Metal pipes for oil wells

By forming an epoxy resin coating on the contact surface of the metal pipe used in oil wells, the problems of wear and adhesion during thread tightening are solved, improving high torque performance and airtightness, and ensuring the stability of tightening torque.

CN119452200BActive Publication Date: 2026-11-17NIPPON STEEL CORPORATION +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380050133.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-07-01
Filing Date
2023-06-29
Publication Date
2026-11-17
Estimated Expiration
2043-06-29

AI Technical Summary

Technical Problem

Existing metal pipes for oil wells are prone to wear and jamming during the tightening and loosening of threads, and have failed to effectively improve high torque performance, affecting the adjustment of tightening torque and airtightness.

Method used

A resin coating is formed on the contact surfaces of the male and female threads of the metal pipe used in oil wells. Specifically, epoxy resin is used as the coating material, and the weighted average value of the spin-spin relaxation time T2 of the resin coating is controlled to be below 110.0 μs by 1H pulse NMR method to improve adhesion and crosslinking density.

Benefits of technology

This technology improves the high torque performance of metal pipes used in oil wells, enhances the stability and airtightness of tightening torque, and reduces wear and adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119452200B_ABST
    Figure CN119452200B_ABST
Patent Text Reader

Abstract

A metal pipe for oil wells with excellent high torque performance is provided. The metal pipe (1) for oil wells disclosed herein comprises a pipe body (10). The pipe body (10) includes a male thread portion (40) and a female thread portion (50). The male thread portion (40) has a male thread contact surface (400) including an external thread portion (41). The female thread portion (50) has a female thread contact surface (500) including an internal thread portion (51). The metal pipe (1) for oil wells further comprises a resin coating (100) formed as the uppermost layer of at least one of the male thread contact surface (400) and the female thread contact surface (500). The resin coating (100) contains epoxy resin. 1 When the resin coating (100) was measured by H-pulse NMR, the obtained free induction decay signal was divided into three components in sequence from the component with the long spin-spin relaxation time (T2): high-motor component, medium-motor component, and low-motor component. The weighted average of the spin-spin relaxation time (T2) of the three components was less than 110.0 μs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to metal pipes for oil wells. Background Technology

[0002] Oil well metal tubing is used in oil wells and natural gas wells (hereinafter, oil wells and natural gas wells are collectively referred to as "oil wells"). Specifically, at the oil well production site, multiple oil well metal tubings are connected to form an oil well tubing connection, represented by casing and tubing. An oil well tubing connection is formed by tightening threaded joints together. There are situations where the oil well tubing connection needs to be inspected. In such cases, the oil well tubing connection is pulled up and the threads are loosened. The oil well metal tubing is removed from the connection by loosening the threads and inspected. After inspection, the threaded joints of the oil well metal tubing are tightened again, and the connection is reused as part of the oil well tubing connection.

[0003] The oil well metal pipe has a male thread and a female thread. The male thread has a male thread contact surface, including an external thread, on the outer circumferential surface of the end of the oil well metal pipe. The female thread has a female thread contact surface, including an internal thread, on the inner circumferential surface of the end of the oil well metal pipe. In this specification, the external thread and the internal thread are collectively referred to as "threaded portion". In this specification, the male thread contact surface and the female thread contact surface are collectively referred to as "contact surface". The male thread contact surface may also include a threadless metal contact portion, which includes a male thread sealing surface and a male thread shoulder surface. Similarly, the female thread contact surface may also include a threadless metal contact portion, which includes a female thread sealing surface and a female thread shoulder surface.

[0004] The contact surfaces of oil well metal pipes are subjected to strong friction during repeated tightening and loosening of the threads. Therefore, the contact surfaces are prone to abrasion and seizure (irreparable adhesion) after repeated tightening and loosening of the threads. Consequently, oil well metal pipes require sufficient durability against friction, i.e., excellent resistance to adhesion.

[0005] Previously, composite greases containing heavy metal powders, known as dopants, were used to improve the anti-adhesion properties of metal pipes used in oil wells. Applying composite grease to the contact surfaces improved the anti-adhesion properties of the metal pipes. However, there is a possibility that the heavy metal powders such as Pb, Zn, and Cu contained in the composite grease could have environmental impacts. Therefore, it is desirable to develop metal pipes for oil wells that exhibit excellent anti-adhesion properties even without the use of composite grease.

[0006] Techniques for improving the adhesion resistance of metal pipes used in oil wells have been proposed, for example, in Japanese Patent Application Publication No. 2002-348587 (Patent Document 1) and International Publication No. 2006 / 104251 (Patent Document 2).

[0007] Patent Document 1 discloses a metal pipe for oil wells in which a solid lubricating film composed of lubricating powder and an adhesive is formed on the contact surface of at least one of the male and female threads. The lubricating powder is composed of one or two types selected from molybdenum disulfide powder and tungsten disulfide powder, and graphite powder. The graphite powder accounts for 2 to 20% by mass of the lubricating powder. Patent Document 1 discloses that this metal pipe for oil wells can improve the anti-adhesion properties of the metal pipe for oil wells.

[0008] Patent Document 2 discloses a metal pipe for oil wells having a viscous liquid or semi-solid lubricating film and a dry solid film formed thereon on the contact surface of at least one of the male and female threads. Patent Document 2 also discloses that this metal pipe for oil wells inhibits rusting even without the use of composite grease, and improves resistance to adhesion and airtightness.

[0009] Existing technical documents

[0010] Patent documents

[0011] Patent Document 1: Japanese Patent Application Publication No. 2002-348587

[0012] Patent Document 2: International Publication No. 2006 / 104251 Summary of the Invention

[0013] The problem the invention aims to solve

[0014] However, what is desirable is high torque performance for oil well tubing. High torque performance means higher shoulder friction torque. Shoulder friction torque refers to the difference between the yield torque of a portion of the threaded joint (male or female) of the oil well tubing and the shoulder torque caused by the abrupt increase in interference between the threaded joints (male and female).

[0015] If the shoulder friction torque increases, adjusting the tightening torque becomes easier. Even in the case where the metal tubing for oil wells does not have a shoulder surface, adjusting the tightening torque becomes easier if the torque increases steadily.

[0016] If the coating disclosed in Patent Documents 1 and 2 is used, the adhesion resistance of metal pipes used in oil wells can be improved. However, high torque performance was not studied in Patent Documents 1 and 2.

[0017] The purpose of this disclosure is to provide metal tubing for oil wells with excellent high torque performance.

[0018] Solution for solving the problem

[0019] The metal pipe for oil wells disclosed herein comprises a pipe body including a first end and a second end.

[0020] The pipe body includes:

[0021] The male fastener is formed at the first end; and

[0022] The female buckle portion is formed at the second end.

[0023] The male thread portion has a male thread contact surface including an external thread portion.

[0024] The female threaded portion has a female threaded portion contact surface.

[0025] The oil well metal pipe also has a resin coating formed as the uppermost layer of at least one of the male thread contact surface and the female thread contact surface.

[0026] The resin coating contains epoxy resin.

[0027] In 1 The resin coating was measured by H-pulse NMR. When the obtained free induction decay signal was divided into three components in sequence from the component with long spin-spin relaxation time (T2): high-motor component, medium-motor component, and low-motor component, the weighted average value of the spin-spin relaxation time (T2) of the three components was less than 110.0 μs.

