An organic-inorganic composite high-resistivity layer for the side glaze of a zinc oxide resistor and its preparation method
By preparing an inorganic-organic composite high-resistivity layer on the side of the zinc oxide resistor, the problems of insufficient high temperature resistance, high current impact resistance, and leakage current performance of the glaze high-resistivity layer on the side of the zinc oxide resistor are solved, thus achieving efficient insulation protection for the resistor.
Patent Information
- Application Number
- CN202411476609.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-10-22
AI Technical Summary
The existing high-resistivity glaze layer on the side of zinc oxide resistor sheets has shortcomings in terms of high temperature resistance, high current impact resistance and leakage current performance, especially the poor adhesion of epoxy glaze, easy cracking of glass glaze and poor insulation of inorganic glaze.
An inorganic-organic composite high-resistivity layer is adopted. An inorganic coating is first prepared on the side of the zinc oxide resistor sheet, and then an organic coating is rolled on. Components such as aluminum salt, water-based epoxy resin, and polyamide resin are used, combined with low-temperature calcination technology to form a dense and uniform high-resistivity layer.
It significantly improves the resistance of the resistor sheet to high temperature, high current impact and leakage current, reduces the curing temperature, enhances the bonding force with the resistor sheet, and improves the uniformity and density of the resistor sheet.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to a high-performance organic-inorganic high-resistivity glaze layer for the side surface of zinc oxide resistors and its preparation method, belonging to the technical field of resistor side surface glaze coating. Background Technology
[0002] Zinc oxide resistance elements possess excellent nonlinear volt-ampere characteristics, large current-carrying capacity, and low leakage current, making them a widely used core component of surge arresters in power systems. They can absorb overvoltage energy from power transmission lines and limit overvoltage amplitude, thus effectively protecting electrical equipment from damage caused by lightning and other overvoltages.
[0003] The ability of a resistive element to withstand high-current surges is one of its important characteristic parameters. When the duration of a high-current pulse is short, surface flashover failure can occur. Therefore, to improve the resistive element's ability to withstand steep-wave high-current surges, it is necessary to solve the surface flashover problem by roll-coating a side insulating layer. Currently, there are three main types of side insulating materials commonly used domestically and internationally: epoxy glaze, glass glaze, and inorganic high-resistivity layer.
[0004] Epoxy glaze is made from epoxy resin and curing agent as the insulating matrix, with the addition of certain amounts of inorganic fillers, diluents, and colorants. It is easily mixed with solids or other substances, exhibits high adhesion, and low shrinkage. Furthermore, it possesses excellent chemical stability, showing superior resistance to various chemicals, low water absorption, and excellent electrical insulation properties, thus enhancing lateral insulation strength to some extent. However, due to its poor adhesion and a significant difference in expansion coefficient compared to valve plates, it is prone to micro-cracks and other defects under thermal shock, leading to a decrease in insulation performance and thus limiting its application range.
[0005] Glass glaze has strong insulation and stain resistance, making it a relatively ideal side protection material. However, the inconsistent coefficients of thermal expansion of glass glazes can easily cause cracking or even detachment when the resistor element is subjected to high current surges. Furthermore, due to environmental protection requirements, lead-free glass glazes are now generally used. However, most lead-free glass glazes have high sintering temperatures, far exceeding the heat treatment temperature of the resistor element, leading to performance degradation and limiting their widespread use.
[0006] Inorganic side glaze is an insulating ceramic formed by high-temperature sintering together with the resistor blank. It features strong bonding and aging resistance. Without affecting the voltage-current characteristics of the resistor itself, it can improve short-wave discharge capacity and enhance moisture resistance, arc resistance, and corona resistance. However, inorganic side glaze generally suffers from poor insulation and weak hydrophobicity, which may reduce insulation performance due to moisture absorption.
[0007] To address the current issues with the high-resistivity glaze layer on the side of resistor sheets, a dense and uniform inorganic coating is first prepared on the side of the resistor sheet. Then, a novel organic composite coating is rolled onto the surface of the inorganic coating, thereby obtaining an organic-inorganic composite high-resistivity layer with low curing temperature, high temperature resistance, high current impact resistance, and low leakage current. Summary of the Invention
[0008] The key technical problem to be solved by the present invention is to provide an organic-inorganic composite high-resistivity layer for the side glaze of zinc oxide resistor sheet and its preparation method, aiming to improve its performance in terms of high temperature resistance, high current impact resistance and low leakage current.
