A low-basis-weight leak-proof PE membrane and its preparation method

By optimizing the resin type and process through a three-layer structure and the disordered distribution of nano-sized calcium carbonate, the problem of decreased strength and leak-proofness of PE film after weight reduction was solved, resulting in a low-weight, high-strength, leak-proof and breathable PE film that meets the needs of hygiene products.

CN119636207BActive Publication Date: 2026-11-17FOSHAN YOUCAI NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411818846.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-11
Publication Date
2026-11-17
Estimated Expiration
2044-12-11

AI Technical Summary

Technical Problem

As the basis weight of existing PE films decreases, their tensile strength and elongation at break also decrease, resulting in poor leak-proof performance. This makes them unsuitable for the use of hygiene products, and their reliance on imports increases production costs.

Method used

The PE membrane adopts a three-layer structure, with the upper, middle and lower membrane layers composed of mLLDPE resin, LLDPE resin, LDPE resin and nano-sized calcium carbonate. The microporous structure is formed through a three-stage step-by-step preheating and micro-stretching process. Combined with the disordered distribution of nano-sized calcium carbonate, the resin type and membrane structure are optimized to improve the impermeability and air permeability.

Benefits of technology

With low basis weight, PE film has high tensile strength, elongation at break, leak-proofness and air permeability, which meets the needs of hygiene products and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005182581530000161
    Figure BDA0005182581530000161
Patent Text Reader

Abstract

This invention discloses a low-basis-weight, leak-proof PE membrane, wherein the basis weight of the PE membrane is 26-28 g / m³. 2 The PE membrane comprises an upper film layer, an intermediate film layer, and a lower film layer distributed sequentially from top to bottom. Each of the upper, intermediate, and lower film layers is obtained by melt extrusion, stretching, and curing of a PE film mixture. The PE film mixture comprises the following raw materials: mLLDPE resin, LLDPE resin, LDPE resin, and nano-sized calcium carbonate, with the nano-sized calcium carbonate accounting for 45-48% by mass percentage. This invention proposes a low-basis-weight, leak-proof PE membrane that, while ensuring low basis weight, not only possesses air permeability and leak-proof properties, but also suitable shrinkage, high tensile strength, and high elongation at break, overcoming the shortcomings of existing technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of PE films, and more particularly to a low-weight, leak-proof PE film and its preparation method. Background Technology

[0002] Polyethylene film (PE film) is a thin film produced by extrusion blow molding, extrusion calendering, or extrusion casting of various types of PE resin and additives. Due to its anti-pollution, softness, comfort, safety and non-toxicity, it is used not only as food packaging film, pharmaceutical packaging film, pool film, waterproof film and agricultural film, but also as a base film for various hygiene products such as sanitary napkins, baby diapers and adult incontinence products.

[0003] With the continuous advancement of hygiene product technology and the increasing demands of consumers, hygiene products are gradually evolving towards being "softer, more comfortable, and thinner." This places higher requirements on PE film, a key raw material for hygiene products. Not only must PE film possess excellent leak-proof properties to protect users from leakage, but it must also have a low basis weight to achieve thinner and lighter hygiene products. This reduces raw material consumption and production costs while ensuring a closer fit and improved wearing comfort. However, the basis weight of traditional PE film is typically around 30g / m³. 2 While its tensile strength and elongation at break are relatively high, its basis weight is also relatively high. Furthermore, due to the manufacturing process and the choice of raw materials, its leakage is relatively large, which cannot meet the market demand for low-weight, leak-proof, high-performance PE films.

[0004] To overcome the shortcomings of traditional PE film products, major PE film manufacturers have been developing and manufacturing low-weight, leak-proof, high-performance PE films to meet market demand. However, as the basis weight of PE films decreases, the tensile strength and elongation at break of the products also decline; in addition, the leak-proof performance of the products remains poor, failing to meet the usage requirements. As a result, the low-weight, leak-proof, high-performance PE films used in hygiene products still mainly rely on imports, which to some extent increases the production cost of high-quality hygiene products. Summary of the Invention

[0005] One of the objectives of this invention is to provide a low-weight, leak-proof PE membrane that, while ensuring low weight, not only has air permeability and leak-proof properties, but also suitable shrinkage, high tensile strength, and high elongation at break, thereby overcoming the shortcomings of the prior art.

[0006] The second objective of this invention is to provide a method for preparing a low-basis-weight, leak-proof PE membrane, which is simple in procedure, easy to operate, and ensures that the basis weight of the obtained PE membrane is as low as 26 g / m³. 2Water vapor permeability ≥1500g / (㎡.24h), transverse tensile strength ≥2.5N / 25mm, longitudinal tensile strength ≥10N / 25mm, transverse elongation at break ≥200%, longitudinal elongation at break ≥150%, longitudinal heat shrinkage 3~6%. Under the premise of ensuring low weight, it not only has air permeability and leak-proofness, but also has suitable shrinkage, high tensile strength and high elongation at break to meet the product's usage requirements.

[0007] To achieve this objective, the present invention adopts the following technical solution:

[0008] A low-basis-weight, leak-proof PE membrane, wherein the basis weight of the PE membrane is 26–28 g / m³. 2 The PE film comprises an upper film layer, an intermediate film layer, and a lower film layer distributed from top to bottom. The upper film layer, the intermediate film layer, and the lower film layer are all obtained by melting, extruding, stretching, and curing the PE film mixture separately.

[0009] The PE mixture includes the following raw materials: mLLDPE resin, LLDPE resin, LDPE resin and nano-sized calcium carbonate, and the amount of nano-sized calcium carbonate added is 45-48% by mass percentage.