[0028] The effects of the invention

[0029] The metal tubing for oil wells disclosed herein has excellent high torque performance. Attached Figure Description

[0030] Figure 1 This is a diagram showing the relationship between the number of threads and the torque when fastening a metal pipe for an oil well with a shoulder surface.

[0031] Figure 2 This is a graph showing the relationship between the relaxation time T2 and the shoulder friction torque ΔT of a resin coating containing epoxy resin.

[0032] Figure 3 This is a side view of the metal pipe for oil wells according to this embodiment.

[0033] Figure 4 It means Figure 3 The diagram shows a partial sectional view of the pipe fitting of an oil well metal pipe, in a section (longitudinal section) parallel to the pipe axis.

[0034] Figure 5 yes Figure 4The diagram shows a cross-sectional view of the portion near the male thread in a metal pipe for oil wells, parallel to the pipe axis.

[0035] Figure 6 yes Figure 4 The diagram shows a cross-sectional view of the portion near the female thread in the oil well tubing, parallel to the pipe axis.

[0036] Figure 7 Is with Figure 3 A partial sectional view, including a longitudinal section, of the metal tubing for oil wells in this embodiment with different structures.

[0037] Figure 8 This is a partial sectional view of the integral metal pipe for oil wells in this embodiment, including the longitudinal section.

[0038] Figure 9 This is a cross-sectional view near the contact surface of the male thread portion of the metal pipe for oil wells in this embodiment.

[0039] Figure 10 Is with Figure 9 A cross-sectional view of the area near the contact surface of the corresponding female buckle.

[0040] Figure 11 Is with Figure 9 A cross-sectional view near the contact surface of the male fastener in this embodiment, but in a different manner.

[0041] Figure 12 Is with Figure 11 A cross-sectional view of the area near the contact surface of the corresponding female buckle. Detailed Implementation

[0042] Hereinafter, this embodiment will be described in detail with reference to the accompanying drawings. The same or equivalent parts in the drawings will be labeled with the same reference numerals and will not be described repeatedly.

[0043] The inventors have studied a method for improving the high-torque performance of metal tubing used in oil wells. The results yielded the following insights.

[0044] When fastening the metal pipes of the oil well to each other, the optimal torque for ending the fastening should be determined in advance. Figure 1 This is a diagram showing the relationship between the number of threads and the torque when fastening a metal pipe with a shoulder surface for oil wells. (Refer to...) Figure 1When tightening the threads of a well pipe, the torque initially increases gradually in proportion to the number of threads. With further tightening, the shoulder surfaces come into contact. This torque is called the shoulder torque Ts. If further tightening is performed after reaching the shoulder torque Ts, the torque increases sharply in proportion to the number of threads. Tightening is complete when the torque reaches a predetermined value (tightening torque To). At the tightening torque To, the contact surfaces interfere with each other with appropriate surface pressure. In this case, the well pipe achieves high airtightness. If excessive tightening is performed after reaching the tightening torque To, the torque reaches the yield torque Ty, and a portion of the male and female threads yields. In this specification, the difference between the shoulder torque Ts and the yield torque Ty is called the shoulder friction torque ΔT.

[0045] In addition, as another type of metal tubing for oil wells, there are tubings with wedge threads but without a shoulder. In the case of such wedge-threaded tubing, the relationship between the number of threads and torque is the same as in the case of tubing with a shoulder. Figure 1 so.

[0046] Wedge-shaped threads are threads with the following structure: In the external thread portion of a wedge-shaped thread, as the male thread is screwed in, the width of the thread teeth gradually narrows along the helix of the thread, while the width of the thread groove gradually widens along the helix of the thread. Similarly, in the internal thread portion of a wedge-shaped thread, as the female thread is screwed in, the width of the thread groove gradually narrows along the helix of the thread, while the width of the thread teeth gradually widens along the helix of the thread. In the case of oil well metal pipes with wedge-shaped threads, as the threads are tightened, the bearing tooth flanks of the external and internal threads come into contact with each other and the insert tooth flanks, creating a locking (interference fit). The torque that creates this locking is also called the locking torque or the locking tooth flank torque.

[0047] In this specification, unless otherwise stated, the locking torque and shoulder torque are not distinguished, and are referred to as shoulder torque Ts. In the case of oil well tubing with wedge threads, similar to the case of oil well tubing with a shoulder surface, if the threads are further tightened after reaching the shoulder torque Ts, the torque increases sharply in proportion to the number of threads. That is, after the shoulder torque Ts, the interference between the threaded joints (male and female threads) increases sharply. Furthermore, if the threads are further tightened, the tightening torque To is reached. If the threads are excessively tightened after reaching the tightening torque To, the yield torque Ty is reached, and part of the male and female threads yields.

[0048] As disclosed in Patent Documents 1 and 2, it is known that there are oil well metal pipes with a resin-containing coating. Therefore, the inventors believe that it is sufficient to form a resin coating on the oil well metal pipe that can improve the high torque performance of the oil well metal pipe.

[0049] The inventors first studied the resin contained in the resin coating. They concluded that if the resin coating contains a resin with high adhesion to metal, peeling of the resin coating can be suppressed even due to shear forces generated by tightening the threads. Therefore, the inventors studied resins with high adhesion to metal. As a result, the following insights were obtained.

[0050] Epoxy resin is a thermosetting synthetic resin with reactive epoxy groups at the ends. A representative epoxy resin is bisphenol A type epoxy resin. Bisphenol A type epoxy resin has secondary alcohol hydroxyl groups within repeating units. Compared to other resins, epoxy resins exhibit higher adhesion to metals. The reasons for the higher adhesion of epoxy resins to metals are uncertain, but the following two reasons are considered: (1) The hydroxyl groups within the epoxy resin form hydrogen bonds with the hydroxyl groups on the metal surface. (2) For the adhesion between iron and zinc and epoxy resin, the phenoxy groups are related to the adhesive interface.

[0051] The inventors believe that if the resin coating contains epoxy resin, peeling of the resin coating can be suppressed even when shear forces are generated due to thread tightening. Therefore, the inventors conducted research on improving the high-torque performance of resin coatings containing epoxy resin. As a result, the following insights were obtained.

[0052] The inventors investigated the relationship between the crosslinking density of epoxy resin coatings and the shoulder friction torque ΔT. Epoxy resin coatings with varying crosslinking densities were formed on steel plates. The initial coefficient of friction was determined by performing a Bowden sliding test on the epoxy resin-coated steel plates. The shoulder friction torque ΔT was calculated from the initial coefficient of friction using FEM analysis. The results are presented in... Figure 2 middle.

[0053] Figure 2 The horizontal axis is based on 1 The weighted average (μs) of spin-spin relaxation time T2 during epoxy resin coating was determined by H-pulse NMR. Figure 2 The spin-spin relaxation time T2 is at the time when the ... 1 The H-pulse NMR method was used to determine the free induction decay signal of epoxy resin coating. The obtained signal was divided into three components with long spin-spin relaxation time T2: high-motor component, medium-motor component, and low-motor component. The weighted average of the spin-spin relaxation time T2 of the three components was obtained. Figure 2The vertical axis represents the shoulder friction torque ΔT (ft.lb). The spin-spin relaxation time T2 is an indicator of the decay characteristics of the magnetization.

