Preparation method of fatigue test sample containing scratch defects and fatigue test method

By standardizing the introduction of scratch defects on the material surface and performing fatigue testing under strictly controlled stress conditions, the problem of difficulty in accurately simulated and tested the fatigue life of defective materials in the prior art is solved, and high-precision fatigue life data acquisition and structural safety improvement are achieved.

CN119574257APending Publication Date: 2025-03-07BEIHANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411808875.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-10-17
Filing Date
2024-12-10
Publication Date
2025-03-07

AI Technical Summary

Technical Problem

The prior art is difficult to accurately simulate and test the fatigue life of defective materials, resulting in insufficient safety margins in design and use.

Method used

By preparing fatigue test samples with scratch defects, standardized tools are used to introduce scratch defects, and fatigue tests are performed under strictly controlled stress conditions to obtain high-precision fatigue life data.

Benefits of technology

The repetition and comparability of the test results are achieved, high-precision experimental data is provided, and a solid experimental basis is provided for fatigue life prediction, which improves the safety and reliability of the structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119574257A_ABST
    Figure CN119574257A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a fatigue test sample containing a scratch defect and a fatigue test method, and relates to the field of material fatigue performance test.The preparation method comprises the steps that firstly, after a sample is machined through a lathe and the scratch defect is introduced, the defect size, the sample size and the surface quality are checked, and it is ensured that requirements are met; and then mounting the sample on a fatigue testing machine for testing, analyzing fracture characteristics after the test is finished, and finally processing and analyzing test data. The method not only can provide reliable data support for the fatigue performance of different materials, but also can be used for verifying an existing fatigue life prediction model, and provides a scientific basis for engineering design and material selection. The method is suitable for the fields of aerospace, automobile manufacturing, mechanical engineering and the like, and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material fatigue performance testing, and in particular to a method for preparing a fatigue test specimen containing a scratch defect and a fatigue test method, which is applied to fields such as aerospace that have high requirements on material fatigue performance. Background Art

[0002] In modern engineering applications, fatigue failure is a major problem that materials and structural parts often face during long-term use. Fatigue failure is usually caused by the gradual accumulation of damage to the material under cyclic loading. This damage manifests itself as the initiation and expansion of cracks at the microscopic level, eventually leading to the fracture of the material or structure. Especially in the fields of aerospace, automobiles, ships, and bridges, fatigue failure may lead to catastrophic consequences, so fatigue life has always been a key topic in scientific and engineering research.

[0003] In practical applications, various forms of defects, such as scratches, corrosion, pits, etc., will inevitably appear on the surface of materials or structures. The presence of these defects complicates the fatigue behavior of the material, significantly reduces the fatigue life of the material, and thus affects the overall safety and reliability of the structure. Based on the fatigue test data of defect-free samples, it is often impossible to accurately predict the life performance of defective materials in real environments, resulting in insufficient safety margins in design and use. Therefore, research and development of methods that can accurately simulate and test the fatigue life of defective materials is of great significance to engineering safety.

[0004] Among the publicly available technologies, research on fatigue testing of materials containing scratch defects is still limited. Existing methods mostly focus on qualitative analysis or simple crack initiation research, lacking systematicity and standardization. The way scratch defects are introduced is often uncontrolled, resulting in poor repeatability and comparability of test results. In addition, during fatigue testing, there are also many technical challenges in terms of how to accurately control stress levels, monitor crack propagation, and analyze fatigue data. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a fatigue test sample containing scratch defects and a fatigue test method. By this method, scratch defects can be introduced in a standardized manner on the surface of a material, and the durability and service life of the material can be evaluated through fatigue testing.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing a fatigue test sample containing a scratch defect comprises the following steps:

[0008] The first step is to use a lathe to process the sample, and then select the appropriate subsequent processing method according to the surface quality requirements of the actual structural parts;

[0009] In the second step, the scratch defect is introduced using a standardized tool that controls the depth, length and shape of the scratch;

[0010] Step 3: Check whether the defect size, sample size, and sample surface roughness meet the design requirements and record them.