[0010] Further, calculated by mass percentage, the PE mixture comprises the following raw materials: 20-30% mLLDPE resin, 12-27% LLDPE resin, 8-10% LDPE resin, and 45-48% nano-grade calcium carbonate.

[0011] Furthermore, the particle size of the nano-sized calcium carbonate is 200–700 nm.

[0012] Furthermore, the weights of the upper film layer, the middle film layer, and the lower film layer are all the same.

[0013] A method for preparing a low-basis-weight leak-proof PE membrane, comprising the following steps:

[0014] S1. Mix mLLDPE resin, LLDPE resin, LDPE resin and nano-sized calcium carbonate evenly according to the formula to obtain PE mixture;

[0015] S2. The PE mixture is added to a twin-screw extruder for melting and then conveyed at a constant temperature to the first, second, and third flow channels of the die cavity. The melt in the first, second, and third flow channels merges at the die lip of the die head and undergoes three-layer co-extrusion. The melt is then pressed by the casting steel roller and casting pressure roller to form the first intermediate film. The first intermediate film is then subjected to matte treatment and cooling to obtain the second intermediate film.

[0016] S3. The second intermediate membrane material is subjected to three-stage step preheating and three-stage step micro-stretching to obtain the third intermediate membrane material, and the third intermediate membrane material has a microporous structure;

[0017] S4. The third intermediate membrane material is subjected to heat setting, cooling and embossing treatment in sequence to obtain the fourth intermediate membrane material; the surface of the fourth intermediate membrane material is subjected to corona treatment, and after winding, a low-grammage leak-proof PE film is obtained.

[0018] Further, in step S3, the specific method of the three-stage stepped preheating is as follows: the second intermediate film material is preheated in the first stage, the second stage, and the third stage using a preheating roller, and the preheating temperature of the first stage is 75-80℃, the preheating temperature of the second stage is 81-85℃, and the preheating temperature of the third stage is 86-90℃.

[0019] Further, in step S3, the specific method of the three-stage stepped micro-stretching is as follows: using three stretching rollers, each with a temperature of 85-95℃, to perform first-stage micro-stretching, second-stage micro-stretching, and third-stage micro-stretching on the second intermediate film material that has undergone three-stage stepped preheating, and the stretching ratio of the first-stage micro-stretching is 1.1-1.2, the stretching ratio of the second-stage micro-stretching is 1.2-1.5, and the stretching ratio of the third-stage micro-stretching is 1.5-1.8.

[0020] Further, in step S2, the temperature of both the casting steel roll and the casting pressure roll is 20–28°C, and the mutual clamping force between the casting steel roll and the casting pressure roll is 4–6 kg / cm². 2 .

[0021] Furthermore, in step S4, the corona current of the corona treatment is 3 to 5 A.

[0022] Further, in step S3, the water vapor transmission rate of the low-weight leak-proof PE film is ≥1500g / (㎡.24h), the transverse tensile strength is ≥2.5N / 25mm, the longitudinal tensile strength is ≥10N / 25mm, the transverse elongation at break is ≥200%, the longitudinal elongation at break is ≥150%, and the longitudinal heat shrinkage is 3-6%.

[0023] The technical solution provided by this invention may include the following beneficial effects:

[0024] 1. Due to the disordered distribution of nano-sized calcium carbonate in the upper, middle, and lower membrane layers, the micropores formed after micro-stretching of the upper, middle, and lower membrane layers are partially or completely misaligned. This means that even if the micropores of any one of the upper, middle, or lower membrane layers are penetrated by liquids such as blood and water, the misaligned arrangement makes it difficult for the position of the micropores in the next membrane layer to coincide with the position of the micropores in the previous penetrated membrane layer. This prevents further leakage of blood and water, greatly reduces the risk of leakage, and further ensures the leak-proof performance of the PE membrane.

[0025] 2. The compact molecular structure of mLLDPE resin effectively prevents the leakage of blood or water. Simultaneously, the linear molecular chains of LLDPE resin, with few or no long branches, allow it to form a tight crystalline structure during processing, effectively preventing blood or water leakage. Furthermore, the shorter molecular chains of LDPE resin, while resulting in weaker intermolecular forces, effectively prevent blood or water leakage. Additionally, mLLDPE, LLDPE, and LDPE resins all possess excellent heat-sealing properties, enabling the upper, middle, and lower film layers to bond tightly, forming a robust seal that also effectively prevents blood or water leakage. Therefore, based on these principles, this technical solution optimizes the type of calcium carbonate, the structure of the PE film, and the type of resin to ensure the resulting PE film exhibits excellent leak-proof properties, meeting the stringent requirements for leak-proof performance in PE film applications.

[0026] 3. Due to its regular molecular chain structure and the presence of a certain amount of long branches, LLDPE resin exhibits excellent heat shrinkage properties when heated, allowing for uniform shrinkage. Similarly, while LLDPE resin has a linear molecular chain structure, it typically contains fewer short branches or no long branches, thus also possessing some heat shrinkage properties. Through the synergy of these two components, PE blends incorporating both LLDPE resin and LLDPE resin achieve suitable heat shrinkage properties, thereby imparting suitable heat shrinkage characteristics to the PE films processed from these blends. Detailed Implementation

[0027] This technical solution provides a low-basis-weight, leak-proof PE membrane, wherein the basis weight of the PE membrane is 26–28 g / m³. 2 The PE film comprises an upper film layer, an intermediate film layer, and a lower film layer distributed from top to bottom. The upper film layer, the intermediate film layer, and the lower film layer are all obtained by melting, extruding, stretching, and curing PE mixtures respectively.

