Separator for electrochemical device and electrochemical device including the same

By using a porous coating of a porous polymer substrate with acrylic polymer binder, copolymer binder and inorganic particles on the partitions of the lithium secondary battery, the dimensional changes of lithium secondary battery under high temperature and humid conditions are solved. The problem of high rate achieves higher dimensional stability and electrode adhesion, extending the service life of the battery.

CN119096410APending Publication Date: 2024-12-06LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202480002299.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-01-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The separator of lithium secondary batteries has a large dimensional change rate under high temperature and humidity conditions, resulting in thermal shrinkage of the electrode and affecting the stability and life of the battery.

Method used

Using a porous polymer substrate, acrylic polymer binder, copolymer binder and inorganic particles, a porous coating is formed with high adhesion and Durable partition.

Benefits of technology

Under high temperature and humid conditions, the thermal shrinkage rate of the separator is significantly reduced, the dimensional stability of the battery and the adhesion of the electrodes are improved, and the service life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005099877880000201
    Figure BDA0005099877880000201
  • Figure BDA0005099877880000211
    Figure BDA0005099877880000211
  • Figure BDA0005099877880000212
    Figure BDA0005099877880000212
Patent Text Reader

Abstract

The present invention relates to a separator for an electrochemical device comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, in which the porous coating layer comprises an acrylic polymer binder, a copolymer binder, and inorganic particles, and the copolymer binder has a weight average molecular weight of 40,000 to 80,000, and the copolymer binder and the inorganic particles are contained in a weight ratio of 1: 93 to 1: 20.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application is based on and claims the benefit of priority from Korean Patent Application Nos. 10-2023-0035101 and 10-2023-0035102, both filed on March 17, 2023, in the Korean Intellectual Property Office, the disclosures of which are incorporated herein by reference in their entirety.

[0002] The present disclosure relates to a separator for an electrochemical device and an electrochemical device including the same. Background Art

[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions, and lithium secondary batteries have been widely used in recent years due to their high energy density and voltage, long cycle life, and versatility in various applications.

[0004] The lithium secondary battery may include an electrode assembly made of a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, and the electrode assembly and the electrolyte are contained in a housing together. The separator may include a porous coating layer containing a polymer binder and inorganic particles on at least one side of a porous substrate. The inorganic particles may be connected to other inorganic particles by a polymer binder to form an interstitial volume, and lithium ions may migrate through the interstitial volume. In addition to fixing the inorganic particles, the polymer binder may also provide adhesion to the porous coating layer, and the porous coating layer may be adhered to the porous substrate and the electrode, respectively.

[0005] Meanwhile, such a separator needs to maintain stability under high temperature and humidity conditions that may occur during the operation of the lithium secondary battery. Summary of the invention

[0006] Technical issues

[0007] The present disclosure provides a separator for an electrochemical device having a reduced dimensional change rate under a high-temperature and humid state, a method for manufacturing the same, and an electrochemical device including the separator.

[0008] Technical Solution

[0009] According to one aspect of the present disclosure, a separator for an electrochemical device includes a porous polymer substrate; and a porous coating formed on at least one surface of the porous polymer substrate. The porous coating contains an acrylic polymer binder, a copolymer binder, and inorganic particles, the copolymer binder has a weight average molecular weight of about 40,000 to 80,000, and the copolymer binder and the inorganic particles are contained in a weight ratio of about 1:93 to 1:20.

[0010] The acrylic polymer binder may include repeating units containing one or more monomers selected from the group consisting of: (meth)acrylic acid, (meth)acrylic acid ester, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, methyl n-Hexyl acrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate and tetradecyl (meth)acrylate.

[0011] The copolymer binder can be obtained by copolymerizing two or more selected from polyacrylic acid, polyacrylamide and polyvinyl alcohol.

[0012] The copolymer binder may be obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of about 8:2 to 5:5.

[0013] The acrylic polymer binder may be in the form of particles having an average particle size (D50) of about 100 nm to 500 nm, and the copolymer binder may be in a non-particulate shape.

[0014] The porous coating layer may include about 90 wt % to 95 wt % of the inorganic particles based on the total weight of the porous coating layer.

[0015] The content of the acrylic polymer binder may be greater than that of the copolymer binder based on the weight of the porous coating layer.

[0016] The acrylic polymer binder and the copolymer binder may be included in a weight ratio of about 5:1 to 1.5:1.

[0017] According to another aspect of the present disclosure, an electrochemical device includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is a separator for an electrochemical device different from that of the above one aspect.

[0018] The electrochemical device may be a lithium secondary battery.

[0019] The electrochemical device may further include an electrolyte including a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a weight ratio of about 3:7.

[0020] According to another aspect of the present disclosure, a method for manufacturing a separator for an electrochemical device includes forming a porous polymer substrate and a porous coating formed on at least one surface of the porous polymer substrate, wherein the porous coating comprises an acrylic polymer binder, a copolymer binder and inorganic particles, the copolymer binder having a weight average molecular weight of about 40,000 to 80,000, and the copolymer binder and the inorganic particles are contained in a weight ratio of about 1:93 to 1:20.

[0021] The acrylic polymer binder may include repeating units containing one or more monomers selected from the group consisting of: (meth)acrylic acid, (meth)acrylic acid ester, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, methyl n-Hexyl acrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate and tetradecyl (meth)acrylate.

[0022] The copolymer binder can be obtained by copolymerizing two or more selected from polyacrylic acid, polyacrylamide and polyvinyl alcohol.

[0023] The copolymer binder may be obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of about 8:2 to 5:5.

[0024] The acrylic polymer binder may be in the form of particles having an average particle size (D50) of about 100 nm to 500 nm, and the copolymer binder may be in a non-particulate shape.

[0025] The porous coating layer may include about 90 wt % to 95 wt % of the inorganic particles based on the total weight of the porous coating layer.

[0026] The content of the acrylic polymer binder may be greater than that of the copolymer binder based on the weight of the porous coating layer.

[0027] The acrylic polymer binder and the copolymer binder may be included in a weight ratio of about 5:1 to 1.5:1.

[0028] According to still another aspect of the present disclosure, a method of manufacturing an electrochemical device is provided, the electrochemical device including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator for an electrochemical device.

[0029] The electrochemical device may further include an electrolyte including a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a weight ratio of about 3:7.

