 10 nm, about 5 nm, or 0.2 nm to 15 nm. In one embodiment, surface region 364 is passivated by the treatments. In one embodiment, surface region 364 is a Cd-rich layer. In one embodiment, surface region 364 includes cadmium and tellurium and the ratio of Cd to Te in surface region 364 is in a range of 1:1 to 4:1.
[0051] In some embodiments, a partially formed device including the layer stack 115 can be subjected to one or more surface treatments to modify a surface region 384 of the first p-type contact layer 180a at the back interface. The surface region 384 of the first p-type contact layer can include a portion of the first p-type contact layer 180a at the second surface 184 and extending into the thickness of the p-type contact layer 180a. In one embodiment, the surface region 384 includes the top surface of the absorber stack 115 extending into the first p-type contact layer 180a to a depth in the range of 0.01% to 10.0% of the thickness of the first p-type contact layer 180a. In one embodiment, the surface region 384 is passivated by the treatments.
[0052] Photovoltaic device 100 may include multiple layers, and when layers are not designated as contiguous, the photovoltaic device may include intervening layers that are not depicted. A layer may include one or more material functional layers and a single layer may have a composition gradient therein. A deployment-ready device may also include electrical connections, packaging, and other features.
[0053] Photovoltaic devices may contain several material layers deposited sequentially on a substrate. The steps of manufacturing photovoltaic devices may include sequentially arranging functional layers or layer precursors in a "stack" of layers by one or more deposition processes, including but not limited to spin coating, spray coating, slit coating, blade coating, dip coating, sputtering, evaporation, molecular beam deposition, pyrolysis, closed space sublimation (CSS), pulsed laser deposition (PLD), chemical vapor deposition (CVD), electrochemical deposition (ECD), atomic layer deposition (ALD) or vapor transport deposition (VTD). One or more methods may be used to treat or process the deposited layer or layer stack to change the properties, such as by annealing, passivation, heating, vapor contact or chemical treatment. The manufacture of photovoltaic devices may also include selectively removing portions of certain layers of the layer stack (such as by scratching) to divide the photovoltaic device into a plurality of photovoltaic cells.
[0054] Surface treatment of the top surface of the absorber stack may include passivation prior to forming the improved carrier extraction layer. For example, chemical passivation may be applied to the back surface of the absorber layer prior to forming the p-type back contact. For CdTe-based absorber materials, including doped ternary and quaternary alloys containing similar amounts of cadmium and tellurium, alkaline treatment may produce a Cd-rich surface. The improved carrier extraction layer may be formed over and directly contact the Cd-rich back surface to form an absorption interface, and the formed p-type contact layer may be formed over and directly contact the improved carrier extraction layer. The described structure may beneficially provide a reduced surface recombination velocity at the absorption interface. However, this benefit may be offset by the high temperature formation of the p-type back contact layer (e.g., by depositing a nitrogen-doped zinc telluride layer by vapor transport deposition over the passivated surface of the absorber layer).
[0055] For some embodiments, continued high temperatures may reduce the benefits of the passivation step, damage the improved carrier extraction layer, or may damage other layers of the partially formed device layer stack. In order to maintain absorber passivation and layer stack integrity, processing steps after absorber surface passivation can be selected to avoid or limit exposure of intermediate structures (where the absorber layer is above the substrate stack) to high temperatures or other conditions that may cause damage. Many p-type contact materials (including most organic polymer hole transport materials) are easily damaged by heat, moisture, etchants and some solvents. Due to these limitations, many processes used for other photovoltaic devices or for early deposited layers may not be suitable for processing steps after the absorber layer Cd enrichment step and the improved carrier extraction layer formation.
[0056] In some embodiments, the step of depositing the layer using a low temperature method is performed by at least one of thermal evaporation, spray pyrolysis, closed space sublimation (CSS), chemical vapor deposition (CVD), atomic layer deposition (ALD), spin coating, spray coating, slot extrusion coating, blade coating, roller coating, dip coating, inkjet printing, or sol-gel coating. In some embodiments, the step of depositing the layer using a low temperature method will prevent excessive heating of the substrate layer stack during the deposition process and is performed at a substrate temperature at or below 150° C., at or below 120° C., or at or below 100° C.
[0057] Passivation of the absorber surface can be performed by alkaline chemical surface cleaning, which can further provide surface cleaning, surface organic contaminant removal and oxide removal. The term "cleaning" or "washing" includes subjecting a surface, such as the back surface of the absorber layer, to, exposing or contacting a cleaning solution. As a non-limiting example, the surface can be at least partially immersed in a bath by immersing the surface in the cleaning solution, or the cleaning solution can be applied to the substrate by spraying, coating, brushing, flowing or otherwise allowing the bath to contact at least a portion of the surface. In addition, the surface of the partially formed device can be subjected to surface cleaning or passivation in a continuous process, such as continuously feeding the substrate into and out of the cleaning solution by a conveyor, or in a batch process.
[0058] Now go to Figure 4 , the ICE layer 170 includes a plurality of molecules 400. Each molecule 400 has a head group 410, a body 420, and may also include a functional end group 430. The head group 410 includes a thiol or a thiol derivative having a sulfur atom (SH) bonded to hydrogen. The body 420 or R-group includes an organic portion covalently bonded to the head group 410. The functional end group 430 or tail includes a functional group that can be represented as X, and the end group 430 is covalently bonded to the body 420. Therefore, the structure of the thiol-based molecule used to form the ICE layer 170 can be represented as a structure having XR-SH.
[0059] The molecule 400 may have a strong molecular dipole. The molecule may be oriented relative to the substrate so that the head group 410 faces the absorber stack 115. In some embodiments, the oriented molecules form a substantially continuous self-assembled monolayer (SAM). The head group 410 may be deprotonated and the sulfur of the head group 410 may be bonded to the Cd atom at the back surface 164 of the absorber. The structure, composition and spatial properties of the main body 420 may adjust the packing density of the molecules 400 forming the ICE layer and may regulate charge transport. The structure and composition of the end group 430 may change the dipole moment of the molecules forming the ICE layer 170 and regulate the surface work function of the absorber / ICE layer stack. In some embodiments, the thiol-based molecule may have a molecular weight in the range of 50-400 Daltons or in the range of 100-200 Daltons.
[0060] Figure 4 A simplified depiction of forming an example ICE layer 170 on an absorber stack 115 is shown. Unbound isolated molecules 400 in solution are in contact with the absorber stack 115 at the absorber back surface 164. The thiol constituents of the head groups 410 are oriented toward the absorber back surface 164. Figure 4 Moving from left to right in FIG. 4 , additional molecules 400 aggregate into a generally ordered layer to form an ICE layer 170 on the absorber stack 115 .
[0061] The thiol composition may include an X group 430, which increases the polarity of the molecule and the dipole moment generated. These include, for example, electron withdrawing groups, such as X groups including fluorine atoms, to generate a negative charge from the X group pointing to the thiol head to a positive charge dipole direction. These also include, for example, electron donating groups, such as X groups including amines, to generate a negative charge from the thiol head pointing to the X group to a positive charge dipole direction. In some embodiments, the dipole moment generated on the thiol molecule exceeds 0.5 debye. In some embodiments, the thiol composition includes an R group 420 composed of an alkane chain or a phenol group. In some embodiments, the thiol composition includes a sufficiently small R group that does not spatially restrict bonding to adjacent Cd sites, thereby facilitating dense molecular stacking and bonding to a high proportion of available Cd sites. In some embodiments, the ICE layer increases the surface work function by up to 450meV relative to the value when there is no ICE layer. In some embodiments, the ICE layer reduces the surface work function by up to 150meV relative to the value when there is no ICE layer. In some embodiments, this produces a surface work function as high as 5.15 eV or as low as 4.55 eV.In some embodiments, the ICE layer consists essentially of a single molecular monolayer of the thiol compound.
[0062] The ICE layer can be formed on the passivation surface of the absorber layer stack 115. The absorber layer stack 115 can have a Cd-rich layer at the surface region 364. The ICE layer 170 can include a plurality of molecules, wherein the molecules are dipoles and include an organic sulfur compound. The ICE layer 170 can be between the absorber layer 160 and the p-type contact layer 180 and directly contact both the absorber layer 160 and the p-type contact layer 180. The p-type contact layer 180 can include a polymer, a small molecule, or an inorganic compound. Without being bound by theory, the applicant has found that when the ICE layer is formed in contact with a II-VI type semiconductor alloy containing cadmium (Cd), providing these materials as described can produce improved electrical properties. It is also believed that the combination of selected materials can provide a robust structure that is resistant to degradation.