[0054] The crosslinking density of the resin and the 1 The spin-spin relaxation time T2, as determined by H-pulse NMR, is directly proportional to the crosslinking density of the resin. In other words, the higher the crosslinking density of the resin, the shorter the spin-spin relaxation time T2. (Refer to...) Figure 2 If the weighted average of the spin-spin relaxation time T2 is reduced, the shoulder friction torque ΔT increases. In other words, increasing the crosslinking density of the epoxy resin coating increases the shoulder friction torque ΔT. Specifically, if the weighted average of the spin-spin relaxation time T2 is below 110.0 μs, the shoulder friction torque ΔT increases. Oil well metal pipes with resin coatings possessing a high shoulder friction torque ΔT exhibit excellent high torque performance.

[0055] Based on the above research, the inventors believe that the high torque performance of metal pipes for oil wells can be improved by increasing the crosslinking density of the epoxy resin coating. Specifically, if the weighted average value of the spin-spin relaxation time T2 of the epoxy resin coating is below 110.0 μs, the high torque performance of the metal pipe for oil wells is improved.

[0056] The rationale for improving the high torque performance of metal pipes for oil wells by increasing the crosslinking density of the epoxy resin coating is uncertain. However, in the examples described later, it is shown that if the weighted average of the spin-spin relaxation time T2 of the epoxy resin coating is 110.0 μs or less, the high torque performance of the metal pipes for oil wells can be improved.

[0057] Based on the above insights, the main idea of ​​the metal pipe for oil wells in this embodiment is as follows.

[0058] [1] A metal pipe for oil wells, comprising a pipe body including a first end and a second end,

[0059] The pipe body includes:

[0060] The male fastener is formed at the first end; and

[0061] The female buckle portion is formed at the second end.

[0062] The male thread portion has a male thread contact surface including an external thread portion.

[0063] The female threaded portion has a female threaded portion contact surface.

[0064] The oil well metal pipe also has a resin coating formed as the uppermost layer of at least one of the male thread contact surface and the female thread contact surface.

[0065] The resin coating contains epoxy resin.

[0066] In 1 The resin coating was measured by H-pulse NMR. When the obtained free induction decay signal was divided into three components in sequence from the component with long spin-spin relaxation time (T2): high-motor component, medium-motor component, and low-motor component, the weighted average value of the spin-spin relaxation time (T2) of the three components was less than 110.0 μs.

[0067] [2] According to the metal pipe for oil wells described in [1], wherein,

[0068] In the above 1 When the resin coating is measured by H-pulse NMR, the ratio of the medium-motor component to the sum of the high-motor component, the medium-motor component, and the low-motor component is higher than the ratio of the low-motor component to the sum.

[0069] [3] According to [1] or [2], the metal pipe for oil wells, wherein,

[0070] At least one of the male buckle contact surface and the female buckle contact surface is further provided with one or more of the following in the group consisting of phosphate coating, plating, chromate coating and zirconium coating between it and the resin coating.

[0071] The following section discusses in detail the metal pipe for oil wells according to this embodiment.

[0072] [Structure of metal pipes for oil wells]

[0073] First, the structure of the oil well metal pipe of this embodiment will be described. Oil well metal pipes have a well-known structure. Oil well metal pipes include T&C type oil well metal pipes and integral type oil well metal pipes. The following will discuss each type of oil well metal pipe in detail.

[0074] [The case where the metal pipe for oil wells is of type T&C]

[0075] Figure 3 This is a side view showing the metal pipe 1 for oil wells according to this embodiment. Figure 3 This is a side view of a so-called T&C (Threaded and Coupled) type metal pipe for oil wells. (Refer to...) Figure 3 The oil well metal pipe 1 has a pipe body 10.

[0076] The tube body 10 extends along the tube axis. The cross-section of the tube body 10 perpendicular to the tube axis is circular. The tube body 10 includes a first end 10A and a second end 10B. The first end 10A is the end opposite to the second end 10B. Figure 3 In the T&C type oil well metal pipe 1 shown, the pipe body 10 includes a male threaded pipe body 11 and a pipe fitting 12. The pipe fitting 12 is installed at one end of the male threaded pipe body 11. More specifically, the pipe fitting 12 is fastened to one end of the male threaded pipe body 11 by threads.

[0077] Figure 4 It means Figure 3 A partial sectional view of the pipe fitting 12 of the oil well metal pipe 1, shown as a section (longitudinal section) parallel to the pipe axis. (Refer to...) Figure 3 and Figure 4 The pipe body 10 includes a male threaded portion 40 and a female threaded portion 50. The male threaded portion 40 is formed at the first end 10A of the pipe body 10. When tightening, the male threaded portion 40 is inserted into the female threaded portion 50 of another oil well metal pipe 1 (not shown) and tightened with the female threaded portion 50 of the other oil well metal pipe 1 by means of threads.

[0078] The female thread 50 is formed at the second end 10B of the pipe body 10. During tightening, the male thread 40 of another oil well metal pipe 1 is inserted into the female thread 50 and tightened with the male thread 40 of the other oil well metal pipe 1 by means of threads.

[0079] [Regarding the structure of the male fastener 40]

[0080] Figure 5 yes Figure 4 A cross-sectional view of the portion near the male thread 40 of the oil well metal pipe 1, shown, parallel to the pipe axis direction of the oil well metal pipe 1. Figure 5 The dashed line indicates the structure of the female thread 50 of the other oil well metal pipe 1 when it is fastened to other oil well metal pipes 1. (Refer to...) Figure 5 The male thread 40 includes a male thread contact surface 400 on the outer peripheral surface of the first end 10A of the pipe body 10. When fastening with other oil well metal pipes 1, the male thread 40 is screwed into the female thread 50 of the other oil well metal pipe 1, and the male thread contact surface 400 contacts the female thread contact surface 500 (described later) of the female thread 50.

[0081] The male thread contact surface 400 includes at least an external thread portion 41 formed on the outer peripheral surface of the first end 10A. Alternatively, the male thread contact surface 400 may also include a male thread sealing surface 42 and a male thread shoulder surface 43. Figure 5In this design, the male thread shoulder surface 43 is disposed on the top surface of the first end portion 10A, and the male thread sealing surface 42 is disposed on the outer peripheral surface of the first end portion 10A, at a position closer to the top surface of the first end portion 10A than the external thread portion 41. That is, the male thread sealing surface 42 is disposed between the external thread portion 41 and the male thread shoulder surface 43. The male thread sealing surface 42 is tapered. Specifically, in the male thread sealing surface 42, along the length direction (pipe axis direction) of the first end portion 10A, the outer diameter gradually decreases from the external thread portion 41 toward the male thread shoulder surface 43.

[0082] When fastened to other oil well metal pipes 1, the male thread sealing surface 42 contacts the female thread sealing surface 52 (described later) of the female thread 50 of the other oil well metal pipe 1. More specifically, during fastening, the male thread 40 is inserted into the female thread 50 of the other oil well metal pipe 1, thereby bringing the male thread sealing surface 42 into contact with the female thread sealing surface 52. Then, by further screwing the male thread 40 into the female thread 50 of the other oil well metal pipe 1, the male thread sealing surface 42 and the female thread sealing surface 52 are tightly fitted together. Thus, during fastening, the male thread sealing surface 42 and the female thread sealing surface 52 are tightly fitted together to form a seal based on metal-metal contact. Therefore, in the mutually fastened oil well metal pipes 1, air tightness can be improved.