[0011] Furthermore, the second step includes:

[0012] For small circular specimens, a custom-made turning tool is used to make a circle of pre-made scratches on the circular specimens; for small scratches of 0.1mm or 0.15mm in depth, one pre-forming is performed; for scratches of 0.25mm in depth, one pre-forming is performed; for large scratches of 0.35mm or 0.4mm in depth, two pre-forming is performed; the surface roughness requirements of the scratches are consistent with the surface roughness requirements of the specimens; after the forming is completed, the scratched surface is no longer processed, and the scratched surface is wiped with fine sandpaper to remove burrs.

[0013] Furthermore, the third step includes:

[0014] 1) Use an ultra-depth-of-field microscope to measure and inspect the size of scratch defects. The dimensions that must be measured include the diameter and depth of the defect on the sample surface. For standard scratch defects, the error in defect depth shall not exceed 10%.

[0015] 2) After finishing, use the measuring method to measure the size of the sample. The size of the working section of the sample is measured after finishing and before the prefabricated scratch defect. The remaining dimensions are measured after the sample preparation is completed. Use a 50-division vernier caliper to measure the sample size, and take the average of three measurements as the measured value; compare the size deviation requirements in the sample drawing to determine whether the sample size meets the drawing.

[0016] 3) In the final machining stage, the surface roughness of the sample is measured by measuring method and calculated by contour.

[0017] The average deviation of the surface was quantified using the optical method, and the surface profile was measured using the optical method.

[0018] The present invention also provides a fatigue test method for a fatigue test sample containing a scratch defect, comprising the following steps:

[0019] The first step is to apply a preload between the test machine fixture and the sensor, and install the sample on the fatigue test machine fixture to ensure that the sample and the test machine spindle are well coaxial.

[0020] The second step is to set the specific parameters of the fatigue test according to the cross-sectional dimensions and stress level of the specimen, conduct the test, and determine the effectiveness of the test;

[0021] The third step is to carry out macro-micro fracture analysis of the sample, and use a scanning electron microscope to take fracture morphology pictures; analyze the crack source location, crack extension trend, instantaneous fracture zone morphology, etc., and record them;

[0022] Step 4: Organize the original data, retain valid test data, remove invalid test data, and perform statistical analysis on the data.

[0023] Furthermore, the first step includes setting up an electro-hydraulic servo fatigue testing machine and a high-frequency fatigue testing machine; the electro-hydraulic servo fatigue testing machine performs axially symmetrical cyclic fatigue tests on metal and non-metallic materials, and the high-frequency fatigue testing machine is used to evaluate the fatigue performance and damage characteristics of the material under high-frequency cyclic loading.

[0024] Furthermore, in the second step, the method for judging the effectiveness of the test is as follows:

[0025] The test results are valid if the failure occurs at the defect. The test results are invalid if the specimen becomes unstable or the bending percentage exceeds 10%. The test results are valid if the specimen fails through the defect. The test results are invalid if the failure area of ​​the specimen is not at the defect.

[0026] Furthermore, in the third step, the fracture analysis includes:

[0027] 1) Observe the failure area of ​​the specimen, find the crack source through its morphology, including river pattern, fan-shaped pattern, ridge type, determine the type of crack source, including cleavage type, quasi-cleavage type, defect, pore, and determine the location of the crack source, including the surface, near the surface, and inside of the specimen;

[0028] 2) Observe whether there are cleavage planes in the crack propagation area, dimples in the instantaneous fracture area, and the density of these structures to determine the main form of specimen failure;

[0029] 3) In the fracture observation plane, observe and record the location and number of crack sources; the crack source is located at the bottom of the scratch defect or inside the cross section, and is divided into single crack source and multiple crack sources according to the number of cracks.

[0030] Beneficial effects:

[0031] (1) The present invention provides a method for preparing a fatigue test sample containing a scratch defect, which can accurately control the geometric size of the scratch in engineering applications and ensure the repeatability and comparability of the test results;

[0032] (2) The present invention provides a fatigue test method for a fatigue test specimen containing a scratch defect, provides high-precision experimental data, and provides a solid experimental basis for fatigue life prediction.