[0063] It was found that thiol-based compounds can be paired with CdTe-based absorbers and other II-VI alloys, and further paired with organic and small molecule p-type contact materials to form improved carrier extraction layers that exhibit a combination of superior optical and electrical properties relative to conventional back contact materials. It was also found that selected compositions that can enhance p-type carrier collection are also well suited for use in manufacturing processes.
[0064] FIG5 shows a simplified energy level diagram illustrating the change in surface work function produced by including AET or 4-FTP as an improved carrier extraction layer between an absorber layer comprising a CdSeTe alloy and a PTAA p-type contact layer. F) and the vacuum level corresponds to the work function (Φ). As indicated by the dashed line, in a given e with AET - In the case of the X-group tail, the surface work function of CdSeTe becomes smaller, giving a more positive valence band shift with PTAA relative to the case without the ICE layer. - In the case of the X-group tail, the surface work function of CdSeTe becomes larger, giving a more negative valence band offset with PTAA relative to the case without the ICE layer. As observed in this figure, the dipole of 4-FTP produces a smaller or more negative valence band offset (VBO) compared to AET, thereby improving the transport of holes.
[0065] Fig. 6A and 6B The energy band diagram of p-type CdTe is shown. Fig. 6A and 6B shows that before applying the EDT layer to the absorber ( Fig. 6A ) and after ( Figure 6B ) shows the effect of chemical passivation by showing an absorber layer containing p-type CdTe material. The electronic energy states (bands) in the material can bend up or down near the junction. In each band diagram, this band bending (E bb ); also shows the vacuum energy level (E vac ) and work function (W f ). Fermi level pinning can create an energy barrier for the flow of electrons and holes, thus reducing efficiency. Figure 6B and Fig. 6A The chemical passivation from Cd-S bonding at the surface was shown to reduce Fermi level pinning and improve band bending. This also affected the work function, which increased after applying the EDT layer.
[0066] Fig. 7A and 7B The energy band diagram of p-type CdTe is shown. Fig. 7A Corresponding to the structure with AET layer. Figure 7B Corresponding to a structure with 4-FTP layers. Fig. 7A and Figure 7B The shift of the work function to the opposite direction due to the charge difference of the surface dipoles is shown. Fig. 7A and Figure 7B The p-CdTe material and the AET material ( Fig. 7A ) or 4-FTP material ( Figure 7B ) is the energy band diagram of the absorption layer. The work function of the surface can be proportional to the dipole change caused by the absorption of the ICE layer. Fig. 7A and 7BAs observed in Fig. 7A ) compared to the dipole moment caused by 4-FTP material ( Figure 7B ) causes the dipole moment to increase the work function.
[0067] Changing the material of the ICE layer and changing the positive and negative orientation of the dipoles will change the work function to higher or lower and lead to a change in the valence band offset (VBO).
[0068] refer to Figures 8A-8B and Fig. 9 , devices with selected chemical compounds for the ICE layer were produced and tested. Tested materials for the ICE layer included: 2-aminoethanethiol (AET); L-cysteine (L-Cys); thioglycolic acid (TGA); 1-octanethiol (OT); 4-fluorothiophenol (4-FTP); 4-fluorobenzyl mercaptan (4-FMB); 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluoro-1-octanethiol (TDF-OT); 4-trifluoromethylbenzyl mercaptan (4-TFMBM); and 1,2-ethanedithiol (EDT).
[0069] Fig. 8A and 8B The film side of the absorber layer ( Fig. 8A ) and the sunny side ( Figure 8B ) versus wavelength. The stages include: a first stage before potassium hydroxide (KOH) treatment; a second stage after applying the KOH treatment to the absorber layer; and a third stage after applying the ICE layer to the absorber layer.
[0070] Photoluminescence (PL) can indicate the quality of the active layer of a solar cell. Film-side or back-side PL measurements are a more direct measure of the quality of the back surface passivation. Sun-side or front-side PL is more indicative of the overall minority carrier lifetime within the device and is less sensitive to back surface treatment and more sensitive to bulk quality. Figures 8A-8B The PL improvement shown in is largely related to chemical passivation at the absorber back interface and is independent of the presence or orientation of the dipole moment. Cd-S bonding reduces the number of dangling Cd bonds at the surface, thus providing chemical passivation. The increase in both the front and back PL observed after the Cd-rich back surface treatment and after the formation of the ICE layer shows that this treatment significantly reduces the non-radiative recombination of photogenerated carriers, indicating an effect on the solar cell Voc. As can be seen from Fig. 8AAs can be observed in Figure 2, devices using AET, EDT, and 4-FTP all show at least an order of magnitude increase in PL on the membrane side. A doubling of the PL corresponds to a 20 mV increase in the open circuit voltage (Voc). PL from the ICE layer and the KOH surface treatment is also evident in the PL measurements on the sun-facing side.
[0071] The backside PL measurement is a more direct measure of the quality of the back surface passivation. The frontside PL is more indicative of the overall minority carrier lifetime within the device and is therefore less sensitive to the back surface treatment and more sensitive to the bulk and front interface quality. The increase in both the frontside and backside PL observed after the Cd-rich back surface treatment and after the formation of the ICE layer shows that this treatment significantly reduces the non-radiative recombination of photogenerated carriers diffusing from the front side, indicating a positive impact on the solar cell Voc.
[0072] Fig. 9 A graph comparing the surface work function (Wf) measured by measuring the contact potential difference (CPD) of the absorber layer at different stages by a vibrating Kelvin probe is shown. The stages include: a first stage in which the absorber layer has a liquid photoresist (NPR) and a KOH treatment; a second stage in which the absorber layer also includes an ICE layer; and a third stage in which the absorber layer also includes a poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine (PTAA) layer. The Kelvin probe technique is used to determine the CPD, which can be directly related to the work function of the absorber layer at different stages. The CPD can be defined as the potential difference between a point near the surface of the absorber layer and a point near the surface of the Kelvin probe at different stages. The CPD can be further calculated by the formula V CPD = is related to the work function, where V CPD is the CPD, Φsample is the work function of the sample (absorption layer at different stages), Φprobe is the work function of the probe, and e is the elementary charge.
[0073] like Fig. 9 As shown in , different materials of the ICE layer directly affect the tunability of the surface work function, which can be directly correlated to the work function. It is worth noting that it can be observed that three materials, 4-FBM, TDF-OT, and 4-TFMBM, have stronger dipoles than 4-FTP. The work function of the surface can be proportional to the dipole change caused by the ICE layer. Experimental data show that OT and 4-FTP have dipole polarity, which will transform the band alignment with PTAA, thereby improving the carrier selectivity of the PTAA contact. This will improve the conductivity of holes while promoting the reflection of electrons.
[0074] The comparative performance characteristics shown in Figures 6-8 and in the comparative test results indicate that the structures tested are effective. Good efficiency, stabilized absorber surface passivation, improvement in fill factor (FF), low charge carrier recombination, low shunting, and good carrier concentration levels were observed. The metrics show that the structures tested performed similarly or better than the control in multiple parameters.
[0075] Figures 10A-10E Comparative performance characteristics are shown, including efficiency (Eff), open circuit voltage (V OC ), fill factor (FF), open circuit resistance (R OC ) and short-circuit current density (J SC ). In this set of measurements, the example devices were prepared by alkaline passivation of an absorber layer comprising cadmium and tellurium, followed by application of 4-FTP as an interface carrier enhancement layer, and application of PTAA as a p-type contact layer. Both the example and comparative devices were treated by contacting the second surface of the absorber with an alkaline passivating agent. In one set of comparative devices (left column), the back contact was applied directly on top of the absorber layer. In another set of comparative devices (middle column), a p-type contact layer comprising PTAA was applied directly on top of the absorber layer, and a back contact was applied directly on top of the PTAA. In the example devices (right column), an ICE layer comprising 4-FTP was applied directly on top of the absorber layer, a p-type contact layer comprising PTAA was applied directly on top of the ICE layer, and a back contact was applied directly on top of the PTAA. The results show that the experimental devices have excellent performance in terms of efficiency, open circuit voltage, and fill factor. The experimental devices exhibit comparable performance in terms of short circuit current density. The data show that the experimental devices improve hole transport and maintain or enhance absorber layer passivation.