[0083] exist Figure 5 In the middle, the male buckle shoulder surface 43 is disposed on the top surface of the first end 10A. That is to say, in Figure 5 In the male thread portion 40 shown, an external thread portion 41, a male thread portion sealing surface 42, and a male thread portion shoulder surface 43 are sequentially arranged from the center of the pipe body 10 toward the first end 10A. When fastened to other oil well metal pipes 1, the male thread portion shoulder surface 43 faces and contacts the female thread portion shoulder surface 53 (described later) of the female thread portion 50 of the other oil well metal pipe 1. More specifically, during fastening, the male thread portion 40 is inserted into the female thread portion 50 of the other oil well metal pipe 1, thereby bringing the male thread portion shoulder surface 43 into contact with the female thread portion shoulder surface 53. This allows for a higher torque during fastening. In addition, the positional relationship between the male thread portion 40 and the female thread portion 50 in the fastened state can be stabilized.

[0084] Furthermore, the male thread contact surface 400 of the male thread portion 40 includes at least the external thread portion 41. That is, the male thread contact surface 400 may also include the external thread portion 41 but exclude the male thread sealing surface 42 and the male thread shoulder surface 43. Alternatively, the male thread contact surface 400 may include the external thread portion 41 and the male thread shoulder surface 43 but exclude the male thread sealing surface 42. Alternatively, the male thread contact surface 400 may include the external thread portion 41 and the male thread sealing surface 42 but exclude the male thread shoulder surface 43.

[0085] [Regarding the structure of the female fastener 50]

[0086] Figure 6 yes Figure 4 A cross-sectional view of the portion near the female threaded portion 50 of the oil well metal pipe 1, shown, parallel to the pipe axis direction of the oil well metal pipe 1. Figure 6 The dashed line indicates the structure of the male thread 40 of the other oil well metal pipe 1 when it is fastened to other oil well metal pipes 1. (Refer to...) Figure 6 The female thread 50 includes a female thread contact surface 500 on the inner circumferential surface of the second end 10B of the pipe body 10. When fastened to other oil well metal pipes 1, the female thread contact surface 500 is screwed into by the male thread 40 of the other oil well metal pipe 1 and contacts the male thread contact surface 400 of the male thread 40.

[0087] The female thread contact surface 500 includes at least an internal thread portion 51 formed on the inner circumferential surface of the second end 10B. During tightening, the internal thread portion 51 engages with the external thread portion 41 of the male thread portion 40 of the other well metal pipe 1.

[0088] Alternatively, the female snap-fit ​​contact surface 500 may also include a female snap-fit ​​sealing surface 52 and a female snap-fit ​​shoulder surface 53. Figure 6 In this design, the female thread sealing surface 52 is positioned on the inner circumferential surface of the second end 10B, closer to the tube body 10 than the internal thread portion 51. That is, the female thread sealing surface 52 is positioned between the internal thread portion 51 and the female thread shoulder surface 53. The female thread sealing surface 52 is tapered. Specifically, in the female thread sealing surface 52, along the length direction (tube axis direction) of the second end 10B, the inner diameter gradually decreases from the internal thread portion 51 toward the female thread shoulder surface 53.

[0089] When fastened to other oil well metal pipes 1, the sealing surface 52 of the female thread portion comes into contact with the sealing surface 42 of the male thread portion 40 of the other oil well metal pipe 1. More specifically, during fastening, by screwing the male thread portion 40 of the other oil well metal pipe 1 into the female thread portion 50, the sealing surface 52 of the female thread portion comes into contact with the sealing surface 42 of the male thread portion, and by further screwing, the sealing surface 52 of the female thread portion and the sealing surface 42 of the male thread portion are tightly fitted together. Thus, during fastening, the sealing surface 52 of the female thread portion and the sealing surface 42 of the male thread portion are tightly fitted together to form a seal based on metal-metal contact. Therefore, in the mutually fastened oil well metal pipes 1, air tightness can be improved.

[0090] exist Figure 6In the female threaded portion 50, the female threaded portion shoulder surface 53 is positioned closer to the pipe body 10 than the female threaded portion sealing surface 52. That is, in the female threaded portion 50, the female threaded portion shoulder surface 53, the female threaded portion sealing surface 52, and the internal thread portion 51 are sequentially arranged from the center of the pipe body 10 toward the top of the second end 10B. When fastened to other oil well metal pipes 1, the female threaded portion shoulder surface 53 faces and contacts the male threaded portion shoulder surface 43 of the male threaded portion 40 of the other oil well metal pipe 1. More specifically, during fastening, the female threaded portion shoulder surface 53 contacts the male threaded portion shoulder surface 43 by inserting the male threaded portion 40 of the other oil well metal pipe 1 into the female threaded portion 50. This allows for a higher torque during fastening. Furthermore, it stabilizes the positional relationship between the male threaded portion 40 and the female threaded portion 50 in the fastened state.

[0091] The female contact surface 500 includes at least an internal thread portion 51. During tightening, the internal thread portion 51 of the female contact surface 500 corresponds to and contacts the external thread portion 41 of the male contact surface 400. The female sealing surface 52 corresponds to and contacts the male sealing surface 42. The female shoulder surface 53 corresponds to and contacts the male shoulder surface 43.

[0092] When the male thread contact surface 400 includes an external thread portion 41 but excludes the male thread sealing surface 42 and the male thread shoulder surface 43, the female thread contact surface 500 includes an internal thread portion 51 but excludes the female thread sealing surface 52 and the female thread shoulder surface 53. When the male thread contact surface 400 includes an external thread portion 41 and the male thread shoulder surface 43 but excludes the male thread sealing surface 42, the female thread contact surface 500 includes an internal thread portion 51 and the female thread shoulder surface 53 but excludes the female thread sealing surface 52. When the male thread contact surface 400 includes an external thread portion 41 and the male thread sealing surface 42 but excludes the male thread shoulder surface 43, the female thread contact surface 500 includes an internal thread portion 51 and the female thread sealing surface 52 but excludes the female thread shoulder surface 53.

[0093] The male thread contact surface 400 may include multiple external thread portions 41, multiple male thread sealing surfaces 42, and multiple male thread shoulder surfaces 43. For example, at the male thread contact surface 400 of the male thread portion 40, the male thread shoulder surface 43, male thread sealing surface 42, external thread portion 41, male thread sealing surface 42, male thread shoulder surface 43, male thread sealing surface 42, and external thread portion 41 may be arranged sequentially from the top of the first end 10A toward the center of the tube body 10. In this case, at the female thread contact surface 500 of the female thread portion 50, the internal thread portion 51, female thread sealing surface 52, female thread shoulder surface 53, female thread sealing surface 52, internal thread portion 51, female thread sealing surface 52, and female thread shoulder surface 53 may be arranged sequentially from the top of the second end 10B toward the center of the tube body 10.

[0094] exist Figure 5 and Figure 6 The diagram illustrates a so-called advanced connector where the male threaded portion 40 includes an external threaded portion 41, a male threaded portion sealing surface 42, and a male threaded portion shoulder surface 43, and the female threaded portion 50 includes an internal threaded portion 51, a female threaded portion sealing surface 52, and a female threaded portion shoulder surface 53. However, it is also possible, as described above, that the male threaded portion 40 includes the external threaded portion 41 but excludes the male threaded portion sealing surface 42 and the male threaded portion shoulder surface 43. In this case, the female threaded portion 50 includes the internal threaded portion 51 but excludes the female threaded portion sealing surface 52 and the female threaded portion shoulder surface 53. Figure 7 Is with Figure 3 A partial sectional view, including a longitudinal section, of the metal tubing for oil wells in this embodiment with different structures.

