A flame-retardant epoxy resin coating and its preparation method

By preparing phosphorus-modified imidazole benzoxazine and chitosan-based flame retardants, the problems of flammability and poor antibacterial effect of epoxy resin coatings were solved, and the flame retardant and antibacterial effects were improved.

CN119684873BActive Publication Date: 2026-11-17FUJIAN KELANGYA DECORATION MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411953660.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-27
Publication Date
2026-11-17
Estimated Expiration
2044-12-27

AI Technical Summary

Technical Problem

Epoxy resin coatings are flammable and have poor antibacterial properties, which limits their application.

Method used

A coating with flame-retardant and antibacterial effects is formed by preparing phosphorus-modified imidazole benzoxazine and chitosan-based flame retardants and mixing them with bisphenol A type epoxy resin, propylene glycol, titanium dioxide, defoamer, leveling agent, wetting and dispersing agent and water.

Benefits of technology

It improves the flame retardant properties and antibacterial effects of the coating, forming a dense protective layer and glassy substance, thereby enhancing the flame retardant properties and antibacterial capabilities of the coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of coating technology and discloses a flame-retardant epoxy resin coating and its preparation method. The invention involves adding bisphenol A type epoxy resin, propylene glycol, phosphorus-modified imidazole benzoxazine, chitosan-based flame retardant, titanium dioxide, BYK-071 defoamer, BYK-345 leveling agent, BYK-220S wetting and dispersing agent, and water to a stirrer and stirring. After stirring, a flame-retardant epoxy resin coating is obtained. The phosphorus, silicon, and benzoxazine elements in the phosphorus-modified imidazole benzoxazine and the chitosan-based flame retardant all exhibit good flame-retardant effects. Chitosan itself in the chitosan-based flame retardant also has good flame-retardant and antibacterial effects. Benzoxazine forms a heat-resistant phenolic resin structure at high temperatures, giving it good flame-retardant properties; the imidazole groups in the phosphorus-modified imidazole benzoxazine also have good antibacterial effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, specifically to a flame-retardant epoxy resin coating and its preparation method. Background Technology

[0002] Epoxy resins possess excellent adhesion, electrical insulation, and mechanical strength, making them widely used in coatings, adhesives, and other fields. However, their flammability limits their application in coatings, and their antibacterial properties also need improvement. Therefore, avoiding these issues is key to solving the problem.

[0003] For example, patent CN108517170A discloses a flame-retardant epoxy coating and its preparation method. This invention first uses ammonium polyphosphate as a raw material and disperses it in dimethylethanolamine, which improves its dispersion compatibility with each raw material and enhances the surface strength and flame-retardant properties of the finished coating; however, its antibacterial effect is not improved. Summary of the Invention

[0004] (a) Technical problems to be solved

[0005] To address the shortcomings of existing technologies, this invention provides a flame-retardant epoxy resin coating and its preparation method, which exhibits good flame-retardant and antibacterial effects.

[0006] (II) Technical Solution

[0007] To achieve the above objectives, the present invention provides the following technical solution: a flame-retardant epoxy resin coating, comprising the following weight components: 40-65 parts by weight of bisphenol A type epoxy resin, 1-3 parts by weight of propylene glycol, 4-8 parts by weight of phosphorus-modified imidazolyl benzoxazine, 6-9 parts by weight of chitosan-based flame retardant, 0.8-1.3 parts by weight of titanium dioxide, 0.2-0.5 parts by weight of BYK-071 defoamer, 0.4-0.7 parts by weight of BYK-345 leveling agent, 0.5-0.7 parts by weight of BYK-220S wetting and dispersing agent, and 5-10 parts by weight of water;

[0008] The preparation method of the phosphorus-containing modified imidazolyl benzoxazine is as follows:

[0009] Step 1: Add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium and triethylamine catalyst to dichloromethane solvent, stir mechanically for 10-12 min, add carbon tetrachloride dropwise over an ice bath over 1-1.5 h, then remove the ice bath and continue the reaction at room temperature for 10-14 h. After the reaction is complete, wash with deionized water 2-4 times and vacuum dry at 40-60 °C for 18-24 h to obtain intermediate 1.