[0030] Beneficial Effects

[0031] The separator for an electrochemical device according to the present disclosure can provide improved dimensional stability in a dry state and in a wet state impregnated with an electrolyte solution. For example, the separator can exhibit a dry state heat shrinkage of about 5% or less under high temperature conditions of 200° C. or more and a wet state heat shrinkage of about 5% or less under high temperature conditions of 130° C. or more, thereby preventing the electrode from being exposed due to thermal shrinkage of the separator. DETAILED DESCRIPTION

[0032] Hereinafter, with reference to the accompanying drawings, the embodiments of the present disclosure will be described in detail to facilitate the practice of those skilled in the art to which the present disclosure belongs. The present disclosure can be implemented in various forms and is not limited to or by the embodiments described below.

[0033] As used herein, the term "comprising" is used to list materials, compositions, devices and methods useful in the present disclosure and is not limited to the listed examples.

[0034] As used herein, the words "about," "approximately," and "substantially" are used to mean a range or approximation of values ​​or degrees that take into account inherent manufacturing and material tolerances, and are used to prevent an infringer from taking unfair advantage of the present disclosure where precise or absolute numbers are provided to aid in understanding the present disclosure.

[0035] As used herein, the term "electrochemical device" may refer to a primary battery, a secondary battery, or a supercapacitor.

[0036] As used herein, the word “wet” may refer to a state in which a separator is impregnated with at least a portion of an electrolyte, and the word “dry” may refer to a dry state in which a separator is not impregnated with an electrolyte.

[0037] As used herein, the term “durability” may mean the ability of a binder to exhibit adhesion or mechanical strength as an inherent property without swelling or deforming when in contact with an electrolyte.

[0038] The separator used in the lithium secondary battery can prevent the thermal shrinkage of the porous polymer substrate by applying a porous coating containing a polymer binder and inorganic particles to at least one surface of the porous substrate, and the separator including the porous coating generally exhibits good dimensional stability in a dry state without applying an electrolyte. However, in a wet state in which the separator is impregnated with an electrolyte, as the lithium secondary battery including the separator is operated, the adhesion of the polymer binder may deteriorate due to the swelling of the polymer binder by the electrolyte, or due to the separator being exposed to a temperature higher than, for example, about 130°C. Under these high temperature and humid conditions, the separator tends to shrink significantly due to the reduced adhesion of the porous coating. For example, a cylindrical battery in which the electrode assembly is wound and inserted into a housing and tension is applied to the electrode assembly requires less adhesion between the electrode and the separator than a pouch-type battery, and therefore, contains less polymer binder, resulting in further reduced dimensional stability in a wet state.

[0039] According to one embodiment, the present disclosure provides a separator that exhibits good dimensional stability under high temperature and humid conditions while maintaining a relatively low content of polymer binder in the porous coating.

[0040] A separator for an electrochemical device according to an embodiment of the present disclosure includes a porous polymer substrate and a porous coating formed on at least one surface of the porous polymer substrate. The porous coating contains an acrylic polymer binder, a copolymer binder, and inorganic particles, the copolymer binder has a weight average molecular weight of about 40,000 to 80,000, and the copolymer binder and the inorganic particles are contained in a weight ratio of about 1:93 to 1:20.

[0041] The porous polymer substrate can be a porous film having a plurality of pores that electrically insulates the positive and negative electrodes of the electrochemical device to prevent short circuits. For example, when the electrochemical device is a lithium secondary battery, the separator made of the porous polymer substrate can be an ion-conducting barrier that blocks electrical contact between the positive and negative electrodes while allowing lithium ions to pass through. At least some of the pores can form a three-dimensional network that is connected to the surface and interior of the porous polymer substrate, and a fluid can pass through the porous polymer substrate through the pores.

[0042] The porous polymer substrate can be a material that is physically and chemically stable to the electrolyte as an organic solvent. Examples of porous polymer substrates include resins, for example, polyolefins (such as polyethylene, polypropylene and polybutylene), polyvinyl chloride, polyethylene terephthalate, polycycloolefins, polyethersulfones, polyamides, polyimides, polyimide amides, nylons, polytetrafluoroethylene and copolymers or mixtures thereof, but are not limited thereto. For example, polyolefin-based resins can be used as porous polymer substrates. Polyolefin-based resins are suitable for manufacturing electrochemical devices with higher energy density because they can be processed into relatively small thicknesses and are relatively easy to apply coating slurries.

[0043] The porous polymer substrate may have a monolayer or multilayer structure. The porous polymer substrate may include two or more polymer resin layers with different melting points (Tm) to provide a shutdown capability during high temperature runaway of the battery. For example, the porous polymer substrate may include a polypropylene layer with a relatively high melting point and a polyethylene layer with a relatively low melting point. For example, the porous polymer substrate may have a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in this order. When the temperature of the battery rises to a temperature higher than a predetermined temperature, the polyethylene layer melts and closes the pores, thereby preventing thermal runaway of the battery.

[0044] The thickness of the porous polymer substrate may be about 1 μm or more and 100 μm or less. For example, the thickness of the porous polymer substrate may be about 10 μm or more and 90 μm or less, 20 μm or more and 80 μm or less, 30 μm or more and 70 μm or less, or 40 μm or more and 60 μm or less. For example, the thickness of the porous polymer substrate may be about 1 μm or more and 30 μm or less. Alternatively, the thickness of the porous polymer substrate may be about 5 μm or more and 15 μm or less, or about 8 μm or more and 13 μm or less. When the thickness of the porous polymer substrate is adjusted within the above range, for example, a separator is prepared using the porous polymer substrate as an electrical insulator for the positive and negative electrodes of an electrochemical device, while minimizing the volume of the electrochemical element, thereby increasing the amount of active material contained in the electrochemical device.

[0045] The porous polymer substrate may include pores having an average diameter of about 0.01 μm or more and 1 μm or less. For example, the diameter of the pores included in the porous polymer substrate may be about 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. Alternatively, the size of the pores may be about 0.02 μm or more and 0.06 μm or less. When the pore size of the porous polymer substrate is adjusted within the above range, the air permeability and ionic conductivity of the entire prepared separator may be controlled.

[0046] According to one embodiment, the air permeability of the porous polymer substrate can be about 10 seconds / 100cc or more and 100 seconds / 100cc or less. For example, the air permeability of the porous polymer substrate can be about 10 seconds / 100cc or more and 90 seconds / 100cc or less, 20 seconds / 100cc or more and 80 seconds / 100cc or less, 30 seconds / 100cc or more and 70 seconds / 100cc or less, or 40 seconds / 100cc or more and 60 seconds / 100cc or less. Alternatively, the air permeability of the porous polymer substrate can be about 50 seconds / 100cc or more and 70 seconds / 100cc or less. When the air permeability of the porous polymer substrate is within the above range, the air permeability of the prepared separator can be provided within the range suitable for ensuring the output characteristics and cycle characteristics of the electrochemical device.

