A gas-phase thermochemical synthesis of core-shell structure of zero-valent iron nitride material and its preparation method and application
The preparation of core-shell structured zero-valent iron nitride by gas-phase thermochemical synthesis solves the safety hazards and high energy consumption problems of existing methods, and achieves efficient removal of chlorinated hydrocarbon pollutants, which is suitable for groundwater remediation.
Patent Information
- Application Number
- CN202411596925.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-11-11
AI Technical Summary
Existing methods for preparing zero-valent iron nitride have safety hazards, high energy consumption, and low activity, making it difficult to effectively remove chlorinated hydrocarbon organic pollutants.
A gas-phase thermochemical synthesis method was adopted, in which melamine and iron powder were calcined at high temperature in a quartz tube to generate a core-shell structured zero-valent iron nitride material, in which the core is zero-valent iron and the outer shell is Fe4.4N. The ammonia gas generated by the decomposition of melamine is used to form an iron-nitrogen compound layer on the surface of the zero-valent iron, which improves electron transfer efficiency and hydrophobicity.
The prepared core-shell structured zero-valent iron nitride material has high electronic efficiency, can effectively remove chlorinated hydrocarbon pollutants, is easy to operate, and is suitable for in-situ remediation of groundwater.
Smart Images

Figure CN119461622B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of environmental remediation technology, specifically to a core-shell structured zero-valent iron nitride material synthesized by gas-phase thermochemical synthesis, its preparation method, and its application. Background Technology
[0002] Zero-valent iron (Fe) 0 It is abundant and inexpensive, and has strong reducing properties (Fe). 2+ +2e - →Fe(s), E0=-0.44V) and its adsorption properties are widely used in environmental pollution control, and groundwater in-situ remediation technology based on zero-valent iron has received widespread attention both domestically and internationally. However, zero-valent iron is prone to passivation by reacting with water, forming an iron oxide protective layer. When zero-valent iron removes pollutants from groundwater, it first loses electrons and is oxidized. Some of the electrons donated are used for pollutant removal, while others are gained by protons (H) in the water, generating non-toxic, colorless, and odorless hydrogen gas (H2). The generation of H2 reduces the efficiency of zero-valent iron in removing pollutants to some extent. Simultaneously, nano-zero-valent iron, due to its magnetism and high surface energy, easily aggregates into large particles, losing its underground mobility; its activity is high but its lifespan is short, making it unable to continuously degrade pollutants; the dense oxide film formed on the surface of zero-valent iron greatly hinders the contact between active ingredients and target pollutants, thus reducing the activity of zero-valent iron.
[0003] In recent years, numerous studies have demonstrated that doping with heteroatoms of different electronegativity (e.g., S, C, N, or P) is an effective method for readjusting the distribution of delocalized electrons around the d orbitals of Fe atoms. For decades, iron nitride has been used in various research fields as a highly corrosion-resistant material and electrochemical catalyst. Due to the higher electronegativity of N and its more significant electron shuttle effect than S, nitriding modification of zero-valent iron surfaces has gradually become a novel approach to modifying zero-valent iron. Studies have shown that nitriding modification of the surface of zero-valent iron can give it the following advantages: (1) It can form an iron-nitrogen compound layer on the surface of zero-valent iron to replace the original oxide layer. Since the iron-nitrogen compound has excellent electronic conductivity compared with the original iron oxide layer on the surface of zero-valent iron, it can facilitate the transfer of electrons donated by the zero-valent iron core and overcome the disadvantage of low activity of zero-valent iron; (2) The iron-nitrogen compound also has good hydrophobicity, which is conducive to the adhesion of chlorinated hydrocarbon oily organic matter, thereby promoting the contact between pollutants and their active sites. The electrons donated by the zero-valent iron core are also more easily transferred selectively to the target pollutants through the iron-nitrogen compound layer, thereby degrading the target pollutants; (3) The nitrogen element in the iron-nitrogen compound can inhibit H3O + It gains electrons and forms hydrogen gas, thus greatly suppressing the growth of H3O. + It competes with the target pollutant for electrons, thereby increasing the electron efficiency of zero-valent iron.