[0010] Step 2: Add 4-hydroxybenzyl chloride and intermediate 1 to isopropanol solvent, reflux at 60-85℃ for 12-15 h, after the reaction is completed, rotary evaporate, recrystallize from ethanol to obtain phenolyl imidazole;

[0011] Step 3: Add 7-12 parts by weight of phenol-based imidazole, 5-10 parts by weight of aniline, and 12-16 parts by weight of formaldehyde aqueous solution to the reaction flask. Reflux the mixture at 60-85℃, stir until homogeneous, then add 1-2 parts by weight of oxalic acid catalyst to carry out the reaction. After the reaction is complete, add water, allow the mixture to stand and separate into layers, filter and dry to obtain phosphorus-modified imidazole-based benzoxazine.

[0012] Preferably, in step one, the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium, triethylamine catalyst, and carbon tetrachloride is 1.1-1.3:1:0.01-0.02:0.5-0.8.

[0013] Preferably, in step two, the mass ratio of 4-hydroxybenzyl chloride to intermediate 1 is 1.5-1.8:1.

[0014] Preferably, the reaction time in step three is 4-8 hours.

[0015] Preferably, the preparation method of the chitosan-based flame retardant is as follows:

[0016] S1. Add octamethylcyclotetrasiloxane and 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane to the reactor, purge with nitrogen for protection, then continue to add tetramethylammonium hydroxide catalyst, react at 60-80℃ for 2-6 hours, cool and discharge after the reaction to obtain double-ended epoxy silicone oil.

[0017] S2. Add the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate to N,N-dimethylformamide solvent, stir and mix, continue to add boron trifluoride diethyl ether catalyst, react at 80-95℃ for 6-12h, filter after the reaction, wash with deionized water and ethanol in sequence, dry to obtain intermediate 2.

[0018] S3. Add 6-12 parts by weight of diphenylmethane diisocyanate to toluene solvent, purge with nitrogen, add 8-14 parts by weight of intermediate 2, react at 75-85℃ for 4-6 hours, add 5-9 parts by weight of purified chitosan, react at 60-75℃ for 5-7 hours, and obtain chitosan-based flame retardant after the reaction.

[0019] The method for preparing purified chitosan is as follows: Take 50g of chitosan and 300mL of distilled water, add them to a 500mL reactor, stir and dissolve at 90℃, filter while hot, cool and crystallize, and vacuum dry at 80℃ for 24h to obtain purified chitosan.

[0020] Preferably, the mass ratio of octamethylcyclotetrasiloxane, 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane, and tetramethylammonium hydroxide catalyst in S1 is 0.8-1.2:1:0.02-0.03.

[0021] Preferably, the mass ratio of the double-ended epoxy silicone oil, 4-hydroxymethyl cage-like bicyclic phosphate, and boron trifluoride diethyl ether catalyst in S2 is 1:1.4-1.7:0.01-0.023.

[0022] Preferably, the method for preparing the flame-retardant epoxy resin coating is as follows: bisphenol A type epoxy resin, propylene glycol, phosphorus-modified imidazole benzoxazine, chitosan-based flame retardant, titanium dioxide, BYK-071 defoamer, BYK-345 leveling agent, BYK-220S wetting and dispersing agent, and water are added to a stirrer and stirred for 4-6 minutes. After stirring, the flame-retardant epoxy resin coating is obtained.

[0023] (III) Beneficial Technical Effects

[0024] This invention involves adding bisphenol A type epoxy resin, propylene glycol, phosphorus-modified imidazole benzoxazine, chitosan-based flame retardant, titanium dioxide, BYK-071 defoamer, BYK-345 leveling agent, BYK-220S wetting and dispersing agent, and water into a stirrer, stirring, and then obtaining a flame-retardant epoxy resin coating.