[0076] Without wishing to be bound by theory, the ICE layer may consist essentially of a self-assembled monolayer in which sulfur atoms of thiol-based compounds bind to cadmium on the absorber surface. The ICE layer may modulate band alignment between layers, such as between the absorber and the p-type contact, by effectively passivating the depinning of the surface Fermi level and / or providing additional fields through built-in dipoles. The p-type contact layer may comprise a hole transport material (HTM), such as an organic, inorganic or small molecule composition.
[0077] Hole transport materials (HTMs) have high hole mobility and low electron affinity. Therefore, when minority carriers (electrons) reach the back contact interface, the HTM blocks their transmission through the p-type contact and minimizes interfacial recombination, while allowing easy transmission of majority carriers (holes). The p-type contact layer can be deposited at low temperature to prevent damage to the ICE layer and maintain the chemical passivation state of the absorber surface. The p-type contact layer can be deposited on the ICE layer, which can be formed on a cadmium-rich or stoichiometric CdTe surface, where the cadmium-rich or stoichiometric surface can be prepared by treating the as-grown CdTe polycrystalline film with one or more alkaline solutions such as potassium hydroxide or tetramethylammonium hydroxide.
[0078] The p-type contact layer that can be formed above the ICE layer has a large conduction band offset from CdTe to block electron recombination at the metal contact, and a small valence band offset to allow efficient hole transport. As the diffusion length of photogenerated minority carriers becomes comparable to the thickness of the absorber film, the value of the back contact surface recombination velocity can significantly affect the overall device recombination current. In addition, for bifacial solar cell designs, the reduction in back contact surface recombination has a large impact on the open circuit voltage and the potential for back-side illumination efficiency gain. A reduction in the back contact recombination rate can result in photovoltaic devices with improved minority carrier lifetimes and higher open circuit voltages (Voc).
[0079] In an exemplary method, a device is prepared. A TCO on glass can be used as a front electrode. An absorber can be deposited directly on the TCO layer or can be deposited on a buffer layer or a transparent layer above the TCO layer to form an absorber stack. The absorber material can include CdTe and other II-VI semiconductor alloys, for example, sublayers of cadmium selenide telluride with cadmium telluride, cadmium zinc telluride, cadmium selenide and / or zinc telluride. The absorber can be doped. The absorber surface can be surface treated. The treatment can include doping, heat treatment with cadmium chloride to passivate the surface, cleaning the surface with acid or base and / or removing oxides. In an exemplary process, the absorber stack can be subjected to a chloride heat treatment, followed by a potassium hydroxide (KOH) alkaline wash, thereby forming a passivated surface and a Cd-rich back interface of the absorber at the back surface region of the absorber stack. A thiol-based molecular material can then be deposited on and in contact with the treated surface of the absorber layer to form an improved carrier extraction (ICE) layer. A p-type contact material can then be deposited on and in contact with the ICE layer.
[0080] In order to passivate the absorber surface in preparation for forming the ICE layer, it may be desirable to reduce the surface Te dangling bonds and adjust the surface stoichiometry to the desired ratio, and alkaline etching or passivation with a cleaning solution may be performed. In one example, the method for adjusting the surface stoichiometry of the II-VI semiconductor material includes adjusting the concentration of the cleaning solution to achieve the desired stoichiometric ratio on the surface of the semiconductor material, and passivating the semiconductor material with the cleaning solution. The pH of the cleaning solution can be adjusted to change the surface ratio of Cd to Te in the absorber stack containing an absorber layer, which contains a II-VI semiconductor material alloy including cadmium and tellurium. Using, for example, an alkaline cleaning solution with a pH level between about 8 and 14, a substantially stoichiometric CdTe surface can be modified to a surface having a Cd-rich surface. In some embodiments, the cleaning solution pH level is between 11 and 13. Cleaning passivation can be used to optimize the surface chemistry and electronic properties of the back contact.
[0081] In some embodiments, the cleaning solution comprises a hydroxide. In some embodiments, the cleaning solution comprises an aqueous solution of sodium hydroxide (NaOH), potassium hydroxide (KOH), or tetramethylammonium hydroxide ((CH3)4N(OH)) (also known as TMAH). In some embodiments, the cleaning solution comprises KOH. In some embodiments, the cleaning solution comprises KOH at a concentration in the range of about 0.001M to about 11.67M, in the range of 0.500M to 4.000M, in the range of 1.500M to 2.750M, or in the range of 1.750M to 2.000M. In some embodiments, the cleaning solution comprises 1.50 to 2.00M KOH. In some embodiments, the cleaning solution is contacted with the surface for a contact time in the range of 10 seconds to 90 minutes. In some embodiments, the contact time is in the range of 30 seconds to 30 minutes, or in the range of 30 seconds to 10 minutes. In some embodiments, the contact time is 1 minute. In some embodiments, the cleaning solution temperature is in the range of 0°C to 90°C. In some embodiments, the cleaning liquid temperature is in the range of 20° C. to 30° C. In some embodiments, the cleaning liquid temperature is in the range of 5° C. to 50° C. or in the range of 15° C. to 35° C. In some embodiments, the absorbent surface is rinsed with water after contacting with KOH.
[0082] In some embodiments, the ratio of Cd to Te at the Cd-rich surface region of the absorber layer is in the range of 1: 1 to 4: 1. In some embodiments, the ratio of Cd to Te at the Cd-rich surface region of the absorber layer is greater than 1: 1. In some embodiments, the ratio of Cd to Te at the Cd-rich surface of the absorber layer is between 1.3: 1 and 2.5: 1 as measured by XPS.
[0083] An improved charge carrier extraction (ICE) layer is formed over the treated absorber stack. In some embodiments, the ICE layer is formed in contact with the Cd-rich surface region of the absorber layer.
[0084] In one example, a solution of a thiol-based molecular material in ethanol is provided at a concentration of about 0.01M-0.1M and the solution is contacted with the passivated back surface of the absorber stack for a duration in the range of 20 minutes to 36 hours. In some embodiments, the contact duration is in the range of 30 minutes to 180 minutes. In some embodiments, the sample is rinsed with ethanol to remove aggregates from the surface and the sample is placed in an ethanol ultrasonic bath for 1 to 20 minutes and then dried with compressed air or nitrogen.
[0085] The p-type contact material can be deposited directly on the ICE layer by various methods, including, for example, sputtering, spin coating, or evaporation. In one example, the p-type contact material comprises PTAA. In one example, the structure of the thin film junction stack formed is TCO / CdSeTe / CdTe:As / 4-FTP / PTAA. The partially formed device stack can then be heat treated, for example, at 80-150°C for 30-120 minutes. Post-deposition heat treatment of the p-type contact can be performed using a hot plate, an oven, and / or a pressure-controlled heating chamber. A conductive material can then be applied over the p-type contact layer.
[0086] In one example, a device having a nickel oxide (NiOx) p-type contact layer is prepared. The device is formed with a NiOx layer adjacent to an arsenic-doped p-type absorber comprising a II-VI type alloy including cadmium, tellurium, and selenium.
[0087] Nickel oxide (NiOx) based layers have excellent chemical and thermal stability, and although high temperatures and chemical passivation steps may be used in subsequent processing steps after their deposition, they are convenient to manufacture by maintaining key properties. High temperatures or prolonged heating may have adverse effects on some layers or components of the device, however, NiOx tolerates these same conditions. NiOx does not react with arsenic dopants. Compared with organic p-type charge carrier contact layers, NiOx has excellent chemical stability, low light absorption and relatively high mobility. It has a high conduction band edge and provides electronic blocking. In undoped NiOx, p-type conductivity mainly comes from nickel vacancies.
[0088] NiOx can be deposited by many different methods. For example, the preparation of NiOx layer can be achieved by sputtering, pulsed laser deposition or by thermal decomposition of nickel salts such as chlorides, nitrates or acetates. The NiOx layer can be doped during the deposition process. In some embodiments, it is beneficial for the p-type contact layer to form a NiOx film with a thickness of only a few nanometers. It is usually difficult to deposit an ultra-thin NiOx layer with high film quality.