[0004] Currently, the main existing method for preparing zero-valent iron nitride nanoparticles is the thermochemical ammonia synthesis method (Brumovsky M, Oborna J, Micic V, et al. Iron Nitride Nanoparticles for Enhanced Reductive Dechlorination of Trichloroethylene[J]. Environ Sci Technol, 2022, 56(7):4425-4436.), and the configuration of the iron nitride is Fe. 2-3 N and Fe4N; and ball milling (Gong L, Qiu X, Tratnyek PG, et al. FeN(x)(C)-Coated Microscale Zero-Valent Iron for Fast and Stable Trichloroethylene Dechlorination in both Acidic and Basic pH Conditions[J].Environ Sci Technol,2021,55(8):5393-5402.) The combined forms of nitrogen are pyridine nitrogen, pyrrole nitrogen and graphene nitrogen. However, there are the following shortcomings: (1) The current gas-phase thermochemical synthesis method uses ammonia gas for synthesis. Ammonia gas is not easy to store and transport and is toxic and prone to explosion, posing a safety hazard; (2) The ball milling synthesis method has high energy consumption and is difficult to reach the nanoscale, affecting the degradation rate; (3) The configuration of iron nitride is Fe 2-3 N and Fe4N, as well as their single compound forms, are pyridine nitrogen, pyrrole nitrogen, and graphene nitrogen, and their modified zero-valent iron has low activity.
[0005] Therefore, considering the current research status, it is necessary to explore new methods for preparing zero-valent iron nitride in order to solve the above-mentioned technical problems. Summary of the Invention
[0006] This invention provides a core-shell structured zero-valent iron nitride material synthesized by gas-phase thermochemical synthesis, its preparation method, and its applications. The obtained core-shell structured zero-valent iron nitride material has a core of zero-valent iron and an outer shell of Fe. 4.4 Compared to existing zero-valent iron nitride materials, nitrogen is less prone to oxidation, and the resulting zero-valent iron nitride exhibits higher removal efficiency for chlorinated hydrocarbon organic pollutants. Furthermore, the gas-phase thermochemical synthesis method provided by this invention is simple to operate, has a short preparation cycle, and is more readily applicable to practical engineering projects.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] This invention provides a core-shell structured zero-valent iron nitride material synthesized by gas-phase thermochemical synthesis. The core of the core-shell structured zero-valent iron nitride material is zero-valent iron, and the outer shell is Fe. 4.4 N; The zero-valent iron content is 60-70 wt% based on the mass of the core-shell structured zero-valent iron nitride material.
[0009] This invention also provides a method for preparing a core-shell structured zero-valent iron nitride material by gas-phase thermochemical synthesis, comprising: placing iron powder and melamine in a quartz tube with a partition plate, wherein the partition plate divides the quartz tube into a space for holding iron powder and a space for holding melamine, the space for holding iron powder and the space for holding melamine being interconnected; vacuum sealing the quartz tube, and then calcining the quartz tube containing iron powder and melamine at a temperature above 350°C to obtain the core-shell structured zero-valent iron nitride material.
[0010] Melamine decomposes and releases ammonia gas at temperatures slightly above 350°C (at this temperature, ammonia is the only gaseous product of melamine decomposition). Ammonia can react with the oxide layer (Fe) on the surface of zero-valent iron particles. x O y Or part of the near-outer Fe layer 0 The reaction generates an iron-nitrogen compound layer, which replaces the surface oxide layer of zero-valent iron particles. The superior conductivity of iron nitride accelerates the rate at which the core zero-valent iron transfers electrons to the target pollutants. Furthermore, iron nitride exhibits good hydrophobicity and a strong affinity for hydrophobic pollutants such as chlorinated hydrocarbons, thereby enhancing its performance in degrading these pollutants. On the other hand, the presence of iron nitride can inhibit the hydrogen evolution reaction between zero-valent iron materials and water molecules, weakening the competition for electrons between water molecules and pollutants, thus increasing the electron efficiency of zero-valent iron.