[0047] Meanwhile, air permeability (seconds / 100cc) means the time (in seconds) that 100cc of air takes to pass through a porous polymer substrate or separator of a predetermined area at a constant pressure. Air permeability can be measured using a Gurley air permeability tester according to ASTM D 726-58, ASTM D726-94, or JIS-P8117. For example, the 4110N instrument from Gurley can be used to measure the air permeability of 100cc of air at an air pressure of 0.304 kPa or 1.215 kN / m 2 The water pressure passes through 1 square inch (or 6.54cm 2 For example, the ASAHI SEIKO EG01-55-1MR instrument can be used to measure the time it takes for 100 cc of air to pass through a 1 square inch sample at room temperature under a constant pressure of 4.8 inches of water.

[0048] The porosity of the porous polymer substrate can be about 10% by volume or more and 60% by volume or less. For example, the porosity of the porous polymer substrate can be about 15% by volume or more and 55% by volume or less, 20% by volume or more and 50% by volume or less, 25% by volume or more and 45% by volume or less, or 30% by volume or more and 40% by volume or less. Alternatively, the porosity of the porous polymer substrate can be about 30% by volume or more and 50% by volume or less. When the porosity of the porous polymer substrate is within the above range, the ionic conductivity of the prepared separator can be provided within a range suitable for ensuring the output characteristics and cycle characteristics of the electrochemical device.

[0049] Porosity refers to the ratio of the volume of pores to the total volume of the porous polymer substrate. Porosity can be measured by methods known in the art. For example, porosity can be measured by Brunauer Emmett Teller (BET) measurement using nitrogen adsorption, capillary flow porometer, or water or mercury permeation method.

[0050] The porous coating layer is formed on at least one surface of the porous polymer substrate and includes an acrylic polymer binder, a copolymer binder, and inorganic particles.

[0051] The porous coating layer can be formed by coating at least one surface of the porous polymer substrate with a coating slurry comprising an acrylic polymer binder, a copolymer binder, inorganic particles and a dispersion medium. For example, the separator can be prepared by applying the coating slurry on at least one surface of the porous polymer substrate and then drying to remove the dispersion medium. Since the inorganic particles contained in the porous coating layer are connected by the acrylic polymer binder and the copolymer binder to form a gap volume, the porous coating layer adheres to the porous polymer substrate while allowing lithium ions to pass through the gap volume, thereby preventing thermal shrinkage of the porous polymer substrate.

[0052] The coating slurry may include a dispersion medium to dissolve or disperse at least a portion of an acrylic polymer binder or a copolymer binder, and disperse inorganic particles. The coating slurry in which the polymer binder and inorganic particles are uniformly dispersed by controlling the type and content of the dispersion medium may be used. The example of a dispersion medium includes water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile (acetonitrile) and a combination thereof. According to one embodiment, the dispersion medium may be water. The above-mentioned type of dispersion medium may be used to form a porous coating in which inorganic particles are uniformly dispersed.

[0053] The viscosity of the coating slurry may be about 100 cps or more and 1,000 cps or less. For example, the viscosity of the coating slurry may be about 200 cps or more and 900 cps or less, 300 cps or more and 800 cps or less, 400 cps or more and 700 cps or less, or 500 cps or more and 600 cps or less. Alternatively, the viscosity of the coating slurry may be about 300 cps or more and 800 cps or less.

[0054] The coating slurry may also contain additives such as dispersants, surfactants, defoamers, flame retardants and wetting agents to improve dispersibility and flame retardancy and improve the uniformity of the porous coating formed. Examples of dispersants include one or more selected from oil-soluble polyamines, oil-soluble amine compounds, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, pyrogallic acid and polyacrylic acid. By using the above-mentioned types of dispersants, the stability of the coating slurry can be improved and the uniformity of the porous coating formed by the coating slurry can be ensured.

[0055] Based on the total weight of the coating slurry, the additive may be included in an amount of about 0 wt % or more and 5 wt % or less. For example, the content of the additive may be about 0.01 wt % or more and 4 wt % or less, 0.1 wt % or more and 3 wt % or less, or 1 wt % or more and 2 wt % or less. Alternatively, the content of the additive may be about 3 wt % or more and 5 wt % or less. When the content of the additive is adjusted within the above range, uniform dispersion and stability of the inorganic particles contained in the coating slurry may be achieved.

[0056] After forming the porous coating, the dispersion medium contained in the coating slurry can be removed by drying or heating. For example, the porous coating can contain about 5ppm or less dispersion medium. According to one embodiment, the porous coating can be composed of an acrylic polymer binder, a copolymer binder and inorganic particles. In the process of removing the dispersion medium, a plurality of holes can be formed on the surface and inside of the porous coating. The hole can include a gap volume formed between the inorganic particles, and can have a structure in which a three-dimensional network is formed to allow a fluid to pass through.

[0057] The thickness of the porous coating layer may be about 1 μm or more and 15 μm or less. For example, the thickness of the porous coating layer may be about 2 μm or more and 14 μm or less, 3 μm or more and 13 μm or less, 4 μm or more and 12 μm or less, 5 μm or more and 11 μm or less, 6 μm or more and 10 μm or less, or 7 μm or more and 9 μm or less. Alternatively, the thickness of the porous coating layer may be about 1 μm or more and 5 μm or less. When the thickness of the porous coating layer is adjusted within the above range, the shrinkage of the porous polymer substrate may be minimized and stable adhesion to the porous polymer substrate may be achieved.

[0058] The acrylic polymer binder can bind the inorganic particles contained in the porous coating layer and provide adhesion to the porous coating layer. For example, the acrylic polymer binder can include repeating units containing one or more monomers selected from the following: (meth)acrylic acid, (meth)acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-Hexyl methacrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate and tetradecyl (meth)acrylate.

[0059] For example, the acrylic polymer binder may include one or more selected from the following: polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber and acrylonitrile-butadiene-styrene rubber.

[0060] The acrylic polymer binder can be in the form of particles. For example, the acrylic polymer binder can have particles of spherical shape or elliptical shape, but is not limited thereto. The average particle diameter (D50) of the acrylic polymer binder can be about 100nm or more and 500nm or less. For example, the average particle diameter (D50) of the acrylic polymer binder can be about 150nm or more and 450nm or less, 200nm or more and 400nm or less, or 250nm or more and 350nm or less. Alternatively, the average particle diameter (D50) of the acrylic polymer binder can be about 250nm or more and 400nm or less. When the particle size of the acrylic polymer binder particles is adjusted within the above range, the migration path of lithium ions and the adhesion of the porous coating to the porous polymer substrate can be ensured at the same time.