[0033] The present invention can obtain high-precision fatigue life data by introducing scratch defects in a standardized manner and performing fatigue tests under strictly controlled stress conditions. These data can be used to verify existing fatigue life prediction models and provide a scientific basis for material selection, structural design and life assessment in engineering applications.

[0034] In addition, the present invention also proposes a scratch prefabrication technology suitable for different materials, which can introduce controllable scratch defects on the surface of various metals and alloy materials to ensure the repeatability of the test and the reliability of the data. This scratch prefabrication technology combined with high-frequency fatigue test methods can be widely used in aerospace, automobile manufacturing, mechanical engineering and other fields, and has important engineering application value for improving structural safety and extending service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a flow chart of a method for preparing a fatigue test sample containing scratch defects according to the present invention;

[0036] Figure 2a It is a schematic diagram of a round smooth specimen;

[0037] Figure 2b Schematic diagram of the scratch defect prefabricated on the circular specimen;

[0038] Figure 3 This is a schematic diagram of the size of the scratch defect part;

[0039] Figure 4 The figure is a flow chart of a fatigue test method for a fatigue test specimen containing a scratch defect. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other. The present invention is further described in detail below in conjunction with the accompanying drawings.

[0041] like Figure 1 As shown, a method for preparing a fatigue test sample containing a scratch defect of the present invention comprises the following steps:

[0042] The first step is to use a lathe to process the sample, and select the appropriate subsequent processing method according to the surface quality requirements of the actual structural parts. If the surface quality requirements of the structural parts are low, turning can be selected. Turning is an efficient and low-cost mechanical processing method, suitable for parts with low surface roughness requirements. When the surface quality requirements are high, grinding can be used. Grinding can achieve higher surface finish and precision through fine cutting with a grinding wheel. In addition, chemical polishing can be used to improve surface smoothness, or surface coating processes (such as electroplating and anodizing) can be selected to enhance corrosion resistance and appearance. If the parts need to improve the mechanical properties of the surface, heat treatment methods such as carburizing or quenching are also common choices. These processing methods can be flexibly selected according to different surface quality requirements.

[0043] The second step is to introduce scratch defects using standardized tools. The standardized tools can be turning tools customized according to the geometric morphology and size of the defects. The standardized tools can control the depth, length and shape of the scratches.

[0044] Step 3: Check whether the defect size, sample size, and sample surface roughness meet the design requirements and record them.

[0045] Furthermore, the design of the small specimen of the material containing the scratch defect is carried out with reference to the HB5287-96 standard and ASTM E466-07. Referring to the geometric dimensions of the standard notched specimen recommended in HB5287-96, the notch is replaced by a scratch. According to the geometric dimensions of the standard circular small specimen with a notch, the specimen without prefabricated scratches is first processed, and then a turning tool is used to scratch a circle on the circular specimen to form a scratch defect.

[0046] A standard smooth specimen is used as the reference specimen for prefabricated scratch defects. The schematic diagram of the specimen is shown in Figure 2a , Figure 2b shown. Figure 2a In the test section, the roughness is consistent with the surface roughness of the real structural part. Figure 2b In the figure, the surface roughness of the sample is consistent with the surface roughness of the real structural part, and the surface roughness of the scratch is consistent with the surface roughness of the sample.

[0047] The geometric shape of the scratch defect is shown in Figure 2. Figure 3 As shown in the figure, the scratch shape is U-shaped, H is the cross-sectional depth of the scratch defect, and R is the semicircular arc radius of the bottom of the scratch defect.

[0048] Preferably, lathe processing is used in the initial stage of sample processing, and then appropriate subsequent processing methods are selected according to the surface quality requirements of the actual structural parts. In the final machining stage, the measurement method that does not change the surface state of the sample (optical and acoustic methods such as optical microscope, laser interferometer, ultrasonic detection and X-ray diffraction) is used to complete the dimensional measurement. In order to reduce the influence of surface roughness on the experimental results, the surface roughness of the sample test section is consistent with the surface roughness of the structural parts.