[0025] The phosphorus, silicon, and benzoxazine elements in phosphorus-modified imidazole-based benzoxazine and chitosan-based flame retardants all exhibit good flame-retardant effects. Chitosan itself in chitosan-based flame retardants also possesses good flame-retardant and antibacterial properties. During combustion, phosphorus generates highly dehydrating polyphosphoric acid and metaphosphoric acid. Because polyphosphoric acid and metaphosphoric acid are not easily volatilized, they can form a dense protective layer on the coating surface, thus achieving a flame-retardant effect. Silicon, when heated, can produce a glassy substance on the material surface, isolating mass transport and energy transfer. Benzoxazine forms a heat-resistant phenolic resin structure at high temperatures, giving it good flame-retardant properties. The phenolic hydroxyl groups in the formed phenolic resin cross-link and cure with the epoxy groups of bisphenol A type epoxy resin, improving their compatibility. Simultaneously, it forms a cured system with the imidazole groups in the phosphorus-modified imidazole-based benzoxazine. The imidazole group in phosphorus-modified imidazole benzoxazine also has a good antibacterial effect; and after the reaction between the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate, the degree of phosphorus substitution is increased, which further improves its flame retardant effect. Detailed Implementation

[0026] Example 1

[0027] (1) Add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium and triethylamine catalyst to dichloromethane solvent, stir mechanically for 10 min, and add carbon tetrachloride under ice bath conditions. The mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium, triethylamine catalyst and carbon tetrachloride is 1.1:1:0.01:0.5. The addition is completed dropwise within 1 h. Then remove the ice bath and continue to react at room temperature for 10 h. After the reaction is completed, wash twice with deionized water and dry under vacuum at 40 °C for 18 h to obtain intermediate 1.

[0028] (2) Add 4-hydroxybenzyl chloride and intermediate 1 to isopropanol solvent, wherein the mass ratio of 4-hydroxybenzyl chloride to intermediate 1 is 1.5:1, reflux at 60°C for 12 h, after the reaction is completed, rotary evaporate, recrystallize from ethanol to obtain phenolimazole.

[0029] (3) Add 7 parts by weight of phenol-based imidazole, 5 parts by weight of aniline, and 12 parts by weight of formaldehyde aqueous solution to the reaction flask. Reflux at 60°C, stir evenly, add 1 part by weight of oxalic acid catalyst, react for 4 hours, add water after reaction, let stand to separate into layers, filter and dry to obtain phosphorus-modified imidazole-based benzoxazine.

[0030] (4) Add octamethylcyclotetrasiloxane and 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane to the reactor, purge with nitrogen, and then add tetramethylammonium hydroxide catalyst. The mass ratio of octamethylcyclotetrasiloxane, 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide catalyst is 0.8:1:0.02. React at 60°C for 2 hours. After the reaction is completed, cool and discharge the product to obtain double-ended epoxy silicone oil.

[0031] (5) Add the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate to N,N-dimethylformamide solvent, stir and mix, and continue to add boron trifluoride diethyl ether catalyst, wherein the mass ratio of double-ended epoxy silicone oil, 4-hydroxymethyl cage-like bicyclic phosphate and boron trifluoride diethyl ether catalyst is 1:1.4:0.01, react at 80℃ for 6h, filter after the reaction, wash with deionized water and ethanol in sequence, and dry to obtain intermediate 2;

[0032] (6) Add 6 parts by weight of diphenylmethane diisocyanate to toluene solvent, purge with nitrogen gas, add 8 parts by weight of intermediate 2, react at 75°C for 4 hours, add 5 parts by weight of purified chitosan, react at 60°C for 5 hours, and obtain chitosan-based flame retardant after the reaction.

[0033] (7) Add 40 parts by weight of bisphenol A type epoxy resin, 1 part by weight of propylene glycol, 4 parts by weight of phosphorus-modified imidazolyl benzoxazine, 6 parts by weight of chitosan-based flame retardant, 0.8 parts by weight of titanium dioxide, 0.2 parts by weight of BYK-071 defoamer, 0.4 parts by weight of BYK-345 leveling agent, 0.5 parts by weight of BYK-220S wetting and dispersing agent, and 5 parts by weight of water to a stirrer and stir for 4 minutes. After stirring, a flame-retardant epoxy resin coating is obtained.