[0011] Preferably, the mass ratio of melamine to iron powder is 0.5 to 3:1.
[0012] More preferably, the mass ratio of melamine to iron powder is 1 to 3:1.
[0013] More preferably, the mass ratio of melamine to iron powder is 1 to 2:1.
[0014] More preferably, the mass ratio of melamine to iron powder is 1 to 1.5:1.
[0015] Preferably, the particle size of the iron powder is 50–800 nm.
[0016] Under these conditions, the relative content of zero-valent iron inside the generated zero-valent iron nitride is appropriate, and the zero-valent iron nitride has a better removal effect on chlorinated hydrocarbon organic pollutants.
[0017] More preferably, the particle size of the iron powder is 100-500 nm.
[0018] More preferably, the particle size of the iron powder is 100-300 nm.
[0019] More preferably, the iron powder has a particle size of 100 nm.
[0020] Preferably, one end of the partition plate is connected to the quartz tube, and the length of the partition plate is 1 / 5 to 1 / 2 of the inner diameter of the quartz tube.
[0021] Preferably, after vacuum sealing, the vacuum degree inside the quartz tube is ≥0.1 MPa.
[0022] Preferably, the calcination specifically involves calcining at 350–400°C for 20–30 minutes, followed by calcination at 400–600°C for 60–120 minutes.
[0023] More preferably, the calcination specifically involves calcining at 350–360°C for 20–30 minutes, followed by calcination at 500–600°C for 80–120 minutes.
[0024] Preferably, the heating rate to 350–400°C is 1–5°C / min; and the heating rate to 400–600°C is 2–3°C / min.
[0025] More preferably, the heating rate to 350–360°C is 1–3°C / min; and the heating rate to 500–600°C is 2°C / min.
[0026] When the iron nitride layer in a core-shell structured zero-valent iron nitride material is too thick, although the electron efficiency of the zero-valent iron nitride can approach 100%, it will lead to a decrease in the relative content of zero-valent iron inside the material particles. Since the zero-valent iron inside the particles is the only electron donor for degrading pollutants, too low a content of zero-valent iron will affect its reactivity.
[0027] Therefore, in the parameter settings of the nitriding process, the calcination temperature, calcination time, heating rate, particle size of iron powder, and the ratio of melamine to iron powder will all affect the thickness of the nitrided iron layer. For example, if the calcination time is too long, the heating rate is too fast, the particle size of iron powder is too small, or the ratio of melamine to iron powder is too high, the degree of nitriding will be too high, thus affecting the degradation rate.
[0028] This invention also provides the application of the above-mentioned core-shell structured zero-valent iron nitride material or the core-shell structured zero-valent iron nitride material prepared by the above-mentioned preparation method in the in-situ remediation of groundwater containing chlorinated hydrocarbon organic pollutants.
[0029] Preferably, the chlorinated hydrocarbon organic pollutant is one or more of trichloroethylene, tetrachloroethylene, trichloroethane, tetrachloroethane, chloromethane, dichloromethane, trichloromethane, carbon tetrachloride, trichloropropane, and hexachlorobutadiene.
[0030] Therefore, the present invention has the following beneficial effects:
[0031] (1) This invention utilizes a core-shell structured nitrided nanomaterial of zero-valent iron obtained through gas-phase chemical thermal synthesis, with a zero-valent iron core and Fe... 4.4 N represents the outer shell; the resulting core-shell structured nitrided nano-zero-valent iron material possesses a more stable surface iron-nitrogen compound, higher electronic efficiency, and can overcome the rapid passivation problem of nano-zero-valent iron during the repair process.
[0032] (2) The present invention uses ammonia gas generated during the calcination of melamine as the synthesis introduction gas, which avoids the disadvantages of ammonia gas being difficult to transport and store and prone to explosion in the existing gas phase synthesis method.
[0033] (3) The gas-phase thermochemical synthesis method provided by the present invention is simple to operate, has a short preparation cycle, and is more likely to meet the application needs of practical engineering.