[0049] For small round specimens, use a custom turning tool to make a circle of pre-made scratches on the round specimen. For small scratches (such as 0.1mm or 0.15mm deep scratches), pre-form once. For 0.25mm deep scratches, pre-form once. For large scratches (such as 0.35mm or 0.4mm deep scratches), cut twice (for example: 0.1 mm + 0.25 mm). The surface roughness requirements of the scratches are consistent with the surface roughness requirements of the specimens. After forming, the scratched surface is no longer processed, but it is necessary to wipe the scratched surface with fine sandpaper to remove possible burrs.

[0050] Preferably, the defect size is measured by a measuring method in the final machining stage so as not to change the surface state of the sample and the defect. It is recommended to use an ultra-depth of field microscope to measure and check the size of the scratch defect. The dimensions that must be measured include the diameter of the defect on the sample surface and the defect depth.

[0051] Preferably, the sample size is measured by a measuring method after finishing so as not to change the surface state of the sample and the defect. The size of the working section of the sample needs to be measured after finishing and before prefabricating scratch defects; the remaining sizes can be measured after the sample is prepared. It is recommended to use a 50-division vernier caliper to measure the sample size and take the average of three measurements as the measurement value. Compare the dimensional deviation requirements in the sample drawing to determine whether the sample size meets the drawing.

[0052] Preferably, the surface roughness of the sample is measured by a measuring method at the final machining stage and is expressed as the arithmetic mean deviation of the profile R a For quantitative characterization, it is recommended to use optical methods for surface profile measurement.

[0053] The prepared specimens should be properly stored to avoid any damage (contact scratches, oxidation, etc.). It is recommended to use independent packaging boxes or tubes with caps to store the specimens. For some materials, such as aluminum alloys, it is necessary to store the specimens in a vacuum container or a desiccator with silica gel.

[0054] like Figure 4 As shown, a fatigue test method of a fatigue test specimen containing a scratch defect of the present invention comprises the following steps:

[0055] The first step is to install the sample on the fatigue testing machine fixture to ensure that the sample and the main axis of the testing machine are well coaxial;

[0056] The second step is to set the specific parameters of the fatigue test according to the cross-sectional dimensions and stress level of the specimen, conduct the test, and determine the effectiveness of the test;

[0057] The third step is to conduct macro-micro fracture analysis of the sample and use a scanning electron microscope to take fracture morphology pictures. Analyze the crack source location, crack extension trend, instantaneous fracture zone morphology, etc. and record them;

[0058] Step 4: Organize the original data, retain valid test data, remove invalid test data, and perform statistical analysis on the data.

[0059] The first step includes setting up an electro-hydraulic servo fatigue testing machine and a high-frequency fatigue testing machine.

[0060] The electro-hydraulic servo fatigue testing machine performs axially symmetrical cyclic fatigue tests on metal and non-metal materials. The whole machine consists of a main machine, a hydraulic source, an electrical control cabinet, and a computer control system. The overall structure adopts a double-column single-space structure, an elastic beam locking structure, and a two-way oil cylinder. The test space can be adjusted arbitrarily. The spoke-type sensor is located at the lower end of the upper beam and is seamlessly connected to the upper beam and the upper chuck body to ensure that the zero-crossing waveform of the test is not distorted. The fatigue test is required to realize any random waveform, sine waveform, square wave, triangle wave, etc., and according to the strength of the specimen, the adjustable frequency range should cover the load frequency range in the load condition.

[0061] The high-frequency fatigue testing machine is used to evaluate the fatigue performance and damage characteristics of materials under high-frequency cyclic loading, and its main components are a load system, a control system, a fixture system, a data acquisition system, control software, an auxiliary system, an operating table, and a sample installation area. The equipment has the characteristics of high-frequency loading capability, high load control accuracy, automated operation, and multi-channel data acquisition, and can provide key data for material design and performance prediction.