[0028] The PE film mixture includes the following raw materials: mLLDPE resin, LLDPE resin, LDPE resin and nano-sized calcium carbonate, and the amount of nano-sized calcium carbonate added is 45-48% by mass percentage.

[0029] To address the technical problem that existing PE films cannot meet usage requirements, this technical solution proposes a low-basis-weight, leak-proof PE film, comprising an upper film layer, an intermediate film layer, and a lower film layer distributed from top to bottom. By innovating the PE preparation process and the PE film mixture formulation, the resulting PE film, while ensuring low basis weight, not only possesses air permeability and leak-proof properties, but also exhibits suitable shrinkage, high tensile strength, and high elongation at break, thus meeting the product's usage requirements.

[0030] Specifically, in existing technologies, calcium carbonate particles are typically incorporated into PE mixtures to create microporous structures in PE films. Subsequently, a twin-screw extruder is used for melt extrusion and micro-stretching to obtain the PE film. During micro-stretching, the PE film is subjected to directional external forces, generating stress. This stress is particularly concentrated around the calcium carbonate particles, causing the molecular chains of the PE film around the calcium carbonate particles to break or slip in an orderly manner, promoting the formation of micropores. In other words, existing technologies use calcium carbonate particles as nucleation sites to guide micropore formation during stretching. However, micropore formation is highly dependent on the size of the calcium carbonate particles. The micron- or millimeter-sized calcium carbonate particles used in traditional technologies, even under a single micro-stretching action, result in relatively large micropores after stretching, increasing the risk of leakage. Furthermore, existing PE films generally employ a single-layer structure design. This single-layer design makes the PE film, when used as a base film for hygiene products, prone to leakage of liquids such as blood and water, further exacerbating the leakage problem. Therefore, the PE film in this design cannot be based on the above principles.

[0031] To impart leak-proof properties to the PE membrane, this technical solution adds nano-sized calcium carbonate to the PE mixture formulation. Because the particle size of nano-sized calcium carbonate is significantly smaller than the micron- or millimeter-sized calcium carbonate particles used in traditional technologies, the micropores formed on the PE membrane after micro-stretching are much smaller. This reduction in micropore size greatly enhances the leak-proof performance of the PE membrane, reducing leakage of liquids such as blood and water, thereby ensuring the leak-proof nature of the PE membrane.

[0032] Furthermore, this technical solution also optimizes the structural design of the PE membrane, making the PE membrane comprise an upper membrane layer, an intermediate membrane layer, and a lower membrane layer distributed sequentially from top to bottom. Due to the disordered distribution of nano-sized calcium carbonate in the upper, intermediate, and lower membrane layers, the micropores formed after micro-stretching of the upper, intermediate, and lower membrane layers are partially or completely misaligned. This means that even if the micropores of any one of the upper, intermediate, or lower membrane layers are penetrated by liquids such as blood and water, the misaligned arrangement makes it difficult for the position of the micropores in the next membrane layer to coincide with the position of the micropores in the previous penetrated membrane layer. This hinders the continued leakage of blood and water, greatly reducing the risk of leakage and further ensuring the leak-proof performance of the PE membrane.

[0033] Since the type of PE resin has a significant impact on the leak-proof performance of PE membranes, simply optimizing the type of calcium carbonate and the structure of the PE membrane is insufficient to meet the extremely high leak-proof requirements of PE membranes. Therefore, this technical solution also optimizes the type of PE resin.

[0034] Specifically, the resin types in PE film blends include mLLDPE resin (metallocene linear low-density polyethylene resin), LLDPE resin (linear low-density polyethylene resin), and LDPE resin (low-density polyethylene resin). mLLDPE resin has a compact molecular structure, effectively preventing the leakage of blood or water. Meanwhile, LLDPE resin has a linear molecular chain structure, but typically contains few or no long branches, allowing it to form a tight crystalline structure during processing, thus effectively preventing blood or water leakage. Additionally, LDPE resin has shorter molecular chains, resulting in weaker intermolecular forces, yet it still effectively prevents blood or water leakage. Furthermore, mLLDPE, LLDPE, and LDPE resins all possess good heat-sealing properties, allowing the upper, middle, and lower film layers to bond tightly, forming a robust sealing structure that also effectively prevents blood or water leakage. Therefore, based on the above principles, this technical solution optimizes the type of calcium carbonate, the structure of the PE film, and the type of resin to ensure that the obtained PE film has anti-leakage properties, meeting the extremely high requirements for the anti-leakage properties of the PE film.

[0035] Secondly, the PE membrane in this technical solution, due to its stretching process, forms micropores, and the micropores in the upper, middle, and lower membrane layers are partially or completely misaligned. However, because water vapor molecules are very small, they have the ability to diffuse through the micropores. This allows water vapor molecules to diffuse and migrate through these tiny pores even with the misaligned arrangement, giving the PE membrane air permeability. Furthermore, although the micropores in the upper, middle, and lower membrane layers are partially or completely misaligned, there is still a certain degree of connectivity between these micropores, allowing water vapor to pass through, which also contributes to the air permeability of the PE membrane. Further, this technical solution limits the addition of nano-sized calcium carbonate in the PE mixture to 45-48%, increasing the number of micropores in the PE membrane and forming a small and dense microporous structure in the upper, middle, and lower membrane layers. This facilitates the diffusion and migration of water vapor, further enhancing the air permeability of the PE membrane. In other words, this technical solution achieves air permeability of the PE membrane through the synergistic effect of these three aspects.