[0061] Acrylic polymer binders can help to exhibit dry adhesion (which is the adhesion of the porous coating in a dry state), and copolymer binders can help to exhibit wet adhesion (which is the adhesion of the porous coating in a wet state). Compared with acrylic-based polymer binders, copolymer binders can be physically or chemically stable in electrolytes, and adhesion may not decrease even in a wet state, so that the adhesion of the porous coating to the porous polymer substrate is maintained in a wet state, thereby reducing thermal shrinkage of the porous polymer substrate.

[0062] The copolymer binder can be obtained by copolymerizing two or more selected from polyacrylic acid (PAA), polyacrylamide (PAM) and polyvinyl alcohol (PVA). For example, the copolymer binder can be obtained by randomly copolymerizing two or more selected from polyacrylic acid, polyacrylamide and polyvinyl alcohol.

[0063] According to one embodiment, the copolymer binder may be a copolymer of polyacrylic acid and polyacrylamide. In the copolymer binder, polyacrylic acid may form bonds between inorganic particles while exhibiting durability to electrolytes. Polyacrylamide exhibits a higher modulus value than polyacrylic acid, which further improves the durability of the copolymer binder to electrolytes, thereby maintaining the shape of the copolymer binder even in electrolytes.

[0064] In the case where the copolymer binder is a copolymer of polyacrylic acid and polyacrylamide, the copolymer binder can be obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of about 8:2 to 5:5. For example, the copolymer binder can be obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of about 8:2, 7:3, 6:4, or 5:5. Alternatively, the copolymer binder can be obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of about 7:3 to 5:5. By copolymerizing polyacrylic acid and polyacrylamide at the above ratio, the interstitial volume can be ensured by the combination of the inorganic particles contained in the porous coating and the durability to the electrolyte can be ensured.

[0065] Meanwhile, the copolymer binder may be in a non-granular shape. The non-granular shape may include irregular shapes other than spherical or elliptical shapes. The non-granular copolymer binder forms bonds between inorganic particles and between inorganic particles and acrylic polymer particles, thereby providing adhesion to the porous coating.

[0066] In addition, the weight average molecular weight (Mw) of the copolymer binder can be about 40,000 or more and 80,000 or less. For example, the weight average molecular weight of the copolymer binder can be about 45,000 or more and 75,000 or less, 50,000 or more and 70,000 or less, or 55,000 or more and 65,000 or less. Alternatively, the weight average molecular weight of the copolymer binder can be about 60,000 or more and 70,000 or less. When the weight average molecular weight of the copolymer binder is adjusted within the above range so that the viscosity of the coating slurry does not exceed 1000cps, the structural modification of the copolymer binder by the electrolyte can be prevented, thereby reducing the wet state heat shrinkage of the separator.

[0067] The weight average molecular weight of copolymer binder can be measured by gel permeation chromatography (gel permeation chromatography, GPC) (PL GPC220, Agilent Technologies).For example, weight average molecular weight can be determined by following: in PL Olexis (Polymer Laboratories) column (column temperature: 160 ℃), trichlorobenzene (TCB) is used as solvent, and under the condition of sample concentration of 1.0 mg / mL, flow rate of 1.0 mL / min and injection volume of 200 μ l, Agilent high temperature RI detector is used (adopting cubic function correction, reference: polystyrene).

[0068] The copolymer binder and the inorganic particles may be included in a weight ratio of about 1:93 to 1:20. For example, the weight ratio of the copolymer binder to the inorganic particles may be about 1:93, 1:92, 1:91, 1:90, 1:85, 1:80, 1:75, 1:70, 1:65, 1:60, 1:55, 1:50, 1:45, 1:40, 1:35, 1:30, 1:25, or 1:20. Alternatively, the weight ratio of the copolymer binder to the inorganic particles may be about 1:93 to 1:46. As a separator suitable for cylindrical batteries within the above range, a separator having reduced thermal shrinkage by maintaining adhesion in a humid state may be manufactured.

[0069] Based on the weight of the porous coating layer, the content of the acrylic polymer binder may be greater than the content of the copolymer binder. The acrylic polymer binder and the copolymer binder may be included in a weight ratio of about 5:1 to 1.5:1. For example, the weight ratio of the acrylic polymer binder to the copolymer binder may be about 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, or 1.5:1. When the content of the binder is adjusted within the above range, a separator suitable for a cylindrical battery having a reduced dry state thermal shrinkage and a wet state thermal shrinkage can be manufactured.

[0070] The inorganic particles can be electrochemically stable. There are no particular limitations on the inorganic particles, as long as no oxidation and / or reduction reactions occur within the operating voltage range of the electrochemical device (e.g., 0 V to 5 V based on Li / Li + . For example, using inorganic particles with a high dielectric constant can help increase the dissociation of electrolyte salts (such as lithium salts) in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte. For the above reasons, the inorganic particles can include high dielectric constant inorganic particles with a dielectric constant of about 5 or greater, such as about 10 or greater. Non-limiting examples of inorganic particles with a dielectric constant of about 5 or greater include BaTiO 3 , Pb(Zr,Ti)O 3 (PZT), Pb 1-x La x Zr 1-y Ti y O 3 (PLZT, 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O 3 -PbTiO 3 (PMN-PT), hafnium dioxide (HfO 2 ), SrTiO 3 , SnO 2 , CeO 2 , MgO, NiO, CaO, ZnO, ZrO 2 , SiO 2 , Y 2 O 3 , Al 2 O 3 , Al(OH) 3 , SiC, AlOOH, TiO 2 and mixtures thereof.

[0071] In addition, inorganic particles with lithium ion transport ability (i.e., inorganic particles containing the element lithium but not storing lithium and having the ability to transport lithium ions) can be used as inorganic particles. Non-limiting examples of inorganic particles with lithium ion transport ability include lithium phosphate (Li 3 PO 4 ), lithium titanium phosphate (Li x Ti y (PO 4 ) 3 , 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO 4 ) 3, (where \(0 \lt x \lt 2\), \(0 \lt y \lt 1\), \(0 \lt z \lt 3\)), \((LiAlTiP)\) x O y series of glasses (\(0 \lt x \lt 4\), \(0 \lt y \lt 13\)) such as 14Li 2 O - 9Al 2 O 3 - 38TiO 2 - 39P 2 O 5 、lithium lanthanum titanate (\(Li\) x La y TiO 3 , where \(0 \lt x \lt 2\), \(0 \lt y \lt 3\)), lithium germanium thiophosphate (\(Li\) x Ge y P z S w , where \(0 \lt x \lt 4\), \(0 \lt y \lt 1\), \(0 \lt z \lt 1\), \(0 \lt w \lt 5\)) such as \(Li\) 3.25 Ge 0.25 P 0.75 S 4 、lithium nitride (\(Li\) x N y , where \(0 \lt x \lt 4\), \(0 \lt y \lt 2\)) such as \(Li\) 3 N, \(SiS\) 2 series of glasses (\(Li\) x Si y S z , where \(0 \lt x \lt 3\), \(0 \lt y \lt 2\), \(0 \lt z \lt 4\)) such as \(Li\) 3 PO 4 - Li 2 S - \(SiS\) 2 and \(P\) 2 S 5 series of glasses (\(Li\) x P y S z , where \(0 \lt x \lt 3\), \(0 \lt y \lt 3\), \(0 \lt z \lt 7\)) such as \(LiI - Li\) 2 S - \(P\) 2 S 5 、or a mixture of two or more of them.