[0034] (4) The core-shell nitrided nano-zero-valent iron material obtained by the present invention has high removal efficiency for chlorinated organic pollutants and can reduce chlorinated organic pollutants into non-polluting ethane, acetylene, ethylene, etc., which is suitable for in-situ remediation of groundwater. Attached Figure Description
[0035] Figure 1 A schematic diagram of a sealed quartz tube;
[0036] Figure 2 This is a schematic diagram of the sealed quartz tube experiment in Example 1;
[0037] Figure 3 The images shown are transmission electron microscope (TEM) images of the vapor-phase chemical thermal synthesis of zero-valent iron nanoparticles prepared in Example 1. A is the TEM morphology image, B is the comprehensive elemental (nitrogen, oxygen, iron) distribution map of the high-angle dark field image (HADDF), C is the HADDF line scan nitrogen, oxygen, and iron elemental content distribution map, D is the HADDF oxygen elemental distribution map, E is the HADDF iron elemental distribution map, and F is the HADDF nitrogen elemental distribution map.
[0038] Figure 4 XRD pattern of the gas-phase chemical thermal synthesis of zero-valent iron nanoparticles in Example 1;
[0039] Figure 5 XPS images of the gas-phase chemical thermal synthesis of zero-valent iron nanoparticles prepared in Example 1 are shown, where a is the full XPS spectrum and b is a partial XPS spectrum.
[0040] The markings in the diagram are: 100 quartz tube; 200 partition plate. Detailed Implementation
[0041] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0042] The zero-valent iron powder and melamine in this section were purchased from Shanghai McLean Biochemical Technology Co., Ltd.
[0043] Example 1
[0044] Prepare a Figure 1 The quartz tube 100 shown has a partition plate 200 connected to one end of it. The length of the partition plate 200 is 1 / 2 of the inner diameter of the quartz tube 100. The following experiment was then conducted.
[0045] like Figure 2 As shown, 5g of zero-valent iron powder (particle size 100nm) and 5g of melamine were placed on both sides of a quartz tube 100. The quartz tube 100 was then vacuum-sealed with a vacuum of 0.1MPa. After sealing, the quartz tube 100 was placed in a muffle furnace. Heating I: The temperature was increased to 360℃ at a rate of 2℃ / min and held for 30min; Heating II: The temperature was increased to 480℃ at a rate of 1℃ / min and held for 100min. During the heating process, when the temperature slightly exceeded 350℃, the melamine decomposed and released ammonia gas, increasing the pressure inside the quartz tube 100. Under high temperature and high pressure conditions, the ammonia gas reacted with the iron oxides on the surface of the iron powder particles and the near-surface Fe... 0 The reaction produces Fe 4.4 After calcination of N and cooling to room temperature, open the quartz tube 100 to obtain a core-shell structured nitride nano-zero-valent iron composite material.
[0046] The nitride nano-zero-valent iron material prepared in this embodiment was characterized, and the results are as follows: Figure 3 , 4 As shown in Figure 5; Figure 3 The transmission electron microscope image of the zero-valent iron nitride nanoparticles prepared in Example 1 clearly shows the presence of nitrogen in the material. The results indicate that the zero-valent iron nitride nanoparticles prepared by this gas-phase thermal synthesis method have a typical core-shell structure, with zero-valent iron as the core and iron-nitrogen compounds as the shell. Figure 4 The XRD pattern shows that the nitrided form of iron is Fe. 4.4 N, unlike zero-valent iron nitride materials obtained by other gas-phase synthesis or ball milling methods; from Figure 5 The XPS image shows that Fe has formed on the material surface. xN, nitrogen, and iron coordinate to form iron nitrides, which are the nitride nano-zero-valent iron materials required in this application. Figure 3 , Figure 4 , Figure 5 It can be concluded that melamine can decompose under high temperature conditions to form NH3 and react with zero-valent iron, forming iron-nitrogen compounds on the particle surface, ultimately yielding core-shell structured nitrided nano-zero-valent iron. Based on the mass of the nitrided nano-zero-valent iron material, the mass percentage of zero-valent iron is 65%, and the mass percentage of iron-nitrogen compounds is 31%.