[0036] Furthermore, the high crystallinity, high strength, and good toughness of mLLDPE resin endow the PE mixture with extremely high tensile strength and high elongation at break; LLDPE resin has high strength and toughness, thus endowing the PE mixture with high tensile strength and elongation at break; LDPE resin (low-density polyethylene resin) has excellent softness and toughness, thus endowing the PE mixture with high elongation at break; nano-sized calcium carbonate particles have a small particle size and a large specific surface area, and these characteristics allow them to effectively and tightly bond with the PE resin matrix (such as mLLDPE resin, LLDPE resin, and LDPE resin). When nano-calcium carbonate is uniformly dispersed in the PE film, it can act as a reinforcing phase, significantly improving the tensile strength and elongation at break of the PE film. Therefore, this technical solution, through the synergistic effect of mLLDPE resin, LLDPE resin, LDPE resin, and nano-sized calcium carbonate, endows the PE mixture with high tensile strength and high elongation at break, thus giving the PE film high tensile strength and high elongation at break.

[0037] Finally, mLLDPE resin, due to its regular molecular chain structure and the presence of a certain amount of long branches, exhibits excellent heat shrinkage properties due to its ability to shrink uniformly when heated. Similarly, LLDPE resin, with its linear molecular chain structure but typically containing fewer or no short branches, also possesses certain heat shrinkage properties. Through the synergy of these two materials, the PE blend containing both mLLDPE resins possesses suitable heat shrinkage properties, thereby endowing the PE film processed from the blend with appropriate heat shrinkage performance. This not only allows the PE film to adhere tightly to other materials in the sanitary napkin during heating, forming a stable structure and improving the product's stability and reliability, but also avoids excessive heat shrinkage, which could lead to excessive shrinkage during heating, resulting in deformation or wrinkles that negatively impact the appearance and usability of the sanitary napkin.

[0038] It should be noted that the crystallinity of both LLDPE and LDPE resins is significantly lower than that of mLLDPE resin. This effectively compensates for the defect that mLLDPE resin, due to its higher crystallinity, has stronger intermolecular forces, requiring higher temperatures to melt and resulting in poorer processing performance of PE mixtures. Thus, PE mixtures have stronger processability.

[0039] In addition, LDPE resin has good flexibility and ductility, which allows the PE film to undergo greater deformation when subjected to external forces without easily breaking or tearing, thus ensuring product integrity. Furthermore, nano-calcium carbonate can also improve the wear resistance and tear resistance of the PE film, increasing its durability.

[0040] To further explain, the PE mixture comprises the following raw materials by mass percentage: 20-30% mLLDPE resin, 12-27% LLDPE resin, 8-10% LDPE resin, and 45-48% nano-grade calcium carbonate.

[0041] This technical solution optimizes the proportions of each raw material in the PE mixture, thereby reducing costs while maximizing the performance of each raw material and achieving better performance of the PE film, thus enhancing the market competitiveness of the PE film.

[0042] Preferably, the PE mixture comprises 25% mLLDPE resin, 20% LLDPE resin, 10% LDPE resin and 45% nano-sized calcium carbonate by weight percentage.

[0043] To further clarify, the particle size of the nano-sized calcium carbonate is 200–700 nm.

[0044] By limiting the particle size of nano-sized calcium carbonate, it is not only beneficial to improve the dispersibility of calcium carbonate in PE film, making it less prone to agglomeration, thereby ensuring the formation of uniformly dispersed and small and dense micropores, improving the leak-proof and air-permeable properties of PE film, but also beneficial to improve the strength and toughness of PE film, thereby improving the tear resistance and rupture resistance of PE film.

[0045] To further clarify, the weights of the upper film layer, the middle film layer, and the lower film layer are all the same.

[0046] By optimizing the basis weight of each film layer in the PE film, the thickness and density distribution of each layer becomes more uniform, reducing the risk of deformation or breakage caused by uneven stress. Furthermore, having the same basis weight for each film layer simplifies the production process and reduces production difficulty and costs.

[0047] A method for preparing a low-basis-weight leak-proof PE membrane, comprising the following steps:

[0048] S1. Mix mLLDPE resin, LLDPE resin, LDPE resin and nano-sized calcium carbonate evenly according to the formula to obtain PE mixture;

[0049] S2. The PE mixture is added to a twin-screw extruder for melting and then conveyed at a constant temperature to the first, second, and third flow channels of the die cavity. The melt in the first, second, and third flow channels merges at the die lip of the die head and undergoes three-layer co-extrusion. The melt is then pressed by the casting steel roller and casting pressure roller to form the first intermediate film. The first intermediate film is then subjected to matte treatment and cooling to obtain the second intermediate film.

[0050] S3. The second intermediate membrane material is subjected to three-stage step preheating and three-stage step micro-stretching to obtain the third intermediate membrane material, and the third intermediate membrane material has a microporous structure;

[0051] S4. The third intermediate membrane material is subjected to heat setting, cooling and embossing treatment in sequence to obtain the fourth intermediate membrane material; the surface of the fourth intermediate membrane material is subjected to corona treatment, and after winding, a low-grammage leak-proof PE film is obtained.

[0052] This technical solution also proposes a method for preparing a low-weight, leak-proof PE membrane. The preparation method is simple and easy to operate, ensuring that the obtained PE membrane, while having a low basis weight, not only has air permeability and leak-proof properties, but also suitable shrinkage, high tensile strength and high elongation at break, to meet the product's usage requirements.