[0089] In some embodiments, it is beneficial to form a p-type contact layer such as a NiOx film using a low temperature method to prevent damage to the lower layer of the layer stack or to maintain a chemical passivation state on the surface of the absorber layer. Although NiOx tolerates high processing temperatures, it can also be formed without using a high heat method. In one example, a sol-gel prepared from a precursor including a nickel compound such as nickel bis(acetylacetonate) or Ni(acac)2 is used to form a nickel oxide layer. The nickel compound is dissolved in a solvent such as 2-methoxyethanol (EGME) or methoxypropanol (PGME). A chelating base such as triethanolamine (TEOA) is added to form a sol-gel mixture. A dopant is optionally added to the sol-gel mixture. The mixture is then ultrasonically treated to form a sol-gel. The sol-gel is applied to a partially formed device. In one example, a sol-gel coating can be formed by dipping, roller coating, spraying, scraping or spin coating. The NiOx sol-gel coating can be cured by heat treatment at a relatively low temperature or a short time of heat treatment to control the thermal exposure of the layer stack of the partially formed photovoltaic device.
[0090] By changing the concentration of the nickel oxide precursor, the NiOx film thickness can be varied in the range of about 2 to 100 nm. The nickel oxide precursor can be a nickel salt. In some embodiments, the NiOx precursor can be one or more of the following: nickel chloride (NiCl2), nickel nitrate Ni(NO3)2, or nickel acetate Ni(CH3COO)2. In some embodiments, the chelating base is selected from: triethanolamine, diethanolamine, ethanolamine, or tris. In some embodiments, the dopant is selected from: CuCl2, CuCl, CuI, CuSCN, LiCl, LiOAC, KCl, CsCl, CsI, MgCl2, or Mg(OAC)2. In some embodiments, the dopant may include one or more of the following: Li, Cs, Cu, Mg, Sr, or rare earths such as Er, Tb, or Eu. In some embodiments, the NiOx precursor sol-gel can be coated one or more times to produce the desired thickness. In some embodiments, the curing temperature can be between 40°C and 400°C, and the duration can be in the range of 1 minute to 120 minutes. In some embodiments, the curing temperature is less than 350°C, less than 325°C, less than 250°C, or less than 200°C. In some embodiments, the curing temperature is in the range of 80°C to 250°C. In some embodiments, the curing time is between 5 minutes and 60 minutes. In some embodiments, the curing time is between 1 minute and 30 minutes. In some embodiments, the curing time is less than 35 minutes, less than 25 minutes, or less than 15 minutes.
[0091] In some embodiments, the absorber layer comprises an n-type material. In some embodiments, a pn junction is formed by the n-type material of the absorber and one or more p-type layers formed on the absorber stack. The one or more p-type layers formed on the absorber stack may include an ICE layer and a p-type contact layer. In some embodiments, the n-type material of the absorber consists essentially of doped or undoped cadmium selenide.
[0092] In some embodiments, the photovoltaic device may include an improved carrier extraction (ICE) layer between the absorber layer and the conductive layer. The device may include a first p-type contact layer between the absorber layer and the ICE layer; alternatively or in addition, the device may include a second p-type contact layer between the ICE layer and the conductive layer. In some embodiments, the ICE layer may be disposed directly adjacent to and in contact with one or both of the first p-type contact layer and the second p-type contact layer. Alternatively, one or both of the first p-type contact layer and the second p-type contact layer may be omitted, and in some embodiments, the ICE layer is directly adjacent to and in contact with one or both of the absorber layer and the conductive layer.
[0093] In some embodiments, the p-type contact layer comprises: one or more of an oxide, a nitride, or an oxynitride. In some embodiments, the p-type contact layer comprises one or more of zinc, tellurium, cadmium, or molybdenum. In one example, the composition of the p-type contact layer includes nitrogen-doped zinc telluride, nitrogen-doped cadmium zinc telluride, nitrogen-doped zinc oxide, molybdenum nitride, or molybdenum oxynitride. In some embodiments, the p-type contact layer comprises an inorganic sublayer and an organic sublayer comprising a polymer material or a small molecule material.
[0094] In an example device, the ICE layer is between and contacts a first p-type contact layer and a p-type absorber; the absorber comprises cadmium, tellurium, and selenium; the first p-type contact layer comprises a polymer material, such as PTAA; and the device includes a second p-type contact layer over the polymer material, such as a layer comprising zinc telluride; and a conductive layer, such as molybdenum nitride, is disposed over the second p-type contact layer.
[0095] The ICE layer is disposed or formed on and in contact with the lower layer. The lower layer may include a p-type contact layer and / or an absorber layer. In some embodiments, a discontinuous p-type layer is formed on the absorber layer and an ICE layer is formed on the discontinuous p-type contact layer, whereby the ICE layer contacts at least a portion of the top surface of both the absorber layer and the p-type contact layer. In some embodiments, the ICE layer is discontinuous. In some embodiments, the ICE layer covers a portion of the lower layer. In some embodiments, the covered portion is in the range of 10% to 95%, greater than 15%, greater than 20%, greater than 25%, less than 90%, less than 80%, less than 75%, or less than 60%.
[0096] In some embodiments, the ICE layer is formed on and in contact with a p-type contact layer comprising zinc and tellurium. In some embodiments, the ICE layer is formed on and in contact with a p-type layer comprising one or more of cadmium, zinc, tellurium, nitrogen, oxygen, or selenium. In some embodiments, the ICE layer is formed on and in contact with an n-type absorber layer comprising cadmium and selenium.
[0097] In some embodiments, the conductive layer may include a conductive material, such as one or more layers of metal, oxide, oxynitride, nitride, or nitrogen-containing metal. In some embodiments, the conductive layer includes one or more of the following: oxygen, nitrogen, zinc, tellurium, cadmium, selenium, molybdenum, tungsten, vanadium, silver, nickel, copper, aluminum, titanium, palladium, chromium, molybdenum, gold. In an example embodiment, the conductive layer includes: nitrogen-doped zinc telluride, nitrogen-doped cadmium zinc telluride, nitrogen-doped zinc oxide, molybdenum nitride, or molybdenum oxynitride.
[0098] Experimental results indicate that the use of an ICE layer can create, enhance, or maintain chemical passivation of the interface with an adjacent layer and can change the alignment of the work function with an adjacent metal-containing layer. In some embodiments, the adjacent layer directly contacting the ICE layer may include one or more of an absorber layer, a p-type contact layer, or a conductive layer.
[0099] In some embodiments of the method of manufacturing a device, the surface of the absorber stack may be surface treated. The treatment may include passivating the surface with cadmium chloride heat treatment, applying a dopant, cleaning the surface with an acid or base, and / or removing oxides. In some embodiments, the step of chemical passivation is initiated before contacting the absorber stack with the thiol compound. In some embodiments, the chemical passivation is performed simultaneously or concurrently with the step of applying a composition comprising molecules for forming an ICE layer to the surface of the layer stack. In some embodiments, chemical passivation is produced by applying a composition comprising molecules for forming an ICE layer to the surface of the layer stack.
[0100] In one example process, the absorber stack may be subjected to a chloride heat treatment followed by an alkaline wash, whereby the surface region of the absorber stack is chemically passivated. In some embodiments, the top surface of the absorber stack is surface treated by contact with at least one passivating composition. In some embodiments, the passivating composition comprises a sodium salt, a lithium salt, or a potassium salt. In some embodiments, the passivating composition comprises a thiol, an organic sulfur compound, a hydroxide, or an acetate. In some embodiments, the passivating composition is selected from the following materials: sodium acetate, betaine, potassium hydroxide, and tetramethylammonium hydroxide.
[0101] In some embodiments of the method, after surface treatment of the absorber stack, a layer is deposited on the absorber stack using a controlled temperature method. The step of depositing a layer on the absorber stack using a controlled temperature method prevents excessive heating of the substrate layer stack during the deposition process by limiting the duration of exposure to a temperature of 120° C. or above to a duration in the range of 0 to 20 minutes, less than 15 minutes, less than 10 minutes, less than 5 minutes, or less than 2 minutes. In some embodiments, the controlled temperature deposition includes sputtering.
[0102] According to embodiments described herein, a photovoltaic device may include an absorber layer on a substrate stack, the absorber layer comprising cadmium. The photovoltaic device may include a p-type back contact layer formed on a back interface of the absorber layer. The photovoltaic device may include an interface carrier enhancement (ICE) layer between the absorber layer and the p-type back contact layer, and the ICE layer may directly contact the back interface of the absorber layer. The ICE layer comprises sulfur in a deprotonated thiol compound.