[0009] To address the aforementioned problems, the present invention provides the following technical solution: An organic-inorganic composite high-resistivity layer for the side glaze of a zinc oxide resistor sheet comprises the following raw materials in parts by weight: Inorganic components: Aluminum salt component 10-20; Inorganic filler component 50-70; Waterborne epoxy resin component 10-30; 5-10g distilled water; Organic components: Epoxy resin component 10-20; Polyamide resin component 3-5; JYM resin powder components 5-7; Acrylic resin component 3-5; Organosilicon resin components 5-7; Silane coupling agent components 2-5; Cyclohexanone 1-5 parts.
[0010] Furthermore, the aluminum salt component is one or two of aluminum phosphate, aluminum dihydrogen phosphate, aluminum chloride, and aluminum oxide.
[0011] Furthermore, the inorganic filler component is one or two of mullite, iron oxide black, and iron oxide red.
[0012] Furthermore, the waterborne epoxy resin component is of type 387w; the epoxy resin component is one or both of type E-12 and E-44.
[0013] Furthermore, the polyamide resin component is one or both of PA12 or PPA with a low molecular weight.
[0014] Furthermore, the acrylic resin component is designated as type 772A, and the silicone resin component is one or both of type 3037 and 3074.
[0015] Furthermore, the silane coupling agent component is one or two of KH550, KH560, and KH602.
[0016] This invention also provides a method for preparing the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet, the specific steps of which are as follows: a. After mixing the inorganic components in proportion, add dispersant and water, grind evenly, and then roll-coat the mixture onto the already formed zinc oxide resistive layer. After calcination, an inorganic high-resistivity layer is obtained. b. After mixing the organic components in proportion, add the dispersant and cyclohexanone, grind them evenly, and then roll them onto the inorganic coating that has been formed after step a. After calcination, an organic high-resistance layer is obtained.
[0017] Furthermore, in step a, the grinding time is 2-5 hours, and the ground slurry is roller-coated onto the already formed zinc oxide resistor sheet with a thickness of 0.1-0.6 mm.
[0018] Furthermore, the calcination temperature in step a is 280-450℃, and the time is 3-8h.
[0019] Furthermore, in step b, the grinding time is 3-7 hours, and the ground slurry is roller-coated onto the surface of the sintered inorganic coating of the resistor sheet, with a thickness of 0.2-0.5 mm.
[0020] Furthermore, the calcination temperature in step b is 170-230°C. o C, the time is 2-5 hours.
[0021] A typical preparation method for the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet of the present invention is as follows: 1. The formula, by weight, includes the following components: aluminum salt component: 10-20 parts, inorganic filler component: 50-70 parts, waterborne epoxy resin component: 10-30 parts, and distilled water: 5-10 parts. 2. Weigh all raw materials according to the formula listed in "1" above, then place them in a ball mill for wet grinding for 2-5 hours. Roll-coat the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of approximately 0.1-0.6 mm, at a temperature of 280-450 °C. o After calcining at C for 3-8 hours, an inorganic high-resistivity layer is obtained; 3. The formula, by weight, includes the following components: epoxy resin: 10-20 parts, polyamide resin: 3-5 parts, JYM resin powder: 5-7 parts, acrylic resin: 3-5 parts, silicone resin: 5-7 parts, silane coupling agent: 2-5 parts, and cyclohexanone: 1-5 parts. 4. Weigh all raw materials according to the formula listed in "3", then place them in a ball mill for wet grinding for 3-7 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of approximately 0.2-0.5 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 2-5 hours at a temperature controlled at 170-230°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze; Compared with the prior art, the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet proposed in this invention has the following advantages: 1. The inorganic high-resistivity layer in the side glaze prepared by the method of the present invention uses a very viscous aluminum salt binder that can be cured at low temperature. Compared with conventional side glaze preparation methods, it greatly reduces the curing temperature, which helps stabilize the zinc oxide resistor sheet blank formulation. At the same time, it has strong bonding force with the blank and significantly improves its resistance to shock, peeling and high-temperature airflow erosion.