[0053] Specifically, in step S3, the second intermediate membrane material undergoes a three-stage stepped preheating and a three-stage stepped micro-stretching. Stepped preheating gradually increases the temperature of the second intermediate membrane material, avoiding thermal stress caused by sudden temperature increases. Simultaneously, since a single stretching process is unlikely to form an ideal microporous structure, and the size and uniformity of the micropores are poor, it can easily affect the leak-proof performance of the PE membrane. Therefore, this technical solution optimizes the stretching process by employing a three-stage stepped micro-stretching method. This allows the microporous structure of the PE membrane to be gradually optimized, resulting in finer and more uniform micropores, thus enhancing the leak-proof performance of the PE membrane. Furthermore, the three-stage stepped micro-stretching also avoids the risk of sudden stress concentration caused by single-stage stretching, which could lead to easy rupture or damage to the PE membrane.

[0054] It should be noted that this technical solution can also use an automatic thickness gauge to measure the thickness and basis weight of the third intermediate film material and feed the test results back to the control system. Through the preset settings of the control system, the extrusion gap of the die head is automatically adjusted to ensure the extrusion stability of the PE film.

[0055] Preferably, in step S1, the mixing weight of the PE mixture is ≤10Kg and the mixing time is 0.8 to 1min, to further ensure uniform mixing and thus ensure the performance of each film layer.

[0056] Preferably, in step S2, the melting temperature of the twin-screw extruder is 200–210°C, the holding temperature is 210–230°C, and the die temperature is 230–250°C.

[0057] By limiting the above parameters, the temperature of the twin-screw extruder is gradually increased from the melt to the die, which helps to ensure the fluidity of the PE mixture in the twin-screw extrusion and ensures that the PE mixture can be co-extruded in three layers after melting.

[0058] Preferably, in step S2, the temperature of the first flow channel is 245-255°C, the temperature of the second flow channel is 235-240°C, and the temperature of the third flow channel is 245-255°C.

[0059] In a preferred embodiment of this technical solution, by setting the temperature of the first and third flow channels to be higher than that of the second flow channel, that is, the temperature on both sides of the die cavity is higher than that in the middle, the first and second mixtures flow more smoothly after melting, thus ensuring three-layer co-extrusion.

[0060] Preferably, in step S4, the temperature of the heat setting treatment is 100-110°C; and the temperature of the cooling treatment is 25-35°C.

[0061] Limiting the temperature of the heat setting process helps ensure the stability of the PE film's dimensions and shape.

[0062] To further explain, in step S3, the specific method of the three-stage stepped preheating is as follows: the second intermediate film material is preheated in the first stage, the second stage, and the third stage using preheating rollers, and the preheating temperature of the first stage is 75-80℃, the preheating temperature of the second stage is 81-85℃, and the preheating temperature of the third stage is 86-90℃.

[0063] By limiting the preheating temperatures of the first, second, and third stages of preheating, the second intermediate film material gradually reaches the appropriate temperature range for stretching, avoiding thermal stress concentration and uneven stretching caused by sudden temperature increases, which is more conducive to ensuring product performance.

[0064] To further explain, in step S3, the specific method of the three-stage stepped micro-stretching is as follows: using three stretching rollers, each with a temperature of 85-95℃, to perform the first-stage micro-stretching, the second-stage micro-stretching, and the third-stage micro-stretching on the second intermediate film material that has undergone three-stage stepped preheating, respectively. The stretching ratio of the first-stage micro-stretching is 1.1-1.2, the stretching ratio of the second-stage micro-stretching is 1.2-1.5, and the stretching ratio of the third-stage micro-stretching is 1.5-1.8.

[0065] The temperature of the stretching roller is set in the range of 85 to 95°C, which matches the temperature of the second intermediate film material after three-stage preheating. This ensures that the second intermediate film material is in the optimal thermoplastic state during the stretching process, thus helping to ensure the stretching effect.

[0066] In addition, by limiting the stretch ratio at each level and increasing the stretch ratio step by step, the second intermediate film material, which has undergone three-stage preheating, gradually reaches the required orientation state during the stretching process. This avoids film material rupture or performance degradation caused by sudden stretching, thus helping to ensure the performance of the final PE film.

[0067] It should be noted that the stretch ratio refers to the ratio of the size of the film after stretching to the size of the film before stretching.

[0068] To further explain, in step S2, the temperature of both the casting steel roll and the casting pressure roll is 20–28°C, and the mutual clamping force between the casting steel roll and the casting pressure roll is 4–6 kg / cm². 2 .

[0069] During the cooling and shaping process, the temperature of the cooling water is 25℃. When the temperature of both the casting steel roller and the casting pressure roller is less than 20℃, the temperature is too low, and the cooling water is prone to condense on the first intermediate film, affecting the subsequent processing of the first intermediate film. When the temperature of both the casting steel roller and the casting pressure roller is greater than 28℃, the temperature is too high, causing the first intermediate film to be brittle and difficult to shape.

[0070] Furthermore, the mutual clamping force between the casting steel roll and the casting pressure roll is 4–6 kg / cm. 2 This ensures that each membrane layer is compressed and formed.

[0071] To further explain, in step S4, the corona current of the corona treatment is 3 to 5 A.

[0072] Since sanitary products consist of a top layer, an absorbent core, and a bottom film, and the PE film serves as the bottom film, it needs to be bonded to the top layer to enclose the absorbent core between the top layer and the bottom film. Therefore, this technical solution limits the corona current of the corona treatment to 3-5A, so that the surface tension of the PE film reaches 36-42mN / m, which facilitates the adhesion between the PE film as the bottom film and the top layer of the sanitary product, ensuring the performance of the PE film.