[0034] Example 2

[0035] (1) Add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium and triethylamine catalyst to dichloromethane solvent, stir mechanically for 10-12 min, and add carbon tetrachloride under ice bath conditions. The mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium, triethylamine catalyst and carbon tetrachloride is 1.3:1:0.02:0.8. The addition is completed dropwise within 1.5 h. Then remove the ice bath and continue to react at room temperature for 14 h. After the reaction is completed, wash with deionized water 4 times and dry under vacuum at 60 °C for 24 h to obtain intermediate 1.

[0036] (2) Add 4-hydroxybenzyl chloride and intermediate 1 to isopropanol solvent, wherein the mass ratio of 4-hydroxybenzyl chloride to intermediate 1 is 1.8:1, reflux at 85°C for 15 h, after the reaction is completed, rotary evaporate, recrystallize from ethanol to obtain phenolimazole.

[0037] (3) Add 12 parts by weight of phenol-based imidazole, 10 parts by weight of aniline, and 16 parts by weight of formaldehyde aqueous solution to the reaction flask. Reflux at 85°C, stir evenly, add 2 parts by weight of oxalic acid catalyst, react for 8 hours, add water after reaction, let stand to separate into layers, filter and dry to obtain phosphorus-modified imidazole-based benzoxazine.

[0038] (4) Octamethylcyclotetrasiloxane and 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane were added to the reactor, and nitrogen gas was introduced for protection. Then, tetramethylammonium hydroxide catalyst was added. The mass ratio of octamethylcyclotetrasiloxane, 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide catalyst was 1.2:1:0.03. The reaction was carried out at 80°C for 6 hours. After the reaction was completed, the product was cooled and discharged to obtain double-ended epoxy silicone oil.

[0039] (5) Add the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate to N,N-dimethylformamide solvent, stir and mix, and continue to add boron trifluoride diethyl ether catalyst, wherein the mass ratio of double-ended epoxy silicone oil, 4-hydroxymethyl cage-like bicyclic phosphate and boron trifluoride diethyl ether catalyst is 1:1.7:0.023, react at 95℃ for 12h, filter after the reaction, wash with deionized water and ethanol in sequence, and dry to obtain intermediate 2;

[0040] (6) 12 parts by weight of diphenylmethane diisocyanate were added to toluene solvent, nitrogen gas was introduced for protection, 14 parts by weight of intermediate 2 were added, and the reaction was carried out at 85°C for 6 hours. Then, 9 parts by weight of purified chitosan were added, and the reaction was carried out at 75°C for 7 hours. After the reaction was completed, chitosan-based flame retardant was obtained.

[0041] (7) Add 65 parts by weight of bisphenol A type epoxy resin, 3 parts by weight of propylene glycol, 8 parts by weight of phosphorus-modified imidazolyl benzoxazine, 9 parts by weight of chitosan-based flame retardant, 1.3 parts by weight of titanium dioxide, 0.5 parts by weight of BYK-071 defoamer, 0.7 parts by weight of BYK-345 leveling agent, 0.7 parts by weight of BYK-220S wetting and dispersing agent, and 10 parts by weight of water to a stirrer and stir for 6 minutes. After stirring, a flame-retardant epoxy resin coating is obtained.

[0042] Example 3

[0043] (1) Add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium and triethylamine catalyst to dichloromethane solvent, stir mechanically for 11 min, and add carbon tetrachloride under ice bath conditions. The mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium, triethylamine catalyst and carbon tetrachloride is 1.2:1:0.015:0.7. The addition is completed dropwise within 1.2 h. Then remove the ice bath and continue to react at room temperature for 12 h. After the reaction is completed, wash with deionized water 3 times and dry under vacuum at 50 °C for 22 h to obtain intermediate 1.