[0062] Example:

[0063] Refer to GB / T 3075-2021 standard to carry out fatigue test on small specimens of materials with scratch defects. The specific test process is as follows:

[0064] Before the test, visually inspect the specimens and record the initial state of the specimens. Write the specimen number according to the type of specimen. Use a vernier caliper to measure and record the geometric parameters of the specimens, and record the temperature and relative humidity of the laboratory.

[0065] Select a suitable chuck, install the sample on the testing machine, check the firmness of the sample installation, and ensure that the clamping part of the test piece is neither damaged nor slipped during the test.

[0066] According to the parameters determined in the preliminary test, the formal fatigue test is carried out. During the test, the state of the specimen is observed. If any abnormality is found, the machine is immediately stopped for processing; when obvious cracks occur or the specimen is completely broken, the test is terminated, the corresponding number of cycles is recorded, and photos of the test piece damage are taken; after the specimen is broken, the test piece is removed and placed in a designated location for safekeeping; according to the test results, calculate whether the number of tests under this load is met. If so, other load tests are carried out. If not, continue the fatigue test under this load.

[0067] During and after the test, the original test data were collated and statistically processed in accordance with GB / T 24176-2009. The specific method is as follows:

[0068] Taking into account the life discreteness of high-cycle fatigue, under the premise of meeting the given confidence level, coefficient of variation and relative error, the number of initial fatigue specimens at each stress level is not less than 3, and fatigue tests are carried out. Statistical analysis is carried out according to the fatigue life, and additional specimens are added according to the minimum number of specimens specified by the batch statistical method. According to the standards "GB / T 3075-2021 Axial Force Control Method for Fatigue Test of Metal Materials" and "GJBZ18A-2005 Data Processing and Expression of Mechanical Properties of Metal Materials", the data obtained from the fatigue test are processed.

[0069] When conducting life tests at selected stress levels, the dispersion of fatigue life should be considered. According to the statistical processing and error analysis requirements of the test data, the number of specimens required is determined according to the following steps:

[0070] 1) Calculate the mean and sample standard deviation S of a set of observations:

[0071] ;

[0072] ;

[0073] in, represents the sample mean, S is the subsample standard deviation, n is the number of elements in the sample, x i represents the i-th data point in the sample, i=1 represents the starting position of the summation, starting from the first data point, and n represents the ending position of the summation, which is the last data point in the sample.

[0074] 2) According to the t distribution theory, the interval estimation formula for the population mean is:

[0075] ;

[0076] Among them, μ is the population mean, t γIt represents the critical value of the t distribution based on the degrees of freedom n, which can be obtained by looking up the table.

[0077] 3) Let δ represent the limit of the relative error of the sample mean relative to the population mean, as shown below:

[0078] ;

[0079] 4) The minimum number of samples n required to estimate the median of the population is calculated as follows:

[0080] ;

[0081] Coefficient of variation The corresponding relationship with the minimum number of samples n can be seen in Table 1.

[0082] Table 1 Relationship between coefficient of variation and number of samples

[0083]

[0084] The initial number of test specimens for each stress level is 3. The minimum number of specimens calculation formula is used to determine whether the number of specimens needs to be increased.

[0085] Under a given test stress S, the logarithm of fatigue life is considered to be normally distributed, and the relationship is:

[0086] ;

[0087] in, , and are the mean and standard deviation of x respectively.

[0088] Sort and number the fatigue life of the specimens in the same group , the i-th series failure probability Pi usually refers to the failure probability of a system or component, which can be composed of multiple independent or dependent components. This series failure analysis is used to study the failure of complex systems, especially when the components in the system are arranged in series or parallel. Pi can be estimated as:

[0089] ;

[0090] definition The value is the probability of failure, for the average and standard deviation The estimate, based on and This is done through the following two relationships:

[0091] ;

[0092] ;

[0093] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a fatigue test sample containing scratch defects, characterized in that: The steps include: The first step is to use a lathe to process the sample, and then select the appropriate subsequent processing method according to the surface quality requirements of the actual structural parts; In the second step, the scratch defect is introduced using a standardized tool that controls the depth, length and shape of the scratch; Step 3: Check whether the defect size, sample size, and sample surface roughness meet the design requirements and record them.