[0073] To further explain, in step S3, the water vapor transmission rate of the low-weight leak-proof PE film is ≥1500g / (㎡.24h), the transverse tensile strength is ≥2.5N / 25mm, the longitudinal tensile strength is ≥10N / 25mm, the transverse elongation at break is ≥200%, the longitudinal elongation at break is ≥150%, and the longitudinal heat shrinkage is 3-6%.

[0074] The PE film obtained by this technical solution has a water vapor transmission rate of ≥1500g / (㎡.24h), a transverse tensile strength of ≥2.5N / 25mm, a longitudinal tensile strength of ≥10N / 25mm, a transverse elongation at break of ≥200%, a longitudinal elongation at break of ≥150%, and a longitudinal heat shrinkage of 3-6%. Under the premise of ensuring low basis weight, it not only has air permeability and leak-proof properties, but also suitable shrinkage, high tensile strength, and high elongation at break, meeting the application requirements of the product.

[0075] The technical solution of the present invention will be further illustrated below through specific embodiments.

[0076] Performance testing:

[0077] Basis weight: Stack 10 layers of PE film, cut 10 samples with an area of ​​0.01 (㎡.24h) using a template with dimensions of 100mm×100mm (i.e., both length and width are 100mm, the same below), and obtain a test sample with a total area of ​​0.1 (㎡.24h). Weigh the test sample using an electronic balance, and then multiply the test result by 10 to obtain the basis weight.

[0078] Heat shrinkage performance: Three test samples, each measuring 100mm × 100mm, were cut from the middle and both sides of the film. The initial longitudinal length L0 of each sample was measured and recorded. The three samples were then placed in a constant-temperature drying oven at 60℃ for 60 minutes, removed, and left at room temperature for 30 minutes. Subsequently, the longitudinal mark length L1 of the three samples after cooling was measured and recorded again. According to the formula: △ L = (L1-L0) / L0*100 calculates the heat shrinkage rate of each test sample, and the average value of the heat shrinkage rates of the three test samples is taken as the final test result.

[0079] Air permeability: Cut a 100mm×100mm test sample, pour 30ml of distilled water into the permeation cup, and weigh the initial weight M0 of the permeation cup containing distilled water; place the permeation cup containing distilled water in an environment with a temperature of 40℃ and a relative humidity of 50%, then place the test sample on the mouth of the permeation cup containing distilled water and tighten and fix the test sample with the matching aluminum ring. After testing for a period of time, measure the weight M1 of the permeation cup containing distilled water. Calculate the water vapor transmission rate according to the formula: Water vapor transmission rate = (M1-M0)×24 / (cup mouth area×test time), where the test time is in hours.

[0080] Elongation at break: The elongation at break was determined according to the test method in GB / T 1040.2-2006 Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics.

[0081] Elastic modulus: The elastic modulus was determined according to the test method in GB / T 1040.2-2006 Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics.

[0082] Leakage resistance: Take a set of test samples with a size of 100mm×100mm at intervals along the width of the film. If the width of the film is ≤1500mm, take 5 samples; if the width is >1500mm, take 8 samples. Place a 70mm diameter filter paper flat on the table, and then place the test sample in the center of the filter paper. Next, place another 70mm diameter filter paper on top of the test sample. Accurately measure 1mL of the prepared 0.2wt% Congo red aqueous solution using a pipette, and drop it into the center of the upper filter paper and let it stand for 1 minute. Press an acrylic plate with a size of 60mm×60mm×5mm (i.e., length and width are both 60mm, and thickness is 5mm) onto the surface of the filter paper, and apply an additional 200g weight to the acrylic plate and let it stand for 1 minute. After the test, remove the test sample and all upper coverings. If no red marks are found on the lower filter paper, the test sample is deemed to have passed the leakage resistance test. The PE film can be deemed to be qualified for leak-proof performance only if all test samples in a group meet this standard.

[0083] Example 1

[0084] S1. Mix 25% LLDPE resin, 20% LLDPE resin, 10% LDPE resin and 45% nano-sized calcium carbonate with a particle size of 400nm evenly to obtain a PE mixture weighing 10kg.

[0085] S2. The PE mixture is melted in a twin-screw extruder at a temperature of 200–210°C and kept at 210–230°C before being conveyed to the die cavity through a first runner at 250°C, a second runner at 235°C, and a third runner at 250°C. The melt in the first, second, and third runners converges at the die lip of the die at 240°C for three-layer co-extrusion, and then pressed by the casting steel roller and casting pressure roller to form a first intermediate film. The first intermediate film is then subjected to matte treatment and cooling to obtain a second intermediate film. The temperature of the casting steel roller and casting pressure roller is 25°C, and the mutual clamping force between the casting steel roller and casting pressure roller is 5 kg / cm². 2 ;

[0086] S3. The second intermediate film material is subjected to three-stage stepped preheating and three-stage stepped micro-stretching to obtain a third intermediate film material, which has a microporous structure. The specific method of the three-stage stepped preheating is as follows: the second intermediate film material is preheated in three stages using preheating rollers, with the preheating temperature of the first stage being 78℃, the preheating temperature of the second stage being 82℃, and the preheating temperature of the third stage being 88℃. The specific method of the three-stage stepped micro-stretching is as follows: the second intermediate film material, which has undergone three-stage stepped preheating, is micro-stretched in three stages using three stretching rollers, each at 88℃, with the stretching ratio of the first stage being 1.2, the stretching ratio of the second stage being 1.5, and the stretching ratio of the third stage being 1.8.