[0044] (2) Add 4-hydroxybenzyl chloride and intermediate 1 to isopropanol solvent, wherein the mass ratio of 4-hydroxybenzyl chloride to intermediate 1 is 1.6:1, reflux at 75°C for 14 h, after the reaction is completed, rotary evaporate, recrystallize from ethanol to obtain phenolimazole;

[0045] (3) Add 10 parts by weight of phenol-based imidazole, 8 parts by weight of aniline, and 14 parts by weight of formaldehyde aqueous solution to the reaction flask. Reflux at 75°C, stir evenly, add 1 part by weight of oxalic acid catalyst, react for 6 hours, add water after reaction, let stand to separate into layers, filter and dry to obtain phosphorus-modified imidazole-based benzoxazine.

[0046] (4) Add octamethylcyclotetrasiloxane and 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane to the reactor, purge with nitrogen, and then add tetramethylammonium hydroxide catalyst. The mass ratio of octamethylcyclotetrasiloxane, 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide catalyst is 0.9:1:0.02. React at 70°C for 5 hours. After the reaction is completed, cool and discharge the product to obtain double-ended epoxy silicone oil.

[0047] (5) Add the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate to N,N-dimethylformamide solvent, stir and mix, and continue to add boron trifluoride diethyl ether catalyst, wherein the mass ratio of double-ended epoxy silicone oil, 4-hydroxymethyl cage-like bicyclic phosphate and boron trifluoride diethyl ether catalyst is 1:1.5:0.02, react at 75℃ for 10h, filter after the reaction, wash with deionized water and ethanol in sequence, and dry to obtain intermediate 2;

[0048] (6) Add 10 parts by weight of diphenylmethane diisocyanate to toluene solvent, purge with nitrogen gas, add 12 parts by weight of intermediate 2, react at 78°C for 5 h, add 7 parts by weight of purified chitosan, react at 65°C for 6 h, and obtain chitosan-based flame retardant after the reaction.

[0049] (7) Add 55 parts by weight of bisphenol A type epoxy resin, 2 parts by weight of propylene glycol, 6 parts by weight of phosphorus-modified imidazolyl benzoxazine, 8 parts by weight of chitosan-based flame retardant, 0.9 parts by weight of titanium dioxide, 0.4 parts by weight of BYK-071 defoamer, 0.6 parts by weight of BYK-345 leveling agent, 0.6 parts by weight of BYK-220S wetting and dispersing agent, and 8 parts by weight of water to a stirrer and stir for 5 minutes. After stirring, a flame-retardant epoxy resin coating is obtained.

[0050] Example 4

[0051] (1) Add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium and triethylamine catalyst to dichloromethane solvent, stir mechanically for 10 min, and add carbon tetrachloride under ice bath conditions. The mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium, triethylamine catalyst and carbon tetrachloride is 1.1:1:0.01:0.5. The addition is completed dropwise within 1 h. Then remove the ice bath and continue to react at room temperature for 10 h. After the reaction is completed, wash twice with deionized water and dry under vacuum at 40 °C for 18 h to obtain intermediate 1.

[0052] (2) Add 4-hydroxybenzyl chloride and intermediate 1 to isopropanol solvent, wherein the mass ratio of 4-hydroxybenzyl chloride to intermediate 1 is 1.5:1, reflux at 60°C for 12 h, after the reaction is completed, rotary evaporate, recrystallize from ethanol to obtain phenolimazole.

[0053] (3) Add 12 parts by weight of phenol-based imidazole, 10 parts by weight of aniline, and 16 parts by weight of formaldehyde aqueous solution to the reaction flask. Reflux at 85°C, stir evenly, add 2 parts by weight of oxalic acid catalyst, react for 8 hours, add water after reaction, let stand to separate into layers, filter and dry to obtain phosphorus-modified imidazole-based benzoxazine.

[0054] (4) Octamethylcyclotetrasiloxane and 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane were added to the reactor, and nitrogen gas was introduced for protection. Then, tetramethylammonium hydroxide catalyst was added. The mass ratio of octamethylcyclotetrasiloxane, 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide catalyst was 1.2:1:0.03. The reaction was carried out at 80°C for 6 hours. After the reaction was completed, the product was cooled and discharged to obtain double-ended epoxy silicone oil.