2. The method for preparing a fatigue test sample containing scratch defects according to claim 1, characterized in that: The second step includes: For small circular specimens, a custom-made turning tool is used to make a circle of pre-made scratches on the circular specimen; for small scratches with a depth of 0.1mm or 0.15mm, one pre-forming is performed; for scratches with a depth of 0.25mm, one pre-forming is performed; for large scratches with a depth of 0.35mm or 0.4mm, two pre-forming is performed; the surface roughness requirements of the scratches are consistent with the surface roughness requirements of the specimens; after the forming is completed, the scratched surface is no longer processed, and the scratched surface is wiped with fine sandpaper to remove burrs.

3. The method for preparing a fatigue test sample containing scratch defects according to claim 1, characterized in that: The third step comprises: 1) Use an ultra-depth-of-field microscope to measure and inspect the size of scratch defects. The dimensions that must be measured include the diameter and depth of the defect on the surface of the sample. For standard scratch defects, the error in the defect depth shall not exceed 10%; 2) After finishing, the sample dimensions are measured by measuring methods. The dimensions of the working section of the sample are measured after finishing and before the scratch defect is prefabricated. The remaining dimensions are measured after the sample preparation is completed. The sample dimensions are measured with a 50-division vernier caliper, and the average of three measurements is taken as the measured value. The sample dimensions are compared with the dimensional deviation requirements in the sample drawing to determine whether the sample dimensions meet the drawing. 3) In the final machining stage, the surface roughness of the sample is measured by the measurement method, and the arithmetic mean deviation of the profile is used for quantitative characterization, and the surface profile is measured by optical method.

4. A fatigue test method for a fatigue test specimen containing a scratch defect, characterized in that: The steps include: The first step is to apply a preload between the test machine fixture and the sensor, and install the sample on the fatigue test machine fixture to ensure that the sample and the test machine spindle are well coaxial. The second step is to set the specific parameters of the fatigue test according to the cross-sectional dimensions and stress level of the specimen, conduct the test, and determine the effectiveness of the test; The third step is to carry out macro-micro fracture analysis of the sample, and use a scanning electron microscope to take fracture morphology pictures; analyze the crack source location, crack extension trend, instantaneous fracture zone morphology, etc., and record them; Step 4: Organize the original data, retain valid test data, remove invalid test data, and perform statistical analysis on the data.

5. A fatigue test method for a fatigue test specimen containing a scratch defect according to claim 4, characterized in that: The first step includes setting up an electro-hydraulic servo fatigue testing machine and a high-frequency fatigue testing machine; the electro-hydraulic servo fatigue testing machine performs axially symmetrical cyclic fatigue tests on metal and non-metal materials, and the high-frequency fatigue testing machine is used to evaluate the fatigue performance and damage characteristics of materials under high-frequency cyclic loading.

6. A fatigue test method for a fatigue test specimen containing a scratch defect according to claim 4, characterized in that: In the second step, the method for judging the effectiveness of the test is as follows: The test results are valid if the failure occurs at the defect. The test results are invalid if the specimen becomes unstable or the bending percentage exceeds 10%. The test results are valid if the specimen fails through the defect. The test results are invalid if the failure area of ​​the specimen is not at the defect.

7. A fatigue test method for a fatigue test specimen containing a scratch defect according to claim 4, characterized in that: In the third step, the fracture analysis includes: 1) Observe the failure area of ​​the specimen, find the crack source through its morphology, including river pattern, fan-shaped pattern, ridge type, determine the type of crack source, including cleavage type, quasi-cleavage type, defect, pore, and determine the location of the crack source, including the surface, near the surface, and inside of the specimen; 2) Observe whether there are cleavage planes in the crack propagation area, dimples in the instantaneous fracture area, and the density of these structures to determine the main form of specimen failure; 3) In the fracture observation plane, observe and record the location and number of crack sources; the crack source is located at the bottom of the scratch defect or inside the cross section, and is divided into single crack source and multiple crack sources according to the number of cracks.