[0072] In addition, inorganic particles with flame retardancy can be used to impart flame retardant properties to the separator or to prevent a rapid increase in temperature inside the electrochemical element. Non - limiting examples of inorganic particles with flame retardancy include \(Sb\) 2 O 3 、\(Sb\) 2 O 4 、\(Sb\) 2 O 5 、\(SrTiO\) 3 、\(SnO\) 2 、\(CeO\)2 、MgO、Mg(OH) 2 、NiO、CaO、ZnO、Zn 2 SnO 4 、ZnSnO 3 、ZnSn(OH) 6 、ZrO 2 , Y 2 O 3 、SiO 2 、Al 2 O 3 、AlOOH、Al(OH) 3 、SiC、TiO 2 , H 3 BO 3 , HBO 2 and mixtures thereof.

[0073] The average particle size (D50) of the inorganic particles can be about 50nm or more and 5,000nm or less. For example, the average particle size (D50) of the inorganic particles can be about 100nm or more and 4,500nm or less, 200nm or more and 4,000nm or less, 300nm or more and 3,000nm or less, 400nm or more and 2,000nm or less, or 500nm or more and 1,000nm or less. When the average particle size of the inorganic particles is less than about 50nm, due to the increase in specific surface area, additional polymer binders are required for bonding between the inorganic particles, which is disadvantageous in terms of resistance. When the average particle size of the inorganic particles exceeds 5,000nm, the surface uniformity of the coating may be reduced, and damage to the porous polymer substrate or electrode may occur during lamination.

[0074] In addition, the aspect ratio of the inorganic particles can be about 1 or more and 2 or less. For example, the aspect ratio of the inorganic particles can be about 1.1 or more and 1.9 or less, 1.2 or more and 1.8 or less, 1.3 or more and 1.7 or less, or 1.4 or more and 1.6 or less. When the aspect ratio of the inorganic particles is adjusted within the above range, a porous coating can be formed: the porous coating promotes the migration of the polymer binder through the pores between the inorganic particles, and ultimately includes a gap volume that allows lithium ions to migrate.

[0075] The BET (Brunauer-Emmett-Teller) specific surface area of ​​the inorganic particles can be about 5 m 2 / g or more and 25m 2 / g or less. For example, the BET specific surface area of ​​the inorganic particles can be about 6m 2 / g or more and 24m 2 / g or less, 7m2 / g or more and 23m 2 / g or less, 8m 2 / g or more and 22m 2 / g or less, 9m 2 / g or more and 21m 2 / g or less, 10m 2 / g or more and 20m 2 / g or less, 11m 2 / g or more and 19m 2 / g or less, 12m 2 / g or more and 18m 2 / g or less, 13m 2 / g or more and 17m 2 / g or less, or 14m 2 / g or more and 26m 2 When the BET specific surface area of ​​the inorganic particles is adjusted within the above range, migration of the polymer binder through pores between the inorganic particles can be controlled.

[0076] Based on the total weight of the porous coating, the porous coating may include about 90% to 95% by weight of inorganic particles. For example, the porous coating may include about 90% by weight or more and 95% by weight or less, 91% by weight or more and 92% by weight or less, or 93% by weight or more and 94% by weight or less of inorganic particles. Alternatively, the porous coating may include about 92% by weight or more and 94% by weight or less of inorganic particles. When the content of the inorganic particles is adjusted within the above range, a separator having mechanical strength and thermal properties suitable for a cylindrical battery can be manufactured.

[0077] In the separator, the loading amount of the porous coating layer relative to the area of ​​the porous polymer substrate may be about 1.0 g / m 2 or larger and 6.0g / m 2 For example, the loading amount of the porous coating can be about 1.5 g / m 2 or larger and 5.5g / m 2 or less, 2.0g / m 2 or larger and 5.0g / m 2 or less, 2.5g / m 2 or larger and 4.5g / m 2 or less, or 3.0g / m 2 or larger and 4.0g / m 2 According to one embodiment, the loading amount of the porous coating layer may be about 5.5 g / m 2 or larger and 6.0g / m 2When the loading amount of the porous coating layer is adjusted within the above range, the durability of the separator to the electrolyte can be ensured.

[0078] The air permeability of the separator for the electrochemical device can be about 50 seconds / 100cc or more and 150 seconds / 100cc or less. For example, the air permeability of the separator can be about 60 seconds / 100cc or more and 140 seconds / 100cc or less, 70 seconds / 100cc or more and 130 seconds / 100cc or less, 80 seconds / 100cc or more and 120 seconds / 100cc or less, or 90 seconds / 100cc or more and 110 seconds / 100cc or less. According to one embodiment, the air permeability of the separator can be 100 seconds / 100cc or more and 120 seconds / 100cc or less. When the air permeability of the separator is within the above range, the output characteristics, stability characteristics and cycle characteristics of the electrochemical device can be ensured.

[0079] At the same time, the thermal shrinkage of the separator for the electrochemical device may be about 10% or less. For example, the dry state thermal shrinkage of the separator may be about 5% or less, and the wet state thermal shrinkage may be about 10% or less. According to one embodiment, the dry state thermal shrinkage of the separator may be a dimensional change rate based on exposure to 200°C for 30 minutes, and the wet state thermal shrinkage may be a dimensional change rate based on exposure to 135°C for 30 minutes when the separator is immersed in an electrolyte. According to one embodiment, the dry state thermal shrinkage may be about 5% or less, and the wet state thermal shrinkage may be about 5% or less.

[0080] When a secondary battery cell is manufactured using a separator for an electrochemical device, the resistance of the secondary battery cell may be about 0.5 ohms or more and 1.5 ohms or less. For example, the resistance of the secondary battery cell may be about 0.6 ohms or more and 1.4 ohms or less, 0.7 ohms or more and 1.3 ohms or less, 0.8 ohms or more and 1.2 ohms or less, or 0.9 ohms or more and 1.1 ohms or less. According to one embodiment, the resistance of the secondary battery cell may be about 0.6 ohms or more and 0.8 ohms or less.