[0055] (5) Add the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate to N,N-dimethylformamide solvent, stir and mix, and continue to add boron trifluoride diethyl ether catalyst, wherein the mass ratio of double-ended epoxy silicone oil, 4-hydroxymethyl cage-like bicyclic phosphate and boron trifluoride diethyl ether catalyst is 1:1.5:0.02, react at 75℃ for 10h, filter after the reaction, wash with deionized water and ethanol in sequence, and dry to obtain intermediate 2;

[0056] (6) Add 10 parts by weight of diphenylmethane diisocyanate to toluene solvent, purge with nitrogen gas, add 12 parts by weight of intermediate 2, react at 78°C for 5 h, add 7 parts by weight of purified chitosan, react at 65°C for 6 h, and obtain chitosan-based flame retardant after the reaction.

[0057] (7) Add 55 parts by weight of bisphenol A type epoxy resin, 2 parts by weight of propylene glycol, 6 parts by weight of phosphorus-modified imidazolyl benzoxazine, 8 parts by weight of chitosan-based flame retardant, 0.9 parts by weight of titanium dioxide, 0.4 parts by weight of BYK-071 defoamer, 0.6 parts by weight of BYK-345 leveling agent, 0.6 parts by weight of BYK-220S wetting and dispersing agent, and 8 parts by weight of water to a stirrer and stir for 5 minutes. After stirring, a flame-retardant epoxy resin coating is obtained.

[0058] Comparative Example 1

[0059] The difference between this comparative example and Example 4 is that no phosphorus-modified imidazolybenzaoxazine was added.

[0060] Comparative Example 2

[0061] The difference between this comparative example and Example 4 is that no chitosan-based flame retardant was added.

[0062] The limiting oxygen index of the coating was tested using an oxygen index meter, and the flammability rating of the coating was tested using a horizontal and vertical burner. The test results are shown in Table 1.

[0063] Table 1: Flame retardancy test.

[0064] project Limiting oxygen index (%) flammability rating Example 1 31.4 V-0 Example 2 32.6 V-0 Example 3 31.5 V-0 Example 4 31.9 V-0 Comparative Example 1 21.4 V-1 Comparative Example 2 20.3 V-1

[0065] As shown in Table 1, Examples 1-4 of the present invention have better flame retardant effects compared with Comparative Examples 1-2.

[0066] Transfer 1 mL of a 10 concentration 8 Add CFU / mL Staphylococcus aureus bacterial suspension to PBS buffer, vortex until homogeneous, and then dilute 10-fold to 10⁻⁶. 5 Add CFU / mL of the coating sample (1cm×1cm×0.2mm) and incubate at 37℃ with shaking for 24h. After incubation, add PBS buffer to dilute the bacterial solution 10-fold. Then, transfer 0.5mL of the bacterial solution to agar medium and continue to incubate at 37℃ with shaking for 24h. After incubation, count the colonies and count the inhibition rate.

[0067] Table 2: Antibacterial performance test.

[0068] project Antibacterial rate (%) Example 1 98.3 Example 2 99.9 Example 3 98.7 Example 4 98.4 Comparative Example 1 81.2 Comparative Example 2 80.6

[0069] As shown in Table 2, Examples 1-4 of the present invention have better antibacterial effects compared with Comparative Examples 1-2.

[0070] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A flame-retardant epoxy resin coating, characterized in that, It comprises the following components by weight: 40-65 parts by weight of bisphenol A type epoxy resin, 1-3 parts by weight of propylene glycol, 4-8 parts by weight of phosphorus-modified imidazolyl benzoxazine, 6-9 parts by weight of chitosan-based flame retardant, 0.8-1.3 parts by weight of titanium dioxide, 0.2-0.5 parts by weight of BYK-071 defoamer, 0.4-0.7 parts by weight of BYK-345 leveling agent, 0.5-0.7 parts by weight of BYK-220S wetting and dispersing agent, and 5-10 parts by weight of water; The phosphorus-modified imidazolylbenzoxazine is prepared by the following method: Step 1: Add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium and triethylamine catalyst to dichloromethane solvent, stir mechanically for 10-12 min, add carbon tetrachloride dropwise over an ice bath over 1-1.5 h, then remove the ice bath and continue the reaction at room temperature for 10-14 h. After the reaction is complete, wash with deionized water 2-4 times and vacuum dry at 40-60 °C for 18-24 h to obtain intermediate 1. Step 2: Add 4-hydroxybenzyl chloride and intermediate 1 to isopropanol solvent, reflux at 60-85℃ for 12-15 h, after the reaction is completed, rotary evaporate, recrystallize from ethanol to obtain phenolyl imidazole; Step 3: Add 7-12 parts by weight of phenol-based imidazole, 5-10 parts by weight of aniline, and 12-16 parts by weight of formaldehyde aqueous solution to the reaction flask. Reflux the mixture at 60-85℃, stir until homogeneous, then add 1-2 parts by weight of oxalic acid catalyst to carry out the reaction. After the reaction is complete, add water, allow the mixture to stand and separate into layers, filter and dry to obtain phosphorus-modified imidazole-based benzoxazine.