[0103] The surface work function of the ICE layer on the layer stack can be tuned over a 600 meV range by thiol compound selection. The surface work function can be assessed by Kelvin probe measurements of the surface work function. The use of the ICE layer results in a shift to a more favorable band alignment with the p-type contact layer (including hole transport material (HTM)) or the back contact layer.
[0104] In some embodiments, the surface work function of the ICE layer has a value amplitude in the range of 4.55 eV to 5.15 eV as measured after the ICE layer is deposited. In some embodiments, the surface work function of the ICE layer has a value amplitude in the range of 4.6 eV to 5.0 eV as measured after the HTM layer is deposited.
[0105] The use of an ICE layer can create, enhance, or maintain chemical passivation of the interface with the cadmium-containing absorber layer. In some embodiments, the absorber layer comprises cadmium and tellurium, and the ratio of Cd to Te in the surface region of the absorber layer is greater than or equal to 1: 1. In some embodiments, the absorber layer comprises tellurium and the ratio of Cd to Te in the surface region of the absorber layer is in the range of 1: 1 to 4: 1.
[0106] In some embodiments, the thiol compound comprises at least one of: isothiourea; cysteamine, also known as 2-aminoethanethiol (AET); 4-fluorothiophenol (4-FTP); 4-aminothiophenol (4-ATP); 1,2-ethanedithiol, also known as ethylenethiol (EDT); L-cysteine, also known as (R)-2-amino-3-mercaptopropionic acid (L-Cys); thioglycolic acid, also known as thioglycolic acid (TGA); 1-octanethiol (OT); 4-fluorobenzylthiol, also known as (4-fluorophenyl)methanethiol (4-FMB); 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluoro-1-octanethiol (TDF-OT); or 4-trifluoromethylbenzylthiol (4-TFMBM).
[0107] In some embodiments, the thiol compound comprises at least one of: TDF-OT, 4-FTP, OT, AET, or 4-FMB.
[0108] In some embodiments, the back contact comprises at least one of: PTAA, poly-TPD, TFB, PF8-TAA, PIF8-TAA, NiOx, or P3HT.
[0109] In some embodiments, the photovoltaic device has improved p-type carrier lifetime. In some embodiments, the average p-type carrier lifetime is greater than 5.0 ns. In some embodiments, the average p-type carrier lifetime is greater than 10 ns. In some embodiments, the average p-type carrier lifetime is in the range of 10 ns to 20 ns.
[0110] In some embodiments, the absorber layer of the photovoltaic device comprises a II-VI semiconductor, wherein the II-type material comprises cadmium (Cd) and the VI-type material comprises tellurium (Te); the absorber layer is doped with at least one dopant selected from phosphorus, arsenic, antimony, or bismuth; the ICE layer is directly adjacent to the second surface of the absorber layer at the passivation surface region, and the ratio of Cd to Te is greater than or equal to 1:1. In some embodiments, the p-type contact layer of the photovoltaic device is directly adjacent to the second surface of the ICE layer, and the p-type contact layer comprises at least one of PTAA, P3HT, poly-TPD, TFB, TTF-1, PF8-TAA, PIF8-TAA, SGT-407, PCDTBT, SpiroOMeTAD, anthracene-based HTM, polythiophene, semiconducting polymer, NiO, CuSCN, or CuI. In some embodiments, the device comprises a conductive layer on the p-type contact layer.
[0111] In some embodiments, the valence band offset from the p-type contact layer is reduced by the presence of the ICE layer.
[0112] In some embodiments, the energy level barrier height at the interface with the p-type contact layer is reduced due to the presence of the ICE layer. In some embodiments, the energy level barrier height at the interface with the p-type contact layer is reduced by 20 to 150 meV due to the presence of the ICE layer compared to a control device without an ICE layer. In some embodiments, the energy level barrier height at the interface with the p-type contact layer is reduced by 50 to 450 meV due to the presence of the ICE layer compared to a control device without an ICE layer.
[0113] In some embodiments, the hole carrier density in the p-type contact layer is increased by the presence of the ICE layer. In some embodiments, the hole carrier density in the p-type contact layer is increased by 50% or more by the presence of the ICE layer compared to a control device without the ICE layer. In some embodiments, this increase in hole carrier density can result in a 50% or more reduction in resistance measured at an open circuit voltage, including a reduction in resistance of more than an order of magnitude.
[0114] In some embodiments, the surface work function is increased by up to 450 meV in the presence of an ICE layer compared to a surface without an ICE layer, or decreased by up to 150 meV in the presence of an ICE layer compared to a surface without an ICE layer.
[0115] According to embodiments described herein, a partially formed photovoltaic layer stack may include an interfacial charge enhancement (ICE) layer between an absorber layer and a p-type contact layer on the substrate stack. The ICE layer includes a deprotonated thiol compound.
[0116] In some embodiments, a partially formed device having an absorber layer stack, an ICE layer, and a p-type contact layer produces a film-side photoluminescence intensity enhancement of two to ten times greater than a comparable partially formed device stack without an ICE layer.
[0117] In some embodiments, the thin film junction stack of the device structure can be adapted for use in tandem photovoltaic devices or in bifacial modules.
[0118] In some embodiments, the ICE layer can have an average transmittance greater than 50% for light having a wavelength between 400 nm and 700 nm. In some embodiments, the ICE layer 170 can have an average transmittance greater than about 50% for light having a wavelength between 400 nm and 1000 nm, for example, greater than about 85% in one embodiment, or greater than about 90% in another embodiment, or greater than about 95% in yet another embodiment.
[0119] In some embodiments, the ICE layer is disposed in a tandem photovoltaic device. The ICE layer may be disposed in a tandem bifacial photovoltaic device. In some embodiments, the tandem device has a top cell and a bottom cell, and the top cell includes the ICE layer.
[0120] Methods of making photovoltaic devices are provided. Methods of processing absorber stacks for making photovoltaic devices are provided. Methods of passivating absorber layers and maintaining passivation by forming an ICE layer in direct contact with the absorber layers are provided. Methods of aligning band structures between absorbers and p-type contact layers are provided. Methods of adjusting the surface work function of an ICE layer within a 600 meV range as measured by Kelvin probe measurements of the surface work function are provided, wherein the ICE layer is disposed between the absorber layer and the p-type contact layer, thereby producing a shift to a more favorable band alignment with the p-type contact layer.
[0121] According to embodiments described herein, a method may include providing an absorber stack having an absorber layer comprising cadmium (Cd). The method may include passivating a surface of the absorber layer to form a passivated surface at a back interface. The method may include forming an improved carrier extraction (ICE) layer on the passivated surface by depositing molecules of a thiol compound on the passivated surface, wherein the molecules have a dipole moment, whereby the thiol compound forms an ICE layer in direct contact with the back interface of the absorber layer. The method may include forming a p-type back contact layer on the ICE layer.
[0122] In some embodiments, the thiol compound comprises a thiophenol or an alkanethiol compound.
[0123] In some embodiments, the passivating step includes contacting the surface of the absorber layer with a basic passivating agent.
[0124] In some embodiments, the thiol compound molecule comprises a head group having a hydrogen-sulfur bond, and the step of forming the ICE layer comprises deprotonating at least a portion of the head group of the molecule, whereby the sulfur of the head group forms a complex with the Cd at the passivation surface and the molecules of the ICE layer are substantially aligned at the back interface, whereby the sulfur of the head region of the molecule is close to the absorber relative to the bulk of the molecule, and the ICE layer comprises a deprotonated conjugate of the thiol compound.
[0125] In some embodiments, the absorber comprises tellurium and the ratio of Cd to Te in the surface region of the absorber layer is greater than or equal to 1:1.
[0126] In some embodiments, the absorber layer comprises a II-VI type semiconductor, wherein the II type material comprises cadmium (Cd) and the VI type material comprises tellurium (Te); and the absorber layer is doped with at least one dopant selected from phosphorus, arsenic, antimony or bismuth.
[0127] In some embodiments, the ICE layer includes sulfur, and the sulfur forms a complex with Cd at the passivating surface of the absorber layer.
[0128] In some embodiments, the passivation step includes contacting the surface of the absorber layer with an alkaline passivating agent. In some embodiments, the alkaline passivating agent comprises at least one of sodium hydroxide (NaOH), potassium hydroxide (KOH), or tetramethylammonium hydroxide ((CH3)4N(OH))TMAH. In some embodiments, the passivation step includes contacting the surface of the absorber layer with an alkaline passivating agent, wherein the surface region of the absorber layer comprises cadmium and tellurium, whereby passivation produces a Cd to Te ratio in the range of 1:1 to 4:1 in the surface region of the absorber layer. In some embodiments, the ratio of Cd to Te in the surface region of the absorber layer is greater than 1:1. In some embodiments, the surface region of the absorber layer consists essentially of a CdTe alloy. In some embodiments, the surface region of the absorber layer comprises a region of the absorber layer at a second surface of the absorber layer and extending into the absorber layer to a depth in the range of 0.2nm to 15nm.