[0022] 2. The organic high-resistivity layer in the side glaze prepared by the method of the present invention is used to prepare zinc oxide resistor sheets by adding polyamide resin components to replace the traditional polymer adhesive polyvinyl alcohol. By utilizing the lubricity of polyamide resin and other series of polymers, the formation of bubbles in each process is reduced, the uniformity and density of the resistor sheet are improved, thereby improving the high current carrying capacity of the resistor sheet.
[0023] 3. After being treated with a composite of inorganic and organic high-resistivity layers, the overall performance of the glaze on the side of the resistor sheet, such as high temperature resistance, high current impact resistance, and leakage current, is significantly improved. Detailed Implementation
[0024] The present invention will be further described below with reference to specific embodiments. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art can make some non-essential improvements and adjustments based on the above-described invention.
[0025] The mass fractions in the embodiments and comparative examples of this invention are all in grams.
[0026] Example 1 The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet in this embodiment is as follows: 1. The formula, by weight, includes the following components: aluminum dihydrogen phosphate: 10 parts; iron oxide black: 70 parts; 387w waterborne epoxy resin: 15 parts; and distilled water: 5 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 3 hours. Roll the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and then heat at 280°C. oAfter calcining at C for 4 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight, includes the following components: E-44 epoxy resin: 15 parts, PPA polyamide resin: 3 parts, JYM resin powder: 5 parts, 772A acrylic resin: 3 parts, 3074 silicone resin: 7 parts, KH560 silane coupling agent: 3 parts, and cyclohexanone: 4 parts. 4. Weigh all raw materials according to the above formula, then wet grind them in a ball mill for 4 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 3 hours at a temperature controlled at 190°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0027] Example 2 The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet in this embodiment is as follows: 1. The formula, by weight, includes the following components: alumina: 12 parts, mullite: 65 parts, 387w waterborne epoxy resin: 13 parts, and distilled water: 10 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 3 hours. Roll the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and then heat at 300°C. o After calcining at C for 5 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight, includes the following components: E-12 epoxy resin: 10 parts, PPA polyamide resin: 4 parts, JYM resin powder: 7 parts, 772A acrylic resin: 5 parts, 3074 silicone resin: 7 parts, KH560 silane coupling agent: 4 parts, and cyclohexanone: 3 parts. 4. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 5 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 3 hours at a temperature controlled at 210°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0028] Example 3 The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet in this embodiment is as follows: 1. The formula, by weight, includes the following components: aluminum phosphate: 15 parts, iron oxide red: 55 parts, 387w waterborne epoxy resin: 23 parts, and distilled water: 7 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 2-5 hours. The ground slurry is then roller-coated onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and heated at 330°C. o After calcining at C for 6 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight, includes the following components: E-12 epoxy resin: 12 parts, PA12 polyamide resin: 5 parts, JYM resin powder: 7 parts, 772A acrylic resin: 4 parts, 3037 silicone resin: 6 parts, KH602 silane coupling agent: 4 parts, and cyclohexanone: 2 parts. 4. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 4 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 4 hours at a temperature controlled at 220°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0029] Example 4 The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet in this embodiment is as follows: 1. The formula, by weight, includes the following components: aluminum chloride: 18 parts, mullite: 37 parts, iron oxide red: 20 parts, 387w waterborne epoxy resin: 17 parts, and distilled water: 8 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 2-5 hours. Roll the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and then heat at 360°. o After calcining at C for 7 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight, specifically includes the following components: E-12 epoxy resin: 18 parts, PA12 polyamide resin: 3 parts, JYM resin powder: 5 parts, 772A acrylic resin: 3 parts, 3037 silicone resin: 5 parts, KH602 silane coupling agent: 1 part, KH550 silane coupling agent: 1 part, cyclohexanone: 4 parts; 4. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 4 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 4 hours at a temperature controlled at 230°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0030] Example 5 The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet in this embodiment is as follows: 1. The formula, by weight, includes the following components: aluminum chloride: 20 parts, mullite: 65 parts, 387w waterborne epoxy resin: 10 parts, and distilled water: 5 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 2-5 hours. The ground slurry is then roller-coated onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and heated at 400°C. o After calcining at C for 8 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight parts, specifically includes: E-12 epoxy resin: 10 parts, E-44 epoxy resin: 10 parts, PA12 polyamide resin: 1 part, PPA polyamide resin: 2 parts, JYM resin powder: 5 parts, 772A acrylic resin: 3 parts, 3037 silicone resin: 1 part, 3074 silicone resin: 4 parts, KH602 silane coupling agent: 1 part, KH560 silane coupling agent: 1 part, cyclohexanone: 2 parts; 4. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 4 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 2 hours at a temperature controlled at 180°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0031] Example 6 The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet in this embodiment is as follows: 1. The formula, by weight, includes the following components: aluminum dihydrogen phosphate: 14 parts, iron oxide red: 50 parts, 387w waterborne epoxy resin: 30 parts, and distilled water: 6 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 2-5 hours. The ground slurry is then roller-coated onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and heated at 450°C. o After calcining at C for 3 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight parts, specifically includes: E-12 epoxy resin: 5 parts, E-44 epoxy resin: 5 parts, PA12 polyamide resin: 2 parts, PPA polyamide resin: 3 parts, JYM resin powder: 6 parts, 772A acrylic resin: 4 parts, 3037 silicone resin: 2 parts, 3074 silicone resin: 3 parts, KH550 silane coupling agent: 2 parts, KH560 silane coupling agent: 3 parts, cyclohexanone: 5 parts; 4. Weigh all raw materials according to the above formula, then wet grind them in a ball mill for 4 hours. Roll the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 5 hours at a temperature controlled at 170°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0032] Compare with Example 1 Based on Example 1, the inorganic component does not contain aluminum dihydrogen phosphate, and the other steps are the same as in Example 1. The specific method is as follows: 1. The formula, by weight, includes the following components: iron oxide black component: 80 parts, 387w waterborne epoxy resin component: 15 parts, distilled water: 5 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 3 hours. Roll the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and then heat at 280°C. o After calcining at C for 4 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight, includes the following components: E-44 epoxy resin: 15 parts, PPA polyamide resin: 3 parts, JYM resin powder: 5 parts, 772A acrylic resin: 3 parts, 3074 silicone resin: 7 parts, KH560 silane coupling agent: 3 parts, and cyclohexanone: 4 parts. 4. Weigh all raw materials according to the above formula, then wet grind them in a ball mill for 4 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 3 hours at a temperature controlled at 190°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0033] Compare with Example 2 Based on Example 1, the polyamide resin component was replaced with the polyvinyl alcohol component, and the other steps were the same as in Example 1. The specific method is as follows: 1. The formula, by weight, includes the following components: aluminum dihydrogen phosphate: 10 parts; iron oxide black: 70 parts; 387w waterborne epoxy resin: 15 parts; and distilled water: 5 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 3 hours. Roll the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and then heat at 280°C. o After calcining at C for 4 hours, an inorganic high-resistivity layer was obtained; 3. The formula, by weight, includes the following components: E-44 epoxy resin: 15 parts, PVA-217 polyvinyl alcohol: 3 parts, JYM resin powder: 5 parts, 772A acrylic resin: 3 parts, 3074 silicone resin: 7 parts, KH560 silane coupling agent: 3 parts, and cyclohexanone: 4 parts. 4. Weigh all raw materials according to the above formula, then wet grind them in a ball mill for 4 hours. Roll-coat the ground slurry onto the surface of the sintered inorganic coating on the resistor sheet, with a thickness of 0.2-0.4 mm. After roller coating, place the resistor sheet in a heating furnace and heat for 3 hours at a temperature controlled at 190°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0034] Compare with Example 3 Based on Example 1, without preparing an organic high-resistivity layer, the other steps are the same as in Example 1, and the specific methods are as follows: 1. The formula, by weight, includes the following components: aluminum dihydrogen phosphate: 10 parts; iron oxide black: 70 parts; 387w waterborne epoxy resin: 15 parts; and distilled water: 5 parts. 2. Weigh all raw materials according to the above formula, then place them in a ball mill for wet grinding for 3 hours. Roll the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.3-0.4 mm, and then heat at 280°C. o After calcining at C for 4 hours, an inorganic high-resistivity layer was obtained; Compare with Example 4 Based on Example 1, without preparing an inorganic high-resistivity layer, the other steps are the same as in Example 1, and the specific methods are as follows: 1. The formula, by weight, includes the following components: E-44 epoxy resin: 15 parts, PPA polyamide resin: 3 parts, JYM resin powder: 5 parts, 772A acrylic resin: 3 parts, 3074 silicone resin: 7 parts, KH560 silane coupling agent: 3 parts, and cyclohexanone: 4 parts. 2. Weigh all raw materials according to the above formula, then wet grind them in a ball mill for 4 hours. Roll-coat the ground slurry onto the pre-formed zinc oxide resistance sheet to a thickness of 0.2-0.4 mm. After roller coating, place the resistance sheet in a heating furnace and heat for 3 hours at a temperature controlled at 190°C. o C, thereby obtaining a high-temperature resistant organic high-resistance layer for the side glaze.