[0087] S4. The third intermediate film material is subjected to heat setting, cooling and embossing treatments in sequence to obtain the fourth intermediate film material; the surface of the fourth intermediate film material is subjected to corona treatment, and after winding, a low basis weight leak-proof PE film is obtained; wherein, the basis weight of the upper film layer, the intermediate film layer and the lower film layer are the same; the heat setting temperature is 100℃; the cooling temperature is 25℃; the corona current of the corona treatment is 4A.

[0088] Example 2

[0089] S1. Mix 30% LLDPE resin, 15% LLDPE resin, 9% LDPE resin and 46% nano-sized calcium carbonate with a particle size of 300nm to obtain a PE mixture weighing 10kg.

[0090] S2. The PE mixture is melted in a twin-screw extruder at 200℃ and conveyed at 220℃ to the first runner, second runner (235℃), and third runner (245℃) in the die cavity. The melt in the first, second, and third runners converges at the die lip at 230℃ for three-layer co-extrusion, and then pressed by the casting steel roller and casting pressure roller to form the first intermediate film. The first intermediate film is then subjected to matte treatment and cooling to obtain the second intermediate film. The temperature of the casting steel roller and casting pressure roller is 20℃, and the mutual clamping force between the casting steel roller and casting pressure roller is 4 kg / cm. 2 ;

[0091] S3. The second intermediate film material is subjected to three-stage stepped preheating and three-stage stepped micro-stretching to obtain a third intermediate film material, which has a microporous structure. The specific method of the three-stage stepped preheating is as follows: the second intermediate film material is preheated in three stages using preheating rollers, with the preheating temperature of the first stage being 77℃, the preheating temperature of the second stage being 81℃, and the preheating temperature of the third stage being 86℃. The specific method of the three-stage stepped micro-stretching is as follows: the second intermediate film material, which has undergone three-stage stepped preheating, is micro-stretched in three stages using three stretching rollers, each at 86℃, with the stretching ratio of the first stage being 1.1, the stretching ratio of the second stage being 1.3, and the stretching ratio of the third stage being 1.5.

[0092] S4. The third intermediate film material is subjected to heat setting, cooling and embossing treatments in sequence to obtain the fourth intermediate film material; the surface of the fourth intermediate film material is subjected to corona treatment, and after winding, a low basis weight leak-proof PE film is obtained; wherein, the basis weight of the upper film layer, the intermediate film layer and the lower film layer are the same; the heat setting temperature is 105℃; the cooling temperature is 30℃; the corona current of the corona treatment is 3A.

[0093] Example 3

[0094] S1. Mix 26% LLDPE resin, 21% LLDPE resin, 8% LDPE resin and 45% nano-sized calcium carbonate with a particle size of 600nm to obtain a PE mixture weighing 10kg.

[0095] S2. The PE mixture is melted in a twin-screw extruder at 200℃ and conveyed at 220℃ to the first runner (255℃), second runner (240℃), and third runner (255℃) in the die cavity. The melt in the first, second, and third runners merges at the die lip of the die head at 248℃ and undergoes three-layer co-extrusion. The resulting material is then pressed by the casting steel roller and casting pressure roller to form the first intermediate film. The first intermediate film is then subjected to matte treatment and cooling to obtain the second intermediate film. The temperature of both the casting steel roller and the casting pressure roller is 25℃, and the mutual clamping force between the casting steel roller and the casting pressure roller is 5 kg / cm². 2 ;

[0096] S3. The second intermediate membrane material is subjected to three-stage stepped preheating and three-stage stepped micro-stretching to obtain a third intermediate membrane material, which has a microporous structure. The specific method of the three-stage stepped preheating is as follows: the second intermediate membrane material is preheated in three stages using preheating rollers, with the preheating temperature of the first stage being 78℃, the preheating temperature of the second stage being 83℃, and the preheating temperature of the third stage being 89℃. The specific method of the three-stage stepped micro-stretching is as follows: the second intermediate membrane material, which has undergone three-stage stepped preheating, is micro-stretched in three stages using three stretching rollers, each at 86℃, with the stretching ratio of the first stage being 1.2, the stretching ratio of the second stage being 1.4, and the stretching ratio of the third stage being 1.6.

[0097] S4. The third intermediate film material is subjected to heat setting, cooling and embossing treatments in sequence to obtain the fourth intermediate film material; the surface of the fourth intermediate film material is subjected to corona treatment, and after winding, a low basis weight leak-proof PE film is obtained; wherein, the basis weight of the upper film layer, the intermediate film layer and the lower film layer are the same; the temperature of the heat setting treatment is 100-110℃; the temperature of the cooling treatment is 25-35℃, and the corona current of the corona treatment is 3-5A.

[0098] Comparative Example 1

[0099] The preparation method and raw materials of Comparative Example 1 are the same as those of Example 1, except that micron-sized calcium carbonate with a particle size of 2 μm is used in the PE mixture formulation of Comparative Example 1.

[0100] Comparative Example 2

[0101] Comparative Example 2 uses the same preparation method and raw materials as Example 1, except that a single-layer membrane structure is used in Comparative Example 2.

[0102] Comparative Example 3

[0103] The preparation method and raw materials of Comparative Example 3 are the same as those of Example 1, except that a single stretching is used in Comparative Example 3.

[0104] The PE films prepared in the above embodiments and comparative examples were subjected to performance tests, and the specific test results are shown in Table 1 below:

[0105] Table 1. Test results of relevant performance of PE film

[0106]

[0107] As can be seen from the performance test results of the embodiments in the table above, the PE film prepared by the method for preparing a low basis weight leak-proof PE film has a basis weight as low as 26 g / m³. 2With a water vapor permeability ≥1500g / (㎡.24h), transverse tensile strength ≥2.5N / 25mm, longitudinal tensile strength ≥10N / 25mm, transverse elongation at break ≥200%, longitudinal elongation at break ≥150%, and longitudinal heat shrinkage 3~6%, it not only has air permeability and leak-proof properties while ensuring low weight, but also has suitable shrinkage, high tensile strength and high elongation at break, meeting the product's usage requirements.