[0081] According to another embodiment of the present disclosure, the electrochemical device includes a positive electrode, a negative electrode and a separator inserted between the positive electrode and the negative electrode, wherein the separator is a separator for the electrochemical device of the above embodiment. The electrochemical device can be manufactured by inserting an electrode assembly including a positive electrode, a negative electrode and a separator inserted between the positive electrode and the negative electrode into a housing or a bag and sealing the housing or the bag. Before sealing the housing or the bag, the electrode assembly can be impregnated with an electrolyte by injecting an electrolyte. The shape of the housing or the bag is not limited. For example, the electrochemical device can be a lithium secondary battery in the shape of a cylinder, a prismatic, a coin, or a bag.

[0082] The positive electrode and the negative electrode can be coated by applying an electrode active material on at least one surface of each current collector and drying. The current collector can be a material that has conductivity without causing chemical changes in the electrochemical device. Examples of current collectors for the positive electrode include aluminum; nickel; titanium; fired carbon and stainless steel; and aluminum or stainless steel subjected to surface treatment with carbon, nickel, titanium or silver, but are not limited thereto. Examples of current collectors for the negative electrode include copper; nickel; titanium; fired carbon and stainless steel; and copper or stainless steel subjected to surface treatment with carbon, nickel, titanium or silver, but are not limited thereto. The current collector can be in various forms, such as a thin metal plate, a film, a foil, a mesh, a porous material, or a foam.

[0083] The positive electrode includes a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material, a conductive material and a binder resin on at least one surface of the current collector. The positive electrode active material includes a layered compound, such as a lithium manganese composite oxide (e.g., LiMn 2 O 4 and LiMnO 2 ), lithium cobalt oxide (LiCoO 2 ) and lithium nickel oxide (LiNiO 2 ), or a compound substituted by one or more transition metal elements; 1+x Mn 2-x O 4 (wherein x is 0 to 0.33) represented by lithium manganese oxide, LiMnO 3 、LiMn 2 O 3 or LiMnO 2 ; Lithium copper oxide (Li 2 CuO 2 ); Vanadium oxides such as LiV 3 O 8 , LiV 3 O 4 、V 2 O 5 , Cu 2 V 2 O 7 ; LiNi1-x M x O 2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x = 0.01 to 0.3) represents Ni-site type lithium nickel oxide; LiMn represented by the formula 1-x M x O 2 (where M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li 2 Mn 3 MO 8 (where M = Fe, Co, Ni, Cu or Zn) represents lithium manganese composite oxide; LiMn 2 O 4 , in which some Li in the formula is replaced by alkaline earth metal ions; disulfide compounds; Fe 2 (MoO 4 ) 3 , which can be used alone or in a mixture of two or more of them.

[0084] The negative electrode includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode active material in the negative electrode includes carbon, such as lithium metal oxide, hard carbon, and graphite carbon; silicon-based materials, such as Li x Fe 2 O 3 (0 ≤ x ≤ 1), Li x WO 2 (0 ≤ x ≤ 1), Si, SiO x (0 < x < 2), SiC, and Si alloys; metal composite oxides, such as Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Groups 1, 2, and 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloys; tin-based alloys; metal oxides, such as SnO, SnO 2 , PbO, PbO 2 , Pb 2 O 3 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 , GeO, GeO 2 , Bi2 O 3 、Bi 2 O 4 and Bi 2 O 5 ; a conductive polymer such as polyacetylene; a Li-Co-Ni based material; and a titanium oxide, which may be used alone or as a mixture of two or more thereof.

[0085] The conductive material may be any one or a mixture of two or more of the following conductive materials: graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, carbon nanotube, activated carbon and polyphenylene derivative. Carbon nanotubes include nano-sized diameters and sp 2 The conductive material is a graphite sheet with a cylindrical shape and a bond structure, and exhibits conductor properties or semiconductor properties according to the angle and structure of the graphite sheet winding. Based on the number of bonds constituting the wall of the carbon nanotube, the carbon nanotube can be classified into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT) and multi-walled carbon nanotubes (MWCNT), and the carbon nanotube can be appropriately selected based on the application of the dispersion. For example, the conductive material can be one selected from the following: natural graphite, artificial graphite, super-p, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate and titanium oxide, or a mixture of two or more thereof.

[0086] The binder resin that can be used herein can be any binder resin commonly used for the electrode of electrochemical device. Non-limiting examples of binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, poly(methyl methacrylate), poly(ethylhexyl acrylate), poly(butyl acrylate), polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan and carboxymethyl cellulose, but are not limited thereto.

[0087] The electrolyte can be prepared by placing a + B - A salt of the structure of is obtained by dissolving or dissociating in an organic solvent such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone, or a mixture thereof, wherein A +Including alkali metal cations such as Li + 、Na + , or K + , or a combination thereof, and B - Including anions such as PF 6 - , BF 4 - , Cl - Br - ,I - , ClO 4 - , AsF 6 - , CH 3 CO 2 - CF 3 SO 3 - 、N(CF 3 SO 2 ) 2 - , or C(CF 2 SO 2 ) 3 - , or a combination thereof.

[0088] For example, the electrolyte may include a solvent having a weight ratio of EC / EMC of about 3 / 7, and the dimensional stability of the separator according to this embodiment may be maximized.

[0089] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including a unit cell, a battery pack including a battery module, and a device including a battery pack as a power source. Examples of the device include small devices such as computers, mobile phones, and power tools; electric vehicles driven by electric motors, including electric vehicles (EV), hybrid electric vehicles (HEV), and plug-in hybrid electric vehicles (PHEV); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and medium to large devices such as power storage systems, but not limited thereto.

[0090] Another embodiment of the present disclosure provides a method for preparing a separator for an electrochemical device, comprising forming a porous coating layer comprising an acrylic polymer binder, a copolymer binder and inorganic particles on at least one surface of a porous polymer substrate. The contents overlapping with those described in the separator for an electrochemical device are replaced with the description of the aforementioned embodiment.

[0091] The step of forming the porous coating layer may include preparing a coating slurry including an acrylic polymer binder, a copolymer binder, inorganic particles, and a dispersion medium, and applying the coating slurry to the porous polymer substrate, followed by drying.