[0035] Using the Φ28*30 size resistor blank produced by the manufacturer as the substrate, the electrical insulation performance (leakage current, high current impact test) of the insulating coating prepared in Examples 1-3 was tested, and the results are shown in Table 1.
[0036] Table 1. Test results of electrical insulation performance of insulating coating in the examples
[0037] As shown in Table 1, the inorganic-organic double-coated side glaze insulating coating prepared using the formula and process provided by this invention resulted in low leakage current and stable 4 / 10 μs high current impact performance for the resistor samples prepared according to Examples 1, 2, and 3. After multiple batch tests, the Φ28*30 resistor successfully passed multiple impact tests at an amplitude of 65 KA in 4 / 10 μs, meeting the requirements for high current resistance. The leakage current level of the Φ28*30 resistor was less than 7 μA, with a leakage current variation of no more than 2 μA, meeting the requirements for leakage current level.
[0038] Using the Φ28*30 size resistor blank produced by the manufacturer as the substrate, the test results of the electrical insulation performance (leakage current, high current impact test) of the insulating coating prepared in Example 1 and Comparative Examples 1-4 are shown in Table 2.
[0039] Table 2 Test results of electrical insulation performance of insulating coatings in comparison examples
[0040] Table 2 shows that the electrical insulation performance (leakage current, high current impact test) test results of the insulating coatings prepared in Example 1 and Comparative Example 1 indicate that when aluminum salt components are used as binders, their bonding force with the resistor valve body is strong, and their performance in terms of shock resistance, peeling resistance, and resistance to high-temperature airflow erosion is significantly improved. Furthermore, it can be cured at low temperatures, which greatly reduces the curing temperature compared with conventional side glaze preparation methods (curing temperature above 1000℃), thus contributing to the stability of the zinc oxide resistor blank formulation.
[0041] The electrical insulation performance (leakage current, high current impulse test) test results of the insulating coatings prepared in Example 1 and Comparative Example 2 show that when polyamide resin component is used to replace polyvinyl alcohol as the polymer adhesive in the preparation of zinc oxide resistor sheet, the uniformity and density of the high-resistivity layer of the resistor sheet are significantly improved, thereby improving the high current carrying capacity of the resistor sheet.
[0042] The test results of the electrical insulation performance (leakage current, high current impact test) of the insulating coatings prepared in Example 1 and Comparative Examples 3-4 show that, compared with the use of separate inorganic high-resistivity layers and organic high-resistivity layers, when the resistor sheet uses an inorganic-organic composite high-resistivity layer, no side flashing or glaze peeling occurs during the test. The overall high temperature resistance, high current impact resistance, and leakage current and other conventional properties of the glaze on the side of the resistor sheet are significantly improved.