[0095] [The case where the metal pipe for oil wells is a single piece]

[0096] Figure 3 , Figure 4 as well as Figure 7 The oil well metal pipe 1 shown is a so-called T&C type oil well metal pipe 1, with the pipe body 10 including the male threaded pipe body 11 and the pipe joint 12. However, the oil well metal pipe 1 of this embodiment may not be T&C type, but may be integral type.

[0097] Figure 8 This is a partial sectional view, including the longitudinal section, of the integral metal pipe 1 for oil wells according to this embodiment. (Refer to...) Figure 8The integral type oil well metal pipe 1 includes a pipe body 10. The pipe body 10 includes a first end 10A and a second end 10B. The first end 10A is located on the side opposite to the second end 10B. As described above, in the T&C type oil well metal pipe 1, the pipe body 10 includes a male threaded pipe body 11 and a pipe connector 12. That is, in the T&C type oil well metal pipe 1, the pipe body 10 is constructed by fastening two separate components (the male threaded pipe body 11 and the pipe connector 12). In contrast, in the integral type oil well metal pipe 1, the pipe body 10 is formed integrally.

[0098] A male threaded portion 40 is formed at the first end 10A of the pipe body 10. During tightening, the male threaded portion 40 is inserted into the female threaded portion 50 of another integral type oil well metal pipe 1 and screwed in, thus tightening the pipe body 1 with the female threaded portion 50. A female threaded portion 50 is formed at the second end 10B of the pipe body 10. During tightening, the male threaded portion 40 of another integral type oil well metal pipe 1 is inserted into the female threaded portion 50 and screwed in, thus tightening the female threaded portion 50 with the male threaded portion 40 of the integral type oil well metal pipe 1.

[0099] The structure of the male thread 40 of the integral metal pipe 1 for oil wells and Figure 5 The male thread 40 of the T&C type oil well metal pipe 1 shown has the same structure. Similarly, the female thread 50 of the integral type oil well metal pipe 1 has the same structure. Figure 6 The structure of the female thread 50 of the T&C type oil well metal pipe 1 shown is the same. Furthermore, in Figure 5 and Figure 6 In the male thread portion 40, a male thread shoulder surface 43, a male thread sealing surface 42, and an external thread portion 41 are sequentially arranged from the top of the first end 10A toward the center of the pipe body 10. Therefore, in the female thread portion 50, an internal thread portion 51, a female thread sealing surface 52, and a female thread shoulder surface 53 are sequentially arranged from the top of the second end 10B toward the center of the pipe body 10. However, similar to the male thread contact surface 400 of the male thread portion 40 of the T&C type oil well metal pipe 1, the male thread contact surface 400 of the integral type oil well metal pipe 1 only needs to include at least the external thread portion 41. Similarly, similar to the female thread contact surface 500 of the female thread portion 50 of the T&C type oil well metal pipe 1, the female thread contact surface 500 of the integral type oil well metal pipe 1 only needs to include at least the internal thread portion 51.

[0100] In summary, the metal pipe 1 for oil wells in this embodiment can be either T&C type or integral type.

[0101] [Resin Coating]

[0102] The oil well metal pipe 1 of this embodiment has a resin coating 100 formed as the uppermost layer of at least one of the male thread contact surface 400 and the female thread contact surface 500. Figure 9 This is a cross-sectional view near the male thread contact surface 400 of the metal pipe 1 for oil wells in this embodiment. Figure 10 Is with Figure 9 A cross-sectional view of the corresponding female buckle contact surface 500.

[0103] Reference Figure 9 The resin coating 100 can also be formed as the uppermost layer of the male snap-fit ​​contact surface 400. In this case, the resin coating 100 may or may not be formed as the uppermost layer of the corresponding female snap-fit ​​contact surface 500. Additionally, refer to... Figure 10 The resin coating 100 may also be formed as the uppermost layer of the female thread contact surface 500. In this case, the resin coating 100 may or may not be formed as the uppermost layer of the corresponding male thread contact surface 400. In summary, the oil well metal pipe 1 of this embodiment has a resin coating 100 formed as the uppermost layer of at least one of the male thread contact surface 400 and the female thread contact surface 500.

[0104] The resin coating 100 contains epoxy resin. If the epoxy resin content in the resin coating 100 is 15% by mass or more, the resin coating 100 can be formed more stably. On the other hand, if the epoxy resin content in the resin coating 100 is 80% by mass or less, the predetermined film thickness can be ensured more stably. Therefore, the epoxy resin content in the resin coating 100 is, for example, 15 to 80% by mass. The lower limit of the epoxy resin content in the resin coating 100 is preferably 18% by mass, more preferably 20% by mass, further preferably 25% by mass, and even more preferably 30% by mass. The upper limit of the epoxy resin content in the resin coating 100 is preferably 70% by mass, more preferably 65% ​​by mass, and even more preferably 60% by mass.

[0105] [Method for determining the content of epoxy resin]

[0106] The epoxy resin content in the resin-coated film 100 was determined using reflux extraction (Soxhlet extraction), which employed a solvent. Specifically, methyl ethyl ketone (MEK) was used as the solvent for reflux extraction of the resin-coated film 100. Specifically, the required amount of resin-coated film 100 was cut from either the male contact surface 400 or the female contact surface 500 and subjected to reflux extraction. Five sheets of resin-coated film 100, each 20 μm thick, 120 mm long, and 15 mm wide, were reflux-extracted for 4 hours using 0.4 L of MEK. If the thickness of the resin-coated film 100 was greater than 20 μm, the number of sheets was adjusted to achieve the same volume as the resin-coated film 100 described above. Similarly, if the thickness of the resin-coated film 100 was less than 20 μm, the number of sheets was also adjusted to achieve the same volume as the resin-coated film 100 described above. The weight of the resin coating 100 after reflux extraction is equivalent to the weight of the epoxy resin. Therefore, the epoxy resin content in the resin coating 100 can be determined by dividing the weight of the resin coating 100 after reflux extraction by the weight of the resin coating 100 before reflux extraction.

[0107] [Relaxation time of pulsed NMR]

[0108] In 1 The resin coating 100 was measured using pulsed nuclear magnetic resonance (NMR). When the obtained free-induction decay signals were sequentially divided into three components—high-motor component, medium-motor component, and low-motor component—starting from the component with the longest spin-spin relaxation time T2, the weighted average of the spin-spin relaxation time T2 for the three components was less than 110.0 μs. As mentioned above, the shorter the relaxation time obtained by pulsed NMR, the higher the crosslinking density. Increasing the crosslinking density of the resin coating 100 increases the shoulder friction torque ΔT. In this case, the high-torque performance of the oil well metal pipe 1 is improved.