[0092] The step of forming a porous coating layer may further include performing a corona discharge treatment on at least one surface of the porous polymer substrate before applying the coating slurry to at least one surface of the porous polymer substrate. The step of performing a corona discharge treatment on at least one surface of the porous polymer substrate may prevent the adhesion between the surface of the porous polymer substrate and the surface of the coating layer from being reduced at a high temperature higher than a predetermined temperature, and prevent the adhesion between the surface of the porous polymer substrate and the surface of the porous coating layer from being reduced due to the electrolyte.

[0093] Corona discharge treatment can be carried out in air at a voltage of about 0.1kV or more and 10kV or less on at least one surface of porous polymer substrate. For example, corona discharge treatment can be carried out at the following voltage: about 0.2kV or more and 9kV or less, 0.3kV or more and 8kV or less, 0.4kV or more and 7kV or less, 0.5kV or more and 6kV or less, 0.6kV or more and 5kV or less, 0.7kV or more and 4kV or less, 0.8kV or more and 3kV or less, 0.9kV or more and 2kV or less, or 1.0kV or more and 2kV or less. According to one embodiment, corona discharge treatment can be carried out in air at a voltage of about 1.8kV. When the applied voltage of corona discharge treatment is adjusted within the above range, a suitable number of functional groups can be formed on the surface of polymer substrate, and the damage to the surface of polymer substrate can be prevented.

[0094] The step of forming the porous coating may include applying the coating slurry to the porous polymer substrate to form the coating. For example, the coating may be formed by, but not limited to, a rod coater, a wire rod coater, a roller coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a blade coater, a slot die coater, a hot melt coater, a comma coater, and a direct metering coater. According to one embodiment, the step of forming the porous coating may include using a rod coater or a slot die coater to simultaneously coat two surfaces of the porous polymer substrate with the coating slurry.

[0095] The step of forming the porous coating layer may include applying the coating slurry to the porous polymer substrate, followed by drying or heating the porous coating layer to evaporate the dispersion medium contained in the porous coating layer. The removal of the dispersion medium may be performed at a temperature that can evaporate only the dispersion medium contained in the porous coating layer without modifying the polymer binder contained in the porous coating layer. For example, the removal of the dispersion medium may be achieved by heating the porous coating layer to a predetermined temperature, but ensuring that the temperature of the surface of the porous coating layer does not exceed 60°C. When the porous coating layer is heated under the above conditions, the thermal energy may be first used to heat the dispersion medium and change the phase, but cannot be used to modify the polymer binder.

[0096] Hereinafter, the present disclosure will be described in more detail with reference to embodiments and experimental examples. The following embodiments and experimental examples are only used to illustrate the present disclosure, and the present disclosure is not limited to the following embodiments and experimental examples.

[0097] Example 1

[0098] Preparation of coating slurry

[0099] 2.77 g (solid content 11.4%) of a copolymer (weight average molecular weight: 70,000, pH 7.2, viscosity 55 cps@RT) as a copolymer binder (obtained by polymerizing polyacrylic acid and polyacrylamide at a ratio of 5:5) and 30 g of Al as inorganic particles were added at room temperature (25°C). 2 O 3 (particle size (D50): 500 nm) and 3.1 g (solid content 25%) of a PAA-based polymer dispersant as an additive were introduced into 53.7 mL of distilled water and stirred with an oscillator for 120 minutes, and then 2.42 g (solid content 40%) of an acrylic polymer binder (particle size (D50): 150 nm, Tg: -25°C) and 0.19 g (solid content 100%) of a wetting agent as an additive were added thereto to prepare a coating slurry in which the copolymer binder and inorganic particles were dispersed.

[0100] Preparation of porous polymer substrates

[0101] As the porous polymer substrate, a polyethylene film (MI: 0.2 g / 10 min, T m : 135°C, porosity: 45%, average pore size: 35nm).

[0102] Preparation of separators

[0103] The coating slurry was coated on both surfaces of the polyethylene film using a bar coater to form a coating layer having a thickness of 1.5 μm.

[0104] The process of applying a low-temperature air volume to the polyethylene film having a coating formed thereon and removing the dispersion medium was repeated five times to prepare a separator having a total thickness of 13 μm and comprising an acrylic polymer binder, a copolymer binder, additives and inorganic particles contained in the porous coating layer in a weight ratio of 3:1:3:93.

[0105] Although the order of the manufacturing method of the separator of the present disclosure has been described, the order of the manufacturing method is not limited thereto and can be appropriately modified and adjusted as needed. For example, the preparation of the porous substrate can be performed before the preparation of the coating slurry, or the two preparations can be performed simultaneously.

[0106] Example 2

[0107] A separator was prepared in the same manner as in Example 1, except that a copolymer binder having a weight average molecular weight of 67,000 was used in preparing the coating slurry.

[0108] Example 3

[0109] A separator was prepared in the same manner as in Example 1 (the weight ratio of the acrylic polymer binder, copolymer binder, additives and inorganic particles contained in the porous coating layer was 3:2:3:92), except that 2.45 g of acrylic polymer binder, 5.6 g of copolymer binder, 30 g of inorganic particles, 3.13 g of dispersant and 0.2 g of wetting agent were contained in the coating slurry.

[0110] Example 4

[0111] A separator was prepared in the same manner as in Example 1, except that a copolymer binder obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of 7:3 was used in preparing the coating slurry.

[0112] Comparative Example 1

[0113] A separator was prepared in the same manner as in Example 1, except that a copolymer binder having a weight average molecular weight of 35,000 was used in preparing the coating slurry.

[0114] Comparative Example 2

[0115] A separator was prepared in the same manner as in Example 1, except that a copolymer binder having a weight average molecular weight of 100,000 was used in preparing the coating slurry.

[0116] Comparative Example 3

[0117] A separator was prepared in the same manner as in Example 1, except that a copolymer binder having a weight average molecular weight of 160,000 was used in preparing the coating slurry.

[0118] Comparative Example 4

[0119] A separator was prepared in the same manner as in Example 1 (the weight ratio of the acrylic polymer binder, copolymer binder, additives and inorganic particles contained in the porous coating layer was 3:0:3:94), except that 2.39 g of acrylic polymer binder and 30 g of inorganic particles were included in the preparation of the coating slurry, but the copolymer binder was not used.

[0120] Comparative Example 5

[0121] A separator was prepared in the same manner as in Example 1 (the weight ratio of acrylic polymer binder, copolymer binder, additives and inorganic particles was 3:5:3:89), except that 2.53 g of acrylic polymer binder, 14.48 g of copolymer binder and 30 g of inorganic particles were included in the preparation of the coating slurry.

[0122] Comparative Example 6

[0123] A separator was prepared in the same manner as in Example 1 (the weight ratio of acrylic polymer binder, copolymer binder, additives and inorganic particles was 3:10:3:84), except that 2.68 g of acrylic polymer binder, 30.68 g of copolymer binder and 30 g of inorganic particles were included in the preparation of the coating slurry.