2. The flame-retardant epoxy resin coating according to claim 1, characterized in that, In step one, the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 1-(3-aminopropyl)imidazolium, triethylamine catalyst, and carbon tetrachloride is 1.1-1.3:1:0.01-0.02:0.5-0.

8.

3. The flame-retardant epoxy resin coating according to claim 1, characterized in that, In step two, the mass ratio of 4-hydroxybenzyl chloride to intermediate 1 is 1.5-1.8:

1.

4. The flame-retardant epoxy resin coating according to claim 1, characterized in that, The reaction time in step three is 4-8 hours.

5. The flame-retardant epoxy resin coating according to claim 1, characterized in that, The chitosan-based flame retardant is prepared by the following method: S1. Add octamethylcyclotetrasiloxane and 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane to the reactor, purge with nitrogen for protection, then continue to add tetramethylammonium hydroxide catalyst, react at 60-80℃ for 2-6 hours, cool and discharge after the reaction to obtain double-ended epoxy silicone oil. S2. Add the double-ended epoxy silicone oil and 4-hydroxymethyl cage-like bicyclic phosphate to N,N-dimethylformamide solvent, stir and mix, continue to add boron trifluoride diethyl ether catalyst, react at 80-95℃ for 6-12h, filter after the reaction, wash with deionized water and ethanol in sequence, dry to obtain intermediate 2. S3. Add 6-12 parts by weight of diphenylmethane diisocyanate to toluene solvent, purge with nitrogen, and continue to add 8-14 parts by weight of intermediate 2. React at 75-85℃ for 4-6 hours. Then add 5-9 parts by weight of purified chitosan and react at 60-75℃ for 5-7 hours. After the reaction is complete, chitosan-based flame retardant is obtained.

6. The flame-retardant epoxy resin coating according to claim 5, characterized in that, The mass ratio of octamethylcyclotetrasiloxane, 1,3-diglycidyl etheroxypropyl-1,1,3,3-tetramethyldisiloxane, and tetramethylammonium hydroxide catalyst in S1 is 0.8-1.2:1:0.02-0.

03.

7. The flame-retardant epoxy resin coating according to claim 5, characterized in that, The mass ratio of the dual-terminal epoxy silicone oil, 4-hydroxymethyl cage-like bicyclic phosphate, and boron trifluoride diethyl ether catalyst in S2 is 1:1.4-1.7:0.01-0.

023.

8. A method for preparing a flame-retardant epoxy resin coating as described in any one of claims 1-7, characterized in that, The method for preparing the flame-retardant epoxy resin coating is as follows: Bisphenol A type epoxy resin, propylene glycol, phosphorus-modified imidazole benzoxazine, chitosan-based flame retardant, titanium dioxide, BYK-071 defoamer, BYK-345 leveling agent, BYK-220S wetting and dispersing agent, and water are added to a stirrer and stirred for 4-6 minutes. After stirring, the flame-retardant epoxy resin coating is obtained.

Citation Information

Patent Citations

  • Flame-retardant epoxy paint and preparation method thereof

    CN108517170A

  • Compound containing benzoxazine structure, resin composition, prepreg, electric copper-clad plate and preparation method and application thereof

    CN114957156A