[0047] Examples 2-20 and Comparative Examples 1-9 were prepared using the same methods as in Example 1, according to the conditions in Table 1, to obtain core-shell structured nitride nano-zero valent iron.
[0048] Table 1. Conditions for each embodiment / comparative example
[0049]
[0050]
[0051] Note: N / Fe 0 The mass ratio of melamine to iron powder
[0052] [Performance Testing]
[0053] Using trichloroethylene (or tetrachloroethylene, trichloroethane, tetrachloroethane, trichloropropane, monochloromethane, dichloromethane, trichloromethane) as the target pollutant, the activity of the nitrided nano-zero-valent iron composite materials prepared in Examples 1-20 and Comparative Examples 1-9 was investigated.
[0054] The specific implementation steps are as follows: Add 0.025g of the nitrided nano-zero-valent iron material obtained in Example 1 (or any group of Examples 1-20 and Comparative Examples 1-9) to a 50mL reaction flask, then add 25mL of deoxygenated pH buffer solution (50mM HEPES, pH=7.0). At this point, the mass concentration of the nitrided nano-zero-valent iron is 1g / L. Then, inject an appropriate amount of trichloroethylene stock solution to ensure that the initial concentration of trichloroethylene is 10mg / L, and conduct the experiment. The concentration of trichloroethylene (or tetrachloroethylene, trichloroethane, tetrachloroethane, trichloropropane, chloroform, dichloromethane, trichloromethane) is monitored periodically using gas chromatography, and the results are shown in Table 2.
[0055] Table 2 Degradation performance of organic pollutants
[0056]
[0057]
[0058] As shown in Table 2, the core-shell structured nitrided nano-zero-valent iron prepared in this application exhibits a removal rate of over 95% for various chlorinated hydrocarbon organic pollutants, including trichloroethylene, tetrachloroethylene, trichloroethane, tetrachloroethane, trichloropropane, chloromethane, dichloromethane, and chloroform.
Claims
1. A method for preparing a core-shell structured zero-valent iron nitride material by gas-phase thermochemical synthesis, characterized in that, include: Iron powder with a particle size of 50-800 nm and melamine were placed in a quartz tube with a partition plate, which divided the quartz tube into a space for holding iron powder and a space for holding melamine. The spaces for holding iron powder and melamine were interconnected. The quartz tube was then vacuum sealed, and the quartz tube containing iron powder and melamine was calcined at 350-400℃ for 20-30 min, followed by calcination at 400-600℃ for 60-120 min to obtain a core-shell structured zero-valent iron nitride material. The heating rate to 350-400℃ was 1-5℃ / min, and the heating rate to 400-600℃ was 2-3℃ / min. The mass ratio of melamine to iron powder is 0.5~3:1; The core-shell structured zero-valent iron nitride material has a zero-valent iron core and an Fe outer shell. 4.4 N; The zero-valent iron content is 60-70 wt% based on the mass of the core-shell structured zero-valent iron nitride material.
2. The preparation method according to claim 1, characterized in that, One end of the partition plate is connected to the quartz tube, and the length of the partition plate is 1 / 5 to 1 / 2 of the inner diameter of the quartz tube.
3. The preparation method according to claim 1 or 2, characterized in that, After vacuum sealing, the vacuum degree inside the quartz tube is ≥0.1 MPa.
4. The application of the core-shell structured zero-valent iron nitride material prepared by the preparation method according to any one of claims 1 to 3 in the in-situ remediation of groundwater containing chlorinated hydrocarbon organic pollutants.
5. The application as described in claim 4, characterized in that, The chlorinated hydrocarbon organic pollutants are one or more of the following: trichloroethylene, tetrachloroethylene, trichloroethane, tetrachloroethane, monochloromethane, dichloromethane, trichloromethane, carbon tetrachloride, trichloropropane, and hexachlorobutadiene.
Citation Information
Patent Citations
Phosphorized zero-valent iron material with core-shell structure as well as preparation method and application of phosphatized zero-valent iron material
CN116351445A