[0109] The lower limit of the weighted average value of the spin-spin relaxation time T2 of the resin coating 100 is not particularly limited, for example, it is 0.5 μs. The lower limit of the weighted average value of the spin-spin relaxation time T2 of the resin coating 100 is preferably 3.0 μs, more preferably 5.0 μs, further preferably 10.0 μs, further preferably 15.0 μs, further preferably 20.0 μs, and further preferably 25.0 μs. The upper limit of the weighted average value of the spin-spin relaxation time T2 of the three components is preferably 100.0 μs, more preferably 90.0 μs, further preferably 80.0 μs, further preferably 70.0 μs, further preferably 60.0 μs, further preferably 50.0 μs, and further preferably 45.0 μs.

[0110] [Ratio of active ingredients]

[0111] Preferably, in the case of 1 When the resin coating 100 is measured by H-pulse NMR, the ratio of the medium-mobility component to the sum of the high-mobility, medium-mobility, and low-mobility components is higher than the ratio of the low-mobility component to the sum of the high-mobility, medium-mobility, and low-mobility components. The distance between crosslinking points of the molecular chains of the medium-mobility component is larger than that of the molecular chains of the low-mobility component. In other words, the crosslinking density of the medium-mobility component is smaller than that of the low-mobility component. Therefore, compared with the low-mobility component, the medium-mobility component has less constraint caused by crosslinking. Compared with the low-mobility component, the molecular chains of the medium-mobility component are more prone to deformation and elongation under the stronger shear stress during thread tightening and loosening. If the ratio of the medium-mobility component is higher than that of the low-mobility component, the resin coating 100 is more prone to shear deformation, thus making it easier to suppress the peeling of the resin coating 100.

[0112] [Methods for determining relaxation time in pulsed NMR]

[0113] The weighted average of the spin-spin relaxation time T2 of the resin coating 100 was determined as follows: The decay curve (free induction decay signal) of the magnetization of the resin coating 100 was obtained using pulsed NMR spectroscopy with a nuclear magnetic resonance (NMR) apparatus. Specifically, an NMR apparatus with an observation frequency of 20 MHz was used. The determination was performed using the following methods: solid echo method, observation nucleus: 1H. Measurement objects: Spin-spin relaxation time T2 (μs), pulse amplitude: 2.50–3.50 μs, pulse interval: 5.00–15.00 μs, repetition time: 4 seconds, cumulative number of times: 32, measurement temperature: 35℃. The least squares method was used to ensure the obtained decay curve matched the fitted curve. The Lorentz function was used for the linear portion, and the Gaussian function for the curved portion. From the fitted curve, components with longer spin-spin relaxation times T2 were subtracted sequentially. Thus, the waveform was separated into three components: a high-motion component with relatively high motion, a medium-motion component with relatively moderate motion, and a low-motion component with relatively low motion. The spin-spin relaxation times T2 of the high-motion component, the medium-motion component, and the low-motion component were calculated. Calculate the ratio of the highly mobile component to the sum of the highly mobile, moderately mobile, and lowly mobile components; the ratio of the moderately mobile component to the sum of the highly mobile, moderately mobile, and lowly mobile components; and the ratio of the lowly mobile component to the sum of the highly mobile, moderately mobile, and lowly mobile components. Multiply the spin-spin relaxation time T2 of each component by its respective ratio. Summate the spin-spin relaxation times T2 multiplied by the ratios of each component to obtain a weighted average of the spin-spin relaxation times T2.

[0114] [Lubricating materials]

[0115] The resin coating 100 may also contain a lubricating material. The lubricating material is sufficient to improve the lubricity of the resin coating 100 and is not particularly limited. Examples of lubricating materials include one or more selected from the group consisting of graphite, zinc oxide, boron nitride, talc, molybdenum disulfide, tungsten disulfide, fluorinated graphite, tin sulfide, bismuth sulfide, organomolybdenum, thiosulfate, polytetrafluoroethylene (PTFE), melamine cyanurate (MCA), and perfluoropolyether (PFPE). The total content of the lubricating material in the resin coating 100 is, for example, 0.1–25% by mass.

[0116] [Other Materials]

[0117] The resin coating 100 may also contain other materials. These other materials may be one or more selected from the group consisting of pigments, rust-inhibiting additives, and corrosion inhibitors. The content of these other materials in the resin coating 100 may be, for example, 0.1% to 25% by mass.

[0118] [Thickness of resin coating]

[0119] The thickness of the resin coating 100 is not particularly limited. For example, the thickness of the resin coating 100 is 1 to 100 μm.

[0120] [Other layers]

[0121] In this embodiment, the oil well metal pipe 1 may also have another layer 80 between at least one of the male thread contact surface 400 and the female thread contact surface 500 and the uppermost resin coating 100. (Refer to...) Figure 11 Alternatively, another layer 80 may be provided below the uppermost resin film 100, i.e., between the male fastener contact surface 400 and the resin film 100. (Refer to...) Figure 12 Alternatively, another layer 80 may be provided in the lower layer of the resin coating 100, that is, between the contact surface 500 of the female buckle and the uppermost resin coating 100.

[0122] Other layers 80 may be one or more selected from the group consisting of phosphate coating, plating, chromate coating, and zirconium coating. Phosphate coating may be selected from the group consisting of zinc phosphate coating, manganese phosphate coating, calcium phosphate coating, and iron phosphate coating. Multiple other layers 80 may also be stacked radially in the well tubing. For example, a plating may be disposed on the male thread contact surface 400, a chromate coating may be disposed on the plating, and a resin coating 100 may be disposed on the chromate coating as the uppermost layer.

[0123] [Chemical composition of tube body 10]

[0124] The chemical composition of the pipe body 10 of the oil well metal pipe 1 in this embodiment is not particularly limited. The pipe body 10 may be formed of, for example, carbon steel, stainless steel, or alloy steel. The oil well metal pipe 1 may also be a steel pipe including Fe-based alloys or an alloy pipe represented by Ni-based alloy pipes. Among these, the steel pipes may be, for example, low-alloy steel pipes, martensitic stainless steel pipes, duplex stainless steel pipes, etc. Among alloy steels, high-alloy steels such as duplex stainless steel containing Ni alloys and alloying elements such as Cr, Ni, and Mo have high corrosion resistance. Therefore, if these high-alloy steels are used as the pipe body 10, excellent corrosion resistance can be obtained in corrosive environments containing hydrogen sulfide, carbon dioxide, etc.

[0125] [Manufacturing Method]

[0126] The following describes the manufacturing method of the metal pipe 1 for oil wells according to this embodiment.

[0127] The manufacturing method of the metal pipe 1 for oil wells in this embodiment includes a preparation step, a composition coating step, and a composition curing step.

[0128] [Preparation Process]

[0129] In the preparation process, an oil well metal pipe 1 with a pipe body 10 is prepared. The pipe body 10 includes a male thread portion 40 and a female thread portion 50. The male thread portion 40 has a male thread contact surface 400 including an external thread portion 41, and the female thread portion 50 has a female thread contact surface 500 including an internal thread portion 51. As described above, the oil well metal pipe 1 of this embodiment has a well-known structure. That is, in the preparation process, it is sufficient to prepare an oil well metal pipe 1 with a well-known structure.