[0129] In some embodiments, providing an absorber stack includes forming an absorber layer over the substrate stack, wherein the absorber layer comprises a II-VI semiconductor, and wherein forming the absorber layer further includes doping, passivation; and removing surface oxide from the II-VI semiconductor prior to depositing the ICE layer.
[0130] In some embodiments, forming the ICE layer comprises depositing a liquid suspension of one or more thiol compounds onto the absorber layer. In some embodiments, the one or more thiol compounds are deposited by dip coating, slot die coating, knife coating, roller coating, spray coating, or spin coating.
[0131] In some embodiments, the ICE layer comprises a compound selected from the group consisting of isothiourea; AET; 4-FTP; 4-ATP; EDT; L-Cys; TGA; OT; 4-FMB; TDF-OT; 4-TFMBM, or a combination thereof. In some embodiments, the ICE layer consists essentially of a compound selected from the group consisting of isothiourea; AET; 4-FTP; 4-ATP; EDT; L-Cys; TGA; OT; 4-FMB; TDF-OT; or 4-TFMBM. In some embodiments, the ICE layer consists essentially of a compound selected from the group consisting of TDF-OT, 4-FTP, OT, or 4-FMB.
[0132] In some embodiments, the ICE layer comprises a monolayer of thiol ligands having a dipole moment aligned with respect to the absorber surface. In some embodiments, the ICE layer consists essentially of a monolayer of thiol ligands having a dipole moment aligned with respect to the absorber surface. In some embodiments, the ICE layer molecules form bonds with the back interface of the absorber layer. In some embodiments, sulfur atoms in the molecules forming the ICE layer are bonded to cadmium atoms at the back interface of the absorber layer.
[0133] In some embodiments, the ICE layer comprises a thiophenol or alkanethiol compound. In some embodiments, the ICE layer comprises a fluorinated thiophenol or alkanethiol compound. In some embodiments, the ICE layer comprises a thiophenol or alkanethiol compound having a primary amine group.
[0134] In some embodiments, the ICE layer comprises thiol ligands spatially arranged to densely bind adjacent Cd sites.
[0135] In some embodiments, the ICE layer is directly between and in direct contact with both the absorber layer and the p-type contact layer.
[0136] In some embodiments, the step of depositing the p-type contact layer is performed at an absorber layer stack temperature at or below 150° C. In some embodiments, the p-type contact layer is deposited by slot extrusion coating, blade coating, roller coating, spray coating, spin coating, sputtering, evaporation, or sol-gel formation. In some embodiments, the p-type contact layer comprises at least one of PTAA, P3HT, poly-TPD, TFB, TTF-1, PF8-TAA, PIF8-TAA, SGT-407, PCDTBT, SpiroOMeTAD, anthracene-based HTM, polythiophene, a semiconducting polymer, NiO, CuSCN, or CuI.
[0137] In some embodiments, the photovoltaic device has a layer comprising sulfur within 20 nm of the second surface of the absorber layer. In one example, the layer comprising sulfur can be detected by at least one of the following: secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), Fourier transform infrared spectroscopy (FTIR), Auger electron spectroscopy (AES), energy dispersive spectroscopy (EDS), Raman spectroscopy, or transmission electron microscopy (TEM). In one example, the layer comprising sulfur can be detected by XPS depth profiling.
[0138] In some embodiments, the ICE layer is formed of a thiol composition comprising: isothiourea; AET; 4-FTP; 4-ATP; EDT; L-Cys; TGA; OT; 4-FMB; TDF-OT; 4-TFMBM; or a combination thereof. In some embodiments, the thiol composition comprises an X group that increases the polarity of the molecule and the dipole moment generated, including, for example, a fluorine atom or an amine. In some embodiments, the dipole moment generated on the thiol molecule exceeds 0.5 Debye. In some embodiments, the thiol composition comprises an R group consisting of an alkane chain or a phenol group. In some embodiments, the thiol composition comprises an R group that is small enough not to spatially restrict bonding to adjacent Cd sites, thereby facilitating dense molecular packing and bonding to a high proportion of available Cd sites. In some embodiments, the ICE layer increases the surface work function by up to 450 meV relative to the value without the ICE layer, or decreases the surface work function by up to 150 meV relative to the value without the ICE layer. In some embodiments, the ICE layer increases the surface work function upward relative to the value without the ICE layer and increases by between 50meV and 450meV, increases by between 75meV and 400meV, increases by at least 100meV, increases by at least 150meV, or increases by 200meV. In some embodiments, the ICE layer is selected to reduce the surface work function relative to the value without the ICE layer and decreases by between 25meV and 150meV, decreases by between 50meV and 125meV, decreases by at least 100meV, decreases by 75meV, or decreases by 50meV. In some embodiments, this produces a surface work function as high as 5.15eV or as low as 4.55eV. In some embodiments, the ICE layer consists essentially of a single molecular monolayer of a thiol compound. In some embodiments, the ICE layer consists essentially of a thiol compound selected from the following: isothiourea; AET; 4-FTP; 4-ATP; EDT; L-Cys; TGA; OT; 4-FMB; TDF-OT; or 4-TFMBM.
[0139] In some embodiments, the thiol compound has a molecular dipole moment with a strength greater than 0.5 Debye. In some embodiments, the thiol compound has a molecular dipole moment with a strength in the range of 0.5 to 11.0 Debye. In some embodiments, the thiol compound has a dipole moment in the range of 1.5 to 8.5 Debye. In some embodiments, the thiol compound has a molecular dipole moment in the range of about 0.5 Debye to about 6 Debye.
[0140] According to embodiments described herein, an ICE layer for a photovoltaic device is provided. In some embodiments, the ICE layer is disposed over the entire directly adjacent passivating absorber layer surface with a substantially uniform thickness. In some embodiments, the ICE layer is disposed over the directly adjacent absorber layer surface with a substantially continuous coverage of 90% to 100% with a substantially uniform thickness.
[0141] In some embodiments, the p-type contact layer includes an HTM layer in contact with the ICE layer, wherein the HTM layer has continuous or discontinuous coverage and a thickness of 0.5 nm to 500 nm. In some embodiments, the thickness of the p-type contact layer is in the range of 0.5 nm to 100 nm, 5 nm to 200 nm, 5 nm to 50 nm, 10 nm to 100 nm, or 10 nm to 50 nm.
[0142] In one example, the p-type contact layer comprises at least one HTM selected from the group consisting of a semiconductor polymer, polytriarylamine, PTAA, poly-TPD, TFB, PF8-TAA, PIF8-TAA, P3HT, PDI, CPB, TCTA, TCP, PCDTBT, anthracene-based HTM, Spiro-OMeTAD, NiOx, CuSCN or CuI, or a combination thereof.
[0143] In some embodiments, forming the absorber layer further includes doping, passivation; and removing oxide from the II-VI semiconductor prior to depositing the ICE layer.
[0144] According to embodiments described herein, there is provided a method of making a photovoltaic device comprising the steps and compositions described.
[0145] It should now be understood that the ICE layer, alone or in combination with a p-type contact layer, can provide an ohmic contact with an absorber layer having improved passivation while providing comparable functionality and reliability relative to known contact layer structures for II-VI absorber materials. Thus, the embodiments provided herein can improve the utility of photovoltaic devices.
[0146] It should be noted that the terms "substantially" and "approximately" may be used herein to represent the inherent degree of uncertainty that may be attributed to any quantitative comparison, value, measurement or other representation. These terms are also used herein to represent the degree by which a quantitative representation may vary from a stated reference without resulting in a change in the basic function of the subject matter at issue.
[0147] Although specific embodiments have been illustrated and described herein, it will be appreciated that various other changes and modifications may be made without departing from the spirit and scope of the claimed subject matter. In addition, although various aspects of the claimed subject matter have been described herein, such aspects need not be used in combination. Therefore, the appended claims are intended to cover all such changes and modifications within the scope of the claimed subject matter.