[0124] Comparative Example 7

[0125] A separator was prepared in the same manner as in Example 1, except that only polyacrylic acid was used instead of the copolymer binder when preparing the coating slurry.

[0126] Comparative Example 8

[0127] A separator was prepared in the same manner as in Example 1, except that a copolymer binder obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of 3:7 was used in preparing the coating slurry.

[0128] Comparative Example 9

[0129] A separator was prepared in the same manner as in Example 1, except that only polyacrylamide was used instead of the copolymer binder when preparing the coating slurry.

[0130] Experimental Example 1. Determination of the characteristics of the separator according to the characteristics of the coating slurry

[0131] Conditions of separators prepared according to Example 1 and Comparative Examples 1 to 3, and characteristics of the separators according to molecular weight as a characteristic of the copolymer binder used were determined and are shown in Table 1 below.

[0132] In Comparative Examples 2 and 3, the viscosity of the coating slurry exceeded 1,000 cps, and thus, coating using a bar coater could not be performed. Hereinafter, characteristics of the separators prepared according to Example 1 and Comparative Example 1 were determined.

[0133] Air permeability measurement

[0134] The air permeability was measured using a Gurley densometer (Gurley, 4110N) to determine the air permeability of 100 cc of air through a 28.6 mm diameter and 645 mm area. 2 The time taken for the separators to be

[0135] Determination of improvement in heat shrinkage in dry state

[0136] The separators of the examples and comparative examples were each prepared into a sample having a size of 5 cm×5 cm. After the prepared samples were stored in a convection oven at 200° C. for 30 minutes, the heat shrinkage in the machine direction (MD) and the heat shrinkage in the transverse direction (TD) were calculated according to [(length of the initial sample−length after storage at 200° C. for 0.5 hours) / (length of the initial sample)]×100(%).

[0137] Determination of improvement in heat shrinkage in wet conditions

[0138] The separators of Examples and Comparative Examples were prepared into samples having a size of 5 cm×5 cm, and put into an aluminum bag having a size of 7 cm×10 cm in size. The bag was filled with 1 g of electrolyte, and the bag was sealed.

[0139] The electrolyte contained 3 mol of vinylene carbonate (VC), 1.5 mol of propane sultone (PS), 1 mol of ethylene sulfate (ESa), and 1 mol of lithium salt LiPF as additives in a solvent mixed with ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a weight ratio of 3 / 7. 6 .

[0140] After the sealed bag was stored in a hot box at 135°C for 30 minutes, the heat shrinkage in the machine direction (MD) and the heat shrinkage in the transverse direction (TD) were calculated according to [(length of the initial sample - length after storage at 135°C for 0.5 hours) / (length of the initial sample)]×100(%).

[0141] Determination of EL wettability of electrolytes

[0142] The separators of the examples and comparative examples were prepared as 5 cm×5 cm specimens, and 2 μl of propylene carbonate (PC) was dropped on the separator surface as an electrolyte. After 5 minutes, the lengths of spread in the MD direction and the TD direction were measured based on the droplet boundary immediately after the electrolyte was dropped on the separator surface.

[0143] [Table 1]

[0144]

[0145] Experimental Example 2. Determination of the characteristics of the separator according to the content of the copolymer binder

[0146] Conditions of separators prepared according to Examples 2 and 3 and Comparative Examples 4 to 6 were determined, and characteristics of the separators according to the content of the copolymer binder used were determined and shown in Table 2 below.

[0147] In Comparative Examples 5 and 6, the viscosity of the coating slurry exceeded 1,000 cps, and therefore, coating using a bar coater could not be performed. Hereinafter, the properties of the separators prepared according to Examples 2 and 3 and Comparative Example 4 were determined. The method for determining each property was the same as in the previous experimental example.

[0148] [Table 2]

[0149]

[0150] Experimental Example 3. Determination of separator characteristics according to copolymerization ratio of copolymer binder

[0151] Conditions of separators prepared according to Examples 1 and 4 and Comparative Examples 7 to 9 were determined, and properties of separators according to copolymerization ratios of the copolymer binders used were determined and shown in the following Table 3. The method for determining each property was the same as in the previous experimental example.

[0152] [Table 3]

[0153]

[0154] From the foregoing, it will be understood that various embodiments of the present disclosure are described herein for illustrative purposes, and that various modifications may be made without departing from the scope and spirit of the present disclosure. Therefore, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims.

Claims

1. A separator for an electrochemical device, comprising: a porous polymer substrate; as well as forming a porous coating layer on at least one surface of the porous polymer substrate, wherein the porous coating layer comprises an acrylic polymer binder, a copolymer binder and inorganic particles, The copolymer binder has a weight average molecular weight of 40,000 to 80,000, and The copolymer binder and the inorganic particles are included in a weight ratio of 1:93 to 1:

20.

2. The separator according to claim 1, wherein the acrylic polymer binder comprises repeating units comprising one or more monomers selected from the group consisting of: (meth)acrylic acid, (meth)acrylic acid ester, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, methyl Isoamyl acrylate, n-hexyl methacrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate and tetradecyl (meth)acrylate. 3 . The separator according to claim 1 , wherein the copolymer binder is obtained by copolymerizing two or more selected from polyacrylic acid, polyacrylamide, and polyvinyl alcohol. The separator according to claim 3 , wherein the copolymer binder is obtained by copolymerizing polyacrylic acid and polyacrylamide at a ratio of 8:2 to 5:

5.

5. The separator according to claim 1, wherein the acrylic polymer binder is in the form of particles having an average particle size (D50) of 100 nm to 500 nm, and The copolymer binder is in non-particulate form. 6 . The separator according to claim 1 , wherein the porous coating layer comprises 90 wt % to 95 wt % of the inorganic particles based on the total weight of the porous coating layer. 7 . The separator according to claim 1 , wherein the content of the acrylic polymer binder is greater than the content of the copolymer binder based on the weight of the porous coating layer. 8 . The separator according to claim 7 , wherein the acrylic polymer binder and the copolymer binder are included in a weight ratio of 5:1 to 1.5:

1.

9. An electrochemical device comprising: positive electrode; negative electrode; and A separator disposed between the positive electrode and the negative electrode, The separator is the separator for an electrochemical device according to claim 1.

10. The electrochemical device according to claim 9, further comprising: An electrolyte including a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a weight ratio of 3:7.

Citation Information

Patent Citations

  • Resource transmission method, device and communication device

    KR1020230035101A

  • Methods for receiving multicast services, configuration methods, terminals, and network-side devices