[0130] [Composition Application Process]

[0131] In the composition coating process, the epoxy resin-containing composition is coated as the uppermost layer of at least one of the male contact surface 400 and the female contact surface 500. The composition is used to form the resin coating 100 described above. There is no particular limitation on the method of setting the weighted average of the spin-spin relaxation time T2 of the resin coating 100 to 110.0 μs or less. For example, the composition used to form the resin coating 100 contains an epoxy resin, an acrylate curing agent containing unsaturated bonds, and an nitrogen-containing catalyst. The acrylate curing agent containing unsaturated bonds is, for example, selected from the group consisting of 2-ethylhexyl 3-(4-methoxyphenyl)acrylate, ethyl 3-(4-methoxyphenyl)acrylate, isoamyl 4-methoxycinnamate, and isopropyl cinnamate. The nitrogen-containing catalyst is, for example, selected from the group consisting of 2-methylpyrazine, 2,5-dimethylpyrazine, 3,5-dimethylpyridine, and 3-quinol. As another method, the composition used to form the resin coating 100 contains an epoxy resin, an acrylate curing agent containing unsaturated bonds, and a nitrile curing agent. The acrylate curing agent containing unsaturated bonds is, for example, selected from the group consisting of 2-ethylhexyl 3-(4-methoxyphenyl)acrylate, ethyl 3-(4-methoxyphenyl)acrylate, isoamyl 4-methoxycinnamate, and isopropyl cinnamate. The nitrile curing agent is, for example, selected from the group consisting of 4-methyl-2-oxopentanonitrile, ethyl cyanoacetate, dimethylmalononitrile, 2-methyl-2-phenylpropionitrile, and 4,4-dimethyl-3-oxopentanonitrile. For example, if the composition used to form the resin coating 100 has the above-described composition, the weighted average value of the spin-spin relaxation time T2 of the resin coating 100 can be adjusted to 110.0 μs or less. The composition used to form the resin coating 100 may also contain a solvent as needed. The solvent is, for example, one or more selected from the group consisting of water, alcohol, and organic solvents. Solvents may also contain trace amounts of surfactants. There is no particular limitation on the proportion of solvent. For example, when the total components excluding the solvent are set at 100% by mass, the proportion of solvent is 40% to 100% by mass.

[0132] Hereinafter, the composition used to form the resin coating 100 will also be referred to simply as the composition. The method of applying the composition to at least one of the male contact surface 400 and the female contact surface 500 is not particularly limited, and any well-known method may be used. For example, the composition in a solution state can be applied to at least one of the male contact surface 400 and the female contact surface 500 by spraying. In this case, the viscosity is adjusted so that the composition can be sprayed under normal temperature and pressure. The method of applying the composition to at least one of the male contact surface 400 and the female contact surface 500 can also be brushing or dipping instead of spraying.

[0133] [Composition Curing Process]

[0134] In the composition curing process, the applied composition is cured to form a resin film 100. For example, the composition is cured at 5 to 30°C for 3 to 16 hours, or at 30 to 70°C for 5 to 180 minutes.

[0135] The metal pipe 1 for oil wells of this embodiment can be manufactured using the manufacturing method described above.

[0136] [Other processes]

[0137] The oil well metal pipe 1 of this embodiment may also include other processes in the manufacturing process. Other processes are, for example, one or more selected from the group consisting of phosphate coating formation process, plating process, chromate coating formation process, zirconium coating formation process, and sandblasting treatment.

[0138] [Phosphate coating formation process]

[0139] In the phosphate coating formation process, at least one of the male thread contact surface 400 and the female thread contact surface 500 of the oil well metal pipe 1 is subjected to phosphate chemical conversion treatment to form a phosphate coating. As the treatment fluid for the phosphate chemical conversion treatment, a well-known phosphate chemical conversion treatment fluid can be used. For example, a zinc phosphate chemical conversion treatment fluid containing 1-150 g / L phosphate ions, 0.5-30 g / L zinc ions, 1-100 g / L nitrate ions, 0-10 g / L nickel ions, and 0-10 g / L manganese ions can be used. A manganese phosphate chemical conversion treatment fluid commonly used for oil well metal pipe 1 can also be used. The temperature of the phosphate chemical conversion treatment fluid is, for example, room temperature to 95°C. The treatment time for the phosphate chemical conversion treatment can be appropriately set according to the desired film thickness, for example, 0.5-15 minutes.

[0140] [Plating Process]

[0141] In the plating process, at least one of the male thread contact surface 400 and the female thread contact surface 500 of the oil well metal pipe 1 is plated to form a coating. The plating process can be performed using well-known methods. For example, electroplating.

[0142] When forming a Zn-Ni alloy coating, the plating bath contains zinc and nickel ions. The composition of the plating bath is, for example, Zn: 1–100 g / L and Ni: 1–50 g / L. The electroplating conditions can be appropriately set. For example, the pH of the plating bath can be set to 1–10, the temperature to 30–80°C, and the current density to 1–100 A / dm³. 2 The plating process is carried out by setting the processing time to 0.1 to 30 minutes.

[0143] [Chromate Coating Formation Process]

[0144] In the chromate coating formation process, at least one of the male thread contact surface 400 and the female thread contact surface 500 of the oil well metal pipe 1 is subjected to chromate treatment to form a chromate coating. A well-known chromate treatment solution can be used as the treatment solution. The temperature of the chromate treatment solution is, for example, room temperature to 95°C. The treatment time for the chromate treatment can be appropriately set according to the desired film thickness, for example, 0.5 to 15 minutes.

[0145] [Zirconium Coating Formation Process]

[0146] In the zirconium coating formation process, a zirconium chemical conversion treatment is performed on the oil well metal pipe 1 to form a zirconium oxide coating. The zirconium chemical conversion treatment can be performed using well-known methods. For example, the zirconium chemical conversion treatment can also be performed by immersing at least one of the male thread contact surface 400 and the female thread contact surface 500 in a treatment solution. Alternatively, the zirconium chemical conversion treatment can be performed by spraying water onto at least one of the male thread contact surface 400 and the female thread contact surface 500. Furthermore, commercially available treatment solutions can be used for the zirconium chemical conversion treatment. Additionally, the treatment conditions in the zirconium coating formation process can be appropriately set. For example, the concentration of the treatment solution can be set to 3–20 g / L, the temperature of the treatment solution can be set to 20–45°C, and the treatment time can be set to 30–240 seconds to perform the zirconium chemical conversion treatment.

[0147] The oil well metal pipe 1 of this embodiment is manufactured using the above-described process. However, the above-described manufacturing method is only one example of the manufacturing method of the oil well metal pipe 1 of this embodiment, and is not limited to this manufacturing method. The oil well metal pipe 1 of this embodiment can also be manufactured using other methods.

[0148] Example

[0149] The effects of the metal pipe for oil wells according to this embodiment will be further explained in detail below using examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effects of the metal pipe for oil wells according to this embodiment. Therefore, the metal pipe for oil wells according to this embodiment is not limited to this one example of conditions.

[0150] Commercially available cold-rolled steel sheet was used for the main body of the metal pipe intended for oil wells. The cold-rolled steel sheet measures 150 mm in length and 70 mm in width. The steel grade is SPCC steel as specified in JIS G 3141 (2021).