[0043] The implementation of this invention can solve practical problems in the actual production of resistor sheets. It comprehensively addresses issues such as adhesion between the side coating material and the zinc oxide resistor body, insulation, high current resistance, and temperature resistance by employing an inorganic-organic composite coating method. The inorganic coating material has a coefficient of thermal expansion close to that of the inorganic insulating coating of the zinc oxide resistor body. This coating has strong adhesion to the body and expands together with the body upon heating, improving heat resistance and providing excellent protection against lightning pulses or overvoltages. The lubricity and density of the resistor sheet are improved by adding polyamide resin and other polymers, thereby enhancing its high current carrying capacity. The inorganic and organic coatings adhere well, the composite insulating coating has a good electrical life, and it provides excellent protection against lightning strikes and overvoltage surges. The prepared product and manufacturing process are environmentally friendly, using raw materials free of toxic substances such as lead and avoiding the use of highly toxic organic solvents such as toluene. It does not cause environmental pollution during manufacturing or disposal, thus possessing significant potential social and economic benefits and broad application prospects.
[0044] The foregoing has shown and described the basic principles and main features of the present invention, as well as its advantages. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A zinc oxide resistor sheet side glaze organic-inorganic composite high-resistivity layer, characterized in that, The raw materials include the following parts by weight: Inorganic components: Aluminum salt component 10-20; Inorganic filler component 50-70; Waterborne epoxy resin component 10-30; 5-10g distilled water; Organic components: Epoxy resin component 10-20; Polyamide resin component 3-5; JYM resin powder components 5-7; Acrylic resin component 3-5; Organosilicon resin components 5-7; Silane coupling agent components 2-5; Cyclohexanone 1-5; The aluminum salt component is one or two of aluminum phosphate, aluminum dihydrogen phosphate, and aluminum chloride. The preparation method of the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet includes the following steps: a. Mix the inorganic components according to the proportion, grind them evenly, roll them onto the formed zinc oxide resistor sheet, and calcine them to obtain an inorganic high-resistivity layer. b. Mix the organic components according to the proportion, grind them evenly, and then roll them onto the inorganic high-resistivity layer that has been formed after step a. After calcination, the organic high-resistivity layer is obtained.
2. The organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 1, characterized in that, The inorganic filler component is one or two of mullite, iron oxide black, and iron oxide red.
3. The organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 1, characterized in that, The waterborne epoxy resin component is of type 387w; the epoxy resin component is one or both of type E-12 and E-44; the polyamide resin component is one or both of type PA12 or PPA.
4. The organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 1, characterized in that, The acrylic resin component is of type 772A, and the silicone resin component is one or both of type 3037 and 3074; the silane coupling agent component is one or both of type KH550, KH560, and KH602.
5. A method for preparing an organic-inorganic composite high-resistivity layer on the side glaze of a zinc oxide resistor sheet according to any one of claims 1-4, characterized in that, The specific steps are as follows: a. Mix the inorganic components according to the proportion, grind them evenly, roll them onto the formed zinc oxide resistor sheet, and calcine them to obtain an inorganic high-resistivity layer. b. Mix the organic components according to the proportion, grind them evenly, and then roll them onto the inorganic high-resistivity layer that has been formed after step a. After calcination, the organic high-resistivity layer is obtained.
6. The method for preparing the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 5, characterized in that, In step a, the grinding time is 2-5 hours. The ground slurry is then rolled onto the already formed zinc oxide resistor sheet with a thickness of 0.1-0.6 mm.
7. The method for preparing the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 5, characterized in that, The calcination temperature in step a is 280-450℃, and the time is 3-8h.
8. The method for preparing the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 5, characterized in that, In step b, the grinding time is 3-7 hours. The ground slurry is then roller-coated onto the surface of the inorganic high-resistivity layer of the calcined resistor sheet, with a thickness of 0.2-0.5 mm.
9. The method for preparing the organic-inorganic composite high-resistivity layer on the side glaze of the zinc oxide resistor sheet according to claim 5, characterized in that, The calcination temperature in step b is 170-230°C. o C, the time is 2-5 hours.
Citation Information
Patent Citations
Preparation method of inorganic insulating coating based on synergistic cooperation of inorganic high-resistance layer and low-temperature glass glaze
CN112694348A
Voltage nonlinear resistor and its producing method
CN1290943A
Method for coating a conductive material
US4036721A