Claims
1. A photovoltaic device, comprising: an absorber layer on the substrate stack, the absorber layer comprising cadmium; a p-type contact layer formed on a back interface at a second surface of the absorber layer; and an improved carrier extraction (ICE) layer between the absorber layer and the p-type contact layer, wherein: The ICE layer is in contact with the back interface of the absorber layer, The ICE layer comprises sulfur in a deprotonated thiol compound, and By selecting the thiol compound, the surface work function of the ICE layer on the absorber layer can be adjusted within a range of 600 meV as measured by Kelvin probe surface work function measurement. 2 . The device of claim 1 , wherein the absorber layer comprises tellurium, and wherein a ratio of Cd to Te in a surface region of the absorber layer is greater than or equal to 1:
1. 3 . The device of claim 1 , wherein the absorber layer comprises tellurium and wherein a ratio of Cd to Te in a surface region of the absorber layer is in a range of 1:1 to 4:
1.
4. The device of claim 1, wherein the thiol compound has a molecular dipole strength greater than 0.5 Debye.
5. The device according to claim 1, wherein the surface work function of the ICE layer has a value amplitude in the range of 4.55 eV to 5.15 eV as measured after the ICE layer is deposited; or the surface work function of the ICE layer has a value amplitude in the range of 4.6 eV to 5.0 eV as measured after the HTM layer is deposited.
6. The device of claim 1, wherein the thiol compound comprises at least one of: isothiourea; cysteamine, also known as 2-aminoethanethiol (AET); 4-fluorothiophenol (4-FTP); 4-aminothiophenol (4-ATP); 1,2-ethanedithiol, also known as ethylenethiol (EDT); L-cysteine, also known as (R)-2-amino-3-mercaptopropionic acid (L-Cys); thioglycolic acid, also known as thioglycolic acid (TGA); 1-octanethiol (OT); 4-fluorobenzylthiol, also known as (4-fluorophenyl)methylthiol (4-FMB); 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluoro-1-octanethiol (TDF-OT); or 4-trifluoromethylbenzylthiol (4-TFMBM). 7 . The device of claim 1 , wherein the thiol compound comprises at least one of: TDF-OT, 4-FTP, OT, AET, or 4-FMB.
8. The device of claim 1, wherein the back contact comprises at least one of: PTAA, poly-TPD, TFB, PF8-TAA, PIF8-TAA, NiOx, or P3HT.
9. The device of claim 1 , wherein the surface work function is increased by at most 450 meV in the presence of the ICE layer compared to a surface without the ICE layer, or is decreased by at most 150 meV in the presence of the ICE layer compared to a surface without the ICE layer.
10. The device according to claim 1, wherein: The absorber layer comprises a II-VI type semiconductor, wherein the II type material comprises cadmium (Cd) and the VI type material comprises tellurium (Te); The absorber layer is doped with at least one dopant selected from phosphorus, arsenic, antimony or bismuth; The ICE layer is directly adjacent to the second surface of the absorber layer at a passivation surface region, wherein a ratio of Cd to Te in the surface region is greater than or equal to 1:1; The p-type contact layer is directly adjacent to the second surface of the ICE layer; The p-type contact layer comprises at least one of PTAA, P3HT, poly-TPD, TFB, TTF-1, PF8-TAA, PIF8-TAA, SGT-407, PCDTBT, SpiroOMeTAD, anthracene-based HTM, polythiophene, a semiconducting polymer, NiO, CuSCN, or CuI; and The device includes a conductive layer on the p-type contact layer.
11. The device of claim 1, wherein a valence band offset from the p-type contact layer is reduced by the presence of the ICE layer. 12 . The device according to claim 1 , wherein an energy level barrier height at an interface with the p-type contact layer is reduced due to the presence of the ICE layer.
13. The device of claim 1, wherein hole carrier density in the p-type contact layer is increased due to the presence of the ICE layer.
14. The device of claim 1, wherein the ICE layer has a thickness in a range of 0.2 nm to 5.0 nm.
15. A method for manufacturing a photovoltaic device, the method comprising: providing an absorber stack having an absorber layer comprising cadmium (Cd); passivating a surface region of the absorber layer to form a passivated surface at a second surface of the absorber layer; An improved carrier extraction (ICE) layer is formed over the passivated surface, wherein: The ICE layer contacts the second surface of the absorber layer, and The ICE layer comprises sulfur in a deprotonated thiol compound; and A p-type contact layer is formed over the ICE layer.
16. The method of claim 15, wherein the surface work function of the ICE layer on the absorber layer can be adjusted within a range of 600 meV measured by Kelvin probe measurement of the surface work function by selecting a thiol compound.
17. The method of claim 15, wherein the passivating step comprises contacting the second surface of the absorber layer with an alkaline passivating agent.
18. The method of claim 15, wherein the absorber layer comprises tellurium and wherein a ratio of Cd to Te in the surface region of the absorber layer is greater than or equal to 1:
1.
19. The method of claim 15, wherein the ICE layer comprises sulfur, and wherein the sulfur forms a complex with Cd at the passivated surface, and whereby the ICE layer produces a photoluminescence intensity enhancement of 2-10 times the photoluminescence intensity of a comparative device without an ICE layer.
20. The method of claim 15, wherein the ICE layer comprises a compound selected from the group consisting of: isothiourea; AET; 4-FTP; 4-ATP; EDT; L-Cys; TGA; OT; 4-FMB; TDF-OT; or 4-TFMBM.
21. The method of claim 15, wherein the step of depositing the p-type contact layer is performed at an absorber layer stack temperature at or below 150°C.
22. The method of claim 15, wherein the passivation step comprises: The surface of the absorption layer is contacted with an alkaline passivating agent, wherein the alkaline passivating agent comprises at least one of the following: sodium hydroxide (NaOH), potassium hydroxide (KOH) or tetramethylammonium hydroxide ((CH3)4N(OH))TMAH.
23. The method of claim 15, wherein the p-type contact layer is deposited by slot die coating, knife coating, roller coating, spray coating, spin coating, sputtering, evaporation, or sol-gel formation.
24. The method of claim 15, wherein providing the absorber layer stack comprises forming the absorber layer on top of a substrate stack, wherein the absorber layer comprises a II-VI type semiconductor, and wherein forming the absorber layer further comprises doping, passivation; and removing oxide from the II-VI type semiconductor prior to depositing the ICE layer.
25. The method of claim 15, wherein the ICE layer comprises a monolayer of thiol ligands having a dipole moment aligned with respect to the second surface of the absorber layer.
26. The method of claim 15, wherein the ICE layer comprises a thiophenol or an alkanethiol compound.
27. The method of claim 15, wherein the ICE layer comprises a fluorinated thiophenol or a fluorinated alkanethiol compound.
28. The method of claim 15, wherein the ICE layer comprises a thiophenol or alkanethiol compound having one or more primary amine groups.
29. The method of claim 15, wherein the ICE layer comprises thiol ligands spatially arranged to densely bind adjacent Cd sites.
30. The method of claim 15, whereby a valence band offset from the p-type contact layer is reduced by the presence of the ICE layer.
31. The method of claim 15, whereby an energy level barrier height at an interface with the p-type contact layer is reduced by the presence of the ICE layer.
32. The method of claim 15, whereby hole carrier density in the p-type contact layer is increased by the presence of the ICE layer.
33. The method of claim 15, wherein the surface work function is increased by at most 450 meV in the presence of the ICE layer compared to a surface without the ICE layer, or decreased by at most 150 meV in the presence of the ICE layer compared to a surface without the ICE layer.
34. The device of claim 1, wherein the ICE layer has a thickness in a range of 0.2 nm to 5.0 nm.
35. A photovoltaic device, comprising: an absorber layer on the substrate stack, the absorber layer comprising cadmium; a p-type contact layer formed on a back interface at a second surface of the absorber layer; and an improved charge extraction (ICE) layer over the absorber layer, wherein: The ICE layer comprises a deprotonated thiol compound.
36. The device of claim 1 or 35, wherein the ICE layer is in contact with the back interface of the absorber layer.
37. The device of claim 35 or 36, wherein the ICE layer is above and in contact with the p-type contact layer.
38. The device of any one of claims 1 or 35-37, wherein the absorber layer comprises selenium.
39. The device of any one of claims 1 or 35-38, wherein the absorber layer is n-type.
40. The device of any one of claims 1 or 35-38, wherein the absorber layer comprises tellurium and wherein the ratio of Cd to Te in a surface region of the absorber layer is greater than or equal to 1:
1.