[0108] In Comparative Example 1, the use of micron-sized calcium carbonate resulted in a decrease in its impermeability, tensile strength, and elongation at break, while its air permeability increased.

[0109] Comparative Example 2, due to its use of a single-layer membrane structure, exhibited decreased impermeability, tensile strength, and elongation at break, while its air permeability increased.

[0110] Comparative Example 3, due to the use of single stretching, makes it difficult to form an ideal microporous structure, and the size and uniformity of the micropores are poor. At the same time, the resulting PE film is prone to stress concentration, which leads to a decrease in its leak-proof performance, tensile strength, air permeability and elongation at break.

[0111] The technical principles of the present invention have been described above with reference to specific embodiments. These descriptions are merely for explaining the principles of the invention and should not be construed as limiting the scope of protection of the invention in any way. Based on this explanation, those skilled in the art can readily conceive of other specific embodiments of the invention without inventive effort, and these embodiments will all fall within the scope of protection of the present invention.

Claims

1. A low-basis-weight, leak-proof PE membrane, characterized in that, The basis weight of the PE film is 26-28 g / m³. 2 Water vapor transmission rate ≥1500g / (m²) 2 .24h), transverse tensile strength ≥2.5N / 25mm, longitudinal tensile strength ≥10N / 25mm, transverse elongation at break ≥200%, longitudinal elongation at break ≥150%, longitudinal heat shrinkage 3~6%; The PE film comprises an upper film layer, an intermediate film layer, and a lower film layer distributed from top to bottom. The upper film layer, the intermediate film layer, and the lower film layer are all obtained by melt extrusion of PE film mixture, followed by three-stage micro-stretching and curing. The upper film layer, the intermediate film layer, and the lower film layer all have a microporous structure. The PE film mixture comprises the following raw materials by weight percentage: 20-30% LLDPE resin, 12-27% LLDPE resin, 8-10% LDPE resin, and 45-48% nano-grade calcium carbonate.

2. The low-basis-weight leak-proof PE membrane according to claim 1, characterized in that, The particle size of the nano-sized calcium carbonate is 200–700 nm.

3. The low-basis-weight leak-proof PE membrane according to claim 1, characterized in that, The upper film layer, the middle film layer, and the lower film layer all have the same weight.

4. A method for preparing a low-basis-weight, leak-proof PE membrane, characterized in that, The method for preparing a low-basis-weight leak-proof PE membrane as described in any one of claims 1 to 3 comprises the following steps: S1. Mix mLLDPE resin, LLDPE resin, LDPE resin and nano-sized calcium carbonate evenly according to the formula to obtain PE film mixture; S2. The PE film mixture is added to a twin-screw extruder for melting and then conveyed at a constant temperature to the first, second, and third flow channels of the die cavity. The melt in the first, second, and third flow channels converges at the die lip of the die head and undergoes three-layer co-extrusion. The mixture is then pressed by the casting steel roller and casting pressure roller to form the first intermediate film. The first intermediate film is then subjected to a matte finish and cooled to obtain the second intermediate film. S3. The second intermediate membrane material is subjected to three-stage step preheating and three-stage step micro-stretching to obtain the third intermediate membrane material, and the third intermediate membrane material has a microporous structure. S4. The third intermediate membrane material is subjected to heat setting, cooling and embossing treatment in sequence to obtain the fourth intermediate membrane material; the surface of the fourth intermediate membrane material is subjected to corona treatment, and after winding, a low-grammage leak-proof PE film is obtained.

5. The method for preparing a low-basis-weight leak-proof PE membrane according to claim 4, characterized in that, In step S3, the specific method of the three-stage stepped preheating is as follows: the second intermediate film material is preheated in the first stage, the second stage, and the third stage using a preheating roller, and the preheating temperature of the first stage is 75-80℃, the preheating temperature of the second stage is 81-85℃, and the preheating temperature of the third stage is 86-90℃.

6. The method for preparing a low-basis-weight, leak-proof PE membrane according to claim 4, characterized in that, In step S3, the specific method of the three-stage stepped micro-stretching is as follows: using three stretching rollers, each with a temperature of 85-95℃, to perform the first-stage micro-stretching, the second-stage micro-stretching, and the third-stage micro-stretching on the second intermediate film material that has undergone three-stage stepped preheating, respectively. The stretching ratio of the first-stage micro-stretching is 1.1-1.2, the stretching ratio of the second-stage micro-stretching is 1.2-1.5, and the stretching ratio of the third-stage micro-stretching is 1.5-1.

8.

7. The method for preparing a low-basis-weight, leak-proof PE membrane according to claim 4, characterized in that, In step S2, the temperature of both the casting steel roll and the casting pressure roll is 20–28°C, and the mutual clamping force between the casting steel roll and the casting pressure roll is 4–6 kg / cm². 2 .

8. The method for preparing a low-basis-weight leak-proof PE membrane according to claim 4, characterized in that, In step S4, the corona current of the corona treatment is 3 to 5 A.

Citation Information

Patent Citations

  • Special WVTR (water vapour transmission rate) breathable film and production process thereof

    CN103496239A

  • Polyethylene (PE) microporous breathable film for medical protective clothing and preparation method thereof