[0151] [Composition Application Process]

[0152] Compositions were applied to the surface of cold-rolled steel sheets. Composition #1 contained epoxy resin, 2-ethylhexyl 3-(4-methoxyphenyl)acrylate, 2-methylpyrazine, and water as a solvent. Composition #2 contained epoxy resin, 2-ethylhexyl 3-(4-methoxyphenyl)acrylate, 4-methyl-2-oxopentanilonitrile, and water as a solvent. Composition #3 contained epoxy resin, 2-ethylhexyl 3-(4-methoxyphenyl)acrylate, 3,5-dimethylpyridine, and water as a solvent. Composition #4 contained epoxy resin. However, composition #4 did not contain any of the following: an acrylate curing agent containing unsaturated bonds, a nitrogen-containing catalyst, or a nitrile curing agent. Composition #5 contained epoxy resin and 2-ethylhexyl 3-(4-methoxyphenyl)acrylate. However, composition #5 did not contain any of the following: a nitrogen-containing catalyst or a nitrile curing agent.

[0153] [Composition Curing Process]

[0154] The compositions for each test number were then cured. Specifically, cold-rolled steel sheets coated with the compositions were heated in a furnace at 50–70°C for 5 minutes. This resulted in the formation of a resin coating.

[0155] [Experimental study on relaxation time of pulsed NMR]

[0156] The weighted average of the spin-spin relaxation time T2 of the resin coating for each test number was obtained as follows: Using an NMR apparatus (Brook Nippon, Minispec MQ20 ​​(20MHz)), the decay curves of the magnetization intensity of the resin coating (free induction decay signal) were obtained using pulsed NMR. Specifically, the observation frequency was 20MHz, the measurement method was Solid echo method, and the observation nucleus was... 1H. Measurement conditions: Spin-spin relaxation time T2 (μs), pulse amplitude: 3.06 μs, pulse interval: 10.00 μs, repetition time: 4 seconds, cumulative number of times: 32, measurement temperature: 35℃. The least squares method was used to ensure the obtained decay curve matched the fitted curve. The Lorentz function was used for the linear portion, and the Gaussian function for the curved portion. The components with longer spin-spin relaxation times T2 were subtracted sequentially from the fitted curve. This separated the waveform into three components: a high-motion component with relatively high motion, a medium-motion component with relatively moderate motion, and a low-motion component with relatively low motion. The spin-spin relaxation times T2 of the high-motion component, the medium-motion component, and the low-motion component were then determined. Calculate the ratio of the highly mobile component to the sum of the highly mobile, moderately mobile, and lowly mobile components; the ratio of the moderately mobile component to the sum of the highly mobile, moderately mobile, and lowly mobile components; and the ratio of the lowly mobile component to the sum of the highly mobile, moderately mobile, and lowly mobile components. Multiply the spin-spin relaxation time T2 of each component by its ratio. Summate the spin-spin relaxation times T2 multiplied by the ratios of each component and calculate the weighted average of the spin-spin relaxation times T2. The results are shown in Table 1.

[0157] [Table 1]

[0158] Table 1

[0159]

[0160] [Shoulder Friction Torque Measurement Test]

[0161] Bowden sliding tests were conducted on cold-rolled steel sheets with resin coating at various test numbers under the following conditions. A Bowden sliding tester manufactured by Kobe Steel Corporation was used, with the following conditions: steel ball: 3 / 16” SUJ2; load: 3 kgf; sliding width: 10 mm; sliding speed: 4 mm / s; lubricant: none; test temperature: room temperature (25°C). One reciprocating sliding motion was defined as one cycle, and the arithmetic mean of the friction coefficients from the first to the fifth cycle was defined as the initial friction coefficient. Using the initial friction coefficient, the shoulder torque and yield torque were determined using FEM analysis. In the FEM analysis, a... Figure 3 , Figure 5 as well as Figure 6The structure shown is a metal pipe for oil wells with an outer diameter of 9”-5 / 8” and a yield strength of 552-655 MPa. The male thread contact surface includes the external thread, the male thread sealing surface, and the male thread shoulder surface. The female thread contact surface includes the internal thread, the female thread sealing surface, and the female thread shoulder surface. In the FEM analysis, it is assumed that a resin coating is formed only on the male thread contact surface. The shoulder friction torque ΔT is obtained by subtracting the shoulder torque from the yield torque obtained in the FEM analysis. The results are shown in Table 1.

[0162] [Evaluation Results]

[0163] Referring to Table 1, the resin coatings in tests 1 through 3 contain epoxy resin. 1 The weighted average of the spin-spin relaxation times T2 obtained by H-pulse NMR for the high-motor, medium-motor, and low-motor components was below 110.0 μs. As a result, compared to the shoulder friction torque ΔT of the resin-coated components in experiments 4 and 5, the shoulder friction torque ΔT of the resin-coated components in experiments 1 to 3 was higher. The resin coatings in experiments 1 to 3 can improve the high-torque performance of metal tubing used in oil wells.

[0164] On the other hand, test numbers 4 and 5 were... 1 The weighted average of the spin-spin relaxation times T2 obtained by H-pulse NMR for the high-motor, medium-motor, and low-motor components exceeded 110.0 μs. As a result, compared to the shoulder friction torque ΔT of the resin-coated materials in tests 1–3, the shoulder friction torque ΔT of the resin-coated materials in tests 4 and 5 was lower. Therefore, the resin-coated materials in tests 4 and 5 could not improve the high-torque performance of metal tubing for oil wells.

[0165] The embodiments of this disclosure have been described above. However, the above embodiments are merely illustrative examples for implementing this disclosure. Therefore, this disclosure is not limited to the above embodiments, and can be implemented by appropriately modifying the above embodiments without departing from its spirit.

[0166] Explanation of reference numerals in the attached figures

[0167] 1. Metal pipe for oil wells; 10. Pipe body; 10A. First end; 10B. Second end; 11. Male thread section of pipe body; 12. Pipe fitting; 40. Male thread section; 41. External thread section; 42. Male thread section sealing surface; 43. Male thread section shoulder surface; 50. Female thread section; 51. Internal thread section; 52. Female thread section sealing surface; 53. Female thread section shoulder surface; 100. Resin coating; 400. Male thread section contact surface; 500. Female thread section contact surface.

Claims

1. A metal pipe for oil wells, comprising a pipe body including a first end and a second end. The pipe body includes: The male fastener is formed at the first end; and The female buckle portion is formed at the second end. The male thread portion has a male thread contact surface including an external thread portion. The female threaded portion has a female threaded portion contact surface. The oil well metal pipe also has a resin coating formed as the uppermost layer of at least one of the male thread contact surface and the female thread contact surface. The resin coating contains epoxy resin. In 1 The resin coating was measured by H-pulse NMR. When the obtained free induction decay signal was divided into three components in sequence from the component with long spin-spin relaxation time (T2): high-motor component, medium-motor component, and low-motor component, the weighted average value of the spin-spin relaxation time (T2) of the three components was less than 110.0 μs.

2. The metal pipe for oil wells according to claim 1, wherein, In the above 1 When the resin coating is measured by H-pulse NMR, the ratio of the medium-motor component to the sum of the high-motor component, the medium-motor component, and the low-motor component is higher than the ratio of the low-motor component to the sum.

3. The metal pipe for oil wells according to claim 1 or 2, wherein, At least one of the male buckle contact surface and the female buckle contact surface is further provided with one or more of the following in the group consisting of phosphate coating, plating, chromate coating and zirconium coating between it and the resin coating.

Citation Information

Patent Citations

  • Screw joint for steel pipe

    JP2002348587A

  • Threaded joint for steel pipes

    WO2006104251A1

  • Threaded joint for pipe and method for producing threaded joint for pipe

    CN110651147A