41. The device of claim 40, wherein the absorber layer comprises tellurium, and wherein the ratio of Cd to Te in a surface region of the absorber layer is in the range of 1:1 to 4:
1.
42. The device of any one of claims 1 or 35-41, wherein the thiol compound has a molecular dipole with a strength greater than 0.5 Debye.
43. A device according to any one of claims 1 or 35-42, wherein the surface work function of the ICE layer has a value amplitude in the range of 4.55eV to 5.15eV measured after deposition of the ICE layer; or the surface work function of the ICE layer has a value amplitude in the range of 4.6eV to 5.0eV measured after deposition of the HTM layer.
44. A device according to any one of claims 1 or 35-43, wherein the thiol compound comprises at least one of the following: isothiourea; cysteamine, also known as 2-aminoethanethiol (AET); 4-fluorothiophenol (4-FTP); 4-aminothiophenol (4-ATP); 1,2-ethanedithiol, also known as ethylenethiol (EDT); L-cysteine, also known as (R)-2-amino-3-mercaptopropionic acid (L-Cys); thioglycolic acid, also known as thioglycolic acid (TGA); 1-octanethiol (OT); 4-fluorobenzylthiol, also known as (4-fluorophenyl)methylthiol (4-FMB); 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluoro-1-octanethiol (TDF-OT); or 4-trifluoromethylbenzylthiol (4-TFMBM).
45. The device of any one of claims 1 or 35-44, wherein the thiol compound comprises at least one of: TDF-OT, 4-FTP, OT, AET, or 4-FMB.
46. The device of any one of claims 1 or 35-45, wherein the surface work function is increased by at most 450 meV in the presence of the ICE layer compared to a surface without the ICE layer, or is decreased by at most 150 meV in the presence of the ICE layer compared to a surface without the ICE layer.
47. The device of any of claims 1 or 35-46, wherein the back contact comprises at least one of: PTAA, poly-TPD, TFB, PF8-TAA, PIF8-TAA, NiOx, or P3HT.
48. The device of any one of claims 1, 35-38, or 41-45, wherein: The absorber layer comprises a II-VI type semiconductor, wherein the II type material comprises cadmium (Cd) and the VI type material comprises tellurium (Te); The absorber layer is doped with at least one dopant selected from phosphorus, arsenic, antimony or bismuth; The ICE layer is directly adjacent to the second surface of the absorber layer at a passivation surface region, wherein a ratio of Cd to Te in the surface region is greater than or equal to 1:1; The p-type contact layer is directly adjacent to the second surface of the ICE layer; The p-type contact layer comprises at least one of PTAA, P3HT, poly-TPD, TFB, TTF-1, PF8-TAA, PIF8-TAA, SGT-407, PCDTBT, SpiroOMeTAD, anthracene-based HTM, polythiophene, a semiconducting polymer, NiO, CuSCN, or CuI; and The device includes a conductive layer on the p-type contact layer.
49. The device of any one of claims 1 or 35-48, wherein a valence band offset from the p-type contact layer is reduced by the presence of the ICE layer.
50. The device according to any one of claims 1 or 35-49, wherein an energy level barrier height at an interface with the p-type contact layer is reduced by the presence of the ICE layer.
51. The device of any one of claims 1 or 35-50, wherein the hole carrier density in the p-type contact layer is increased by the presence of the ICE layer.
52. The device of any one of claims 1 or 35-51, wherein the ICE layer has a thickness in the range of 0.2 nm to 5.0 nm.
53. A method of manufacturing a photovoltaic device, the method comprising: providing an absorber stack having an absorber layer comprising cadmium (Cd); passivating a surface region of the absorber layer to form a passivated surface at a second surface of the absorber layer; forming an improved carrier extraction (ICE) layer over the second surface of the absorber layer, wherein: The ICE layer comprises a thiol compound, wherein the thiol compound comprises a thiophenol or an alkanethiol compound; and A p-type contact layer is formed on the absorber layer.
54. The method of claim 53, wherein the ICE layer contacts the second surface of the absorber layer.
55. The method of claim 53, wherein the step of passivating the surface region of the absorber layer precedes the step of forming the ICE layer.
56. The method of claim 53, wherein the step of passivating the surface region of the absorber layer occurs simultaneously with the step of forming the ICE layer.
57. The method of claim 15 or 53, wherein the absorber is n-type.
58. The method of claim 15 or 53, wherein the absorber is p-type.
59. The method of claim 53, wherein the p-type contact layer is formed over the ICE layer.
60. The method of claim 53, wherein the ICE layer is formed over the p-type contact layer.
61. The method of any one of claims 15, 53-55, or 57-60, wherein the passivating step comprises contacting the second surface of the absorber layer with an alkaline passivating agent.
62. The method of any one of claims 15, 53-56, or 58-61, wherein the absorber layer comprises tellurium and wherein the ratio of Cd to Te in the surface region of the absorber layer is greater than or equal to 1:
1.
63. The method of any one of claims 15 or 53-62, wherein the ICE layer comprises sulfur, and wherein the sulfur forms a complex with Cd at the passivated surface, and whereby the ICE layer produces a photoluminescence intensity enhancement of 2-10 times the photoluminescence intensity of a comparative device without the ICE layer.
64. The method of any one of claims 15 or 53-63, wherein the ICE layer comprises a compound selected from the group consisting of isothiourea; AET; 4-FTP; 4-ATP; EDT; L-Cys; TGA; OT; 4-FMB; TDF-OT; or 4-TFMBM.
65. The method of any of claims 15 or 53-64, wherein the step of depositing the p-type contact layer is performed at an absorber layer stack temperature at or below 150°C.
66. The method of any one of claims 15, 53-55, or 57-65, wherein the passivation step comprises: The surface of the absorption layer is contacted with an alkaline passivating agent, wherein the alkaline passivating agent comprises at least one of the following: sodium hydroxide (NaOH), potassium hydroxide (KOH) or tetramethylammonium hydroxide ((CH3)4N(OH))TMAH.
67. The method of any one of claims 15 or 53-66, wherein the p-type contact layer is deposited by slot die coating, knife coating, roller coating, spray coating, spin coating, sputtering, evaporation, or sol-gel formation.
68. A method according to any one of claims 15, 53-55 or 57-64, wherein providing the absorption layer stack includes forming the absorption layer on a substrate stack, wherein the absorption layer comprises a II-VI type semiconductor, and wherein forming the absorption layer also includes doping, passivation; and removing oxide from the II-VI type semiconductor before depositing the ICE layer.
69. The method of any one of claims 15 or 53-68, wherein the ICE layer comprises a monolayer of thiol ligands having a dipole moment aligned relative to the second surface of the absorber layer.
70. The method of any one of claims 15 or 53-69, wherein the ICE layer comprises a fluorinated thiophenol or fluorinated alkanethiol compound.
71. The method of any one of claims 15 or 53-70, wherein the ICE layer comprises a thiophenol or alkanethiol compound having one or more primary amine groups.
72. The method of any one of claims 15 or 53-71, wherein the ICE layer comprises deprotonated thiol ligands spatially arranged to densely bind adjacent Cd sites.
73. The method of any one of claims 15 or 53-72, whereby a valence band offset from the p-type contact layer is reduced by the presence of the ICE layer.
74. The method of any one of claims 15 or 53-73, whereby an energy level barrier height at an interface with the p-type contact layer is reduced by the presence of the ICE layer.
75. The method of any one of claims 15 or 53-74, whereby hole carrier density in the p-type contact layer is increased by the presence of the ICE layer.
76. The method of any one of claims 15 or 53-75, wherein the surface work function of the ICE layer on the absorber layer can be adjusted within a 600 meV range as measured by Kelvin probe surface work function by selecting a thiol compound.
77. The method of any one of claims 15 or 53-76, wherein the surface work function is increased by up to 450 meV in the presence of the ICE layer compared to a surface without the ICE layer, or the surface work function is decreased by up to 150 meV in the presence of the ICE layer compared to a surface without the ICE layer.
Citation Information
Cited By
Preparation method of vanadium-doped carbon composite back contact layer and application of vanadium-doped carbon composite back contact layer in preparation of cadmium telluride solar cell
CN122121318A
Preparation method of vanadium-doped carbon composite back contact layer and application thereof in preparation of cadmium telluride solar cell
CN122121318B
Photovoltaic devices with charge transport buffers and methods for forming the same
WO2026128644A1