A high-gloss varnish with UV aging resistance and abrasion resistance, its preparation method, and its application.

By combining self-made silicone-modified polyurethane resin with hydroxyl acrylic resin, the performance degradation problem of existing clear varnishes under ultraviolet light and abrasion was solved, resulting in a high-gloss clear varnish with high resistance to ultraviolet aging, abrasion resistance and impact toughness, suitable for outdoor equipment and vehicles.

CN119735981BActive Publication Date: 2026-11-17MARINE CHEM RES INST CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510033731.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-01-09
Publication Date
2026-11-17
Estimated Expiration
2045-01-09

AI Technical Summary

Technical Problem

Existing varnishes are difficult to combine high resistance to UV aging, abrasion resistance, and impact toughness, resulting in a decline in the performance of the protective coating under UV radiation and abrasion, affecting its service life and safety.

Method used

By combining self-made silicone-modified polyurethane resin with hydroxyl acrylic resin and adjusting the additive components, a wear-resistant high-gloss varnish is formed, which improves the coating's anti-aging and scratch resistance, while also enhancing its impact toughness and high and low temperature alternating performance.

Benefits of technology

This high-gloss clear varnish achieves high resistance to UV aging and abrasion, maintains good gloss and mechanical properties, and improves the coating's anti-aging and scratch resistance, making it suitable for equipment and vehicles in outdoor environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005234925630000131
    Figure BDA0005234925630000131
  • Figure BDA0005234925630000141
    Figure BDA0005234925630000141
Patent Text Reader

Abstract

This invention relates to the field of functional coatings, specifically to a high-gloss clear varnish with UV aging resistance and abrasion resistance, its preparation method, and its application. The invention first develops an organosilicon-modified polyurethane resin. This self-made organosilicon-modified polyurethane resin is then combined with a hydroxyl acrylic resin as a resin component in the clear varnish formulation. Further adjustments are made to the additive components in the clear varnish formulation to obtain an abrasion-resistant high-gloss clear varnish that balances UV aging resistance, abrasion resistance, and impact toughness. The abrasion-resistant high-gloss clear varnish provided by this invention, when applied to a colored paint surface, exhibits excellent adhesion to the paint, effectively improving the coating's anti-aging and scratch resistance. It also demonstrates good impact toughness and high / low temperature alternating performance, while maintaining a gloss level above 90°.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional coatings, and more specifically, to a high-gloss clear varnish with UV aging resistance and abrasion resistance, its preparation method, and its application. Background Technology

[0002] Protective coatings are applied to the surfaces of transportation vehicles such as airplanes, high-speed trains, and automobiles. The purpose of these coatings is to protect their surfaces from chemical or electrochemical reactions with the surrounding environment, preventing or delaying surface damage. Simultaneously, these protective coatings also provide a decorative function to the vehicle surfaces. With development, the demand for protective coatings is constantly increasing, and the performance requirements for these coatings are evolving from simple corrosion prevention and aesthetics to better aging resistance, wear resistance, and resistance to environmental changes.

[0003] The most common problems encountered by protective coatings on aircraft, high-speed trains, and automobiles during use are UV aging and surface scratches. Protective coatings age under prolonged UV exposure, the most obvious impact being loss of gloss and discoloration of the paint film. Severe aging can lead to chalking, and even reduced strength, cracking, blistering, crazing, and peeling, rendering the protective coating ineffective. During high-speed operation, protective coatings are easily scratched by rainwater, dust, gravel, and other debris carried by airflow, forming scratches. In severe cases, these scratches may penetrate the coating, exposing the substrate and accelerating surface corrosion, causing the coating to lose its protective performance and shortening its service life. Both UV aging and surface scratches significantly affect the performance of protective coatings and may even threaten driving safety.

[0004] As the outermost layer of the protective coating, varnish is applied over the primer and topcoat. Existing varnishes often fail to achieve a protective coating that simultaneously possesses high resistance to UV aging and abrasion while maintaining good mechanical properties. Summary of the Invention

[0005] Technical problem to be solved: The protective coating formed by existing varnishes is difficult to combine high resistance to UV aging, abrasion resistance and impact toughness.

[0006] This invention first develops an organosilicon-modified polyurethane resin. This self-made organosilicon-modified polyurethane resin is then combined with hydroxyl acrylic resin as a resin component in a clear varnish formulation. Further adjustments are made to the additive components in the clear varnish formulation to obtain a wear-resistant, high-gloss clear varnish that balances UV aging resistance, abrasion resistance, and impact toughness. The wear-resistant, high-gloss clear varnish provided by this invention, when applied to a colored paint surface, exhibits excellent adhesion to the paint, effectively improving the coating's anti-aging and scratch resistance. It also demonstrates good impact toughness and high / low temperature alternating performance, while maintaining a gloss level above 90°.

[0007] One of the objectives of this invention is to provide a high-gloss varnish (hereinafter referred to as high-gloss varnish) with high resistance to ultraviolet aging and abrasion.

[0008] The high-gloss varnish with high resistance to UV aging and abrasion includes a base material, a curing agent, and a diluent; the weight ratio of the base material, curing agent, and diluent is 2:(1.0-1.3):(1.2-2.4), preferably 2:(1.1-1.2):(1.8-2.4);

[0009] Based on a total weight of 100 parts by weight, the base material comprises the following components:

[0010] 20-40 parts by weight of silicone-modified polyurethane resin, preferably 25-35 parts by weight;

[0011] 30-60 parts by weight of hydroxyl acrylic resin, preferably 35-55 parts by weight;

[0012] The anti-sagging agent is used in amounts of 1.0-3.5 parts by weight, preferably 2.0-3.0 parts by weight;

[0013] The defoamer is used in an amount of 0.1-0.5 parts by weight, preferably 0.1-0.3 parts by weight;

[0014] The leveling agent is used in an amount of 0.5-2.0 parts by weight, preferably 0.5-1.5 parts by weight;

[0015] 1-10 parts by weight of light stabilizer, preferably 2-5 parts by weight;

[0016] 1-10 parts by weight of ultraviolet absorber, preferably 2-5 parts by weight;

[0017] The base solvent is 5-25 parts by weight, preferably 10-20 parts by weight;

[0018] Based on 100 parts by weight of the cured material, the cured material comprises the following components:

[0019] 70-100 parts by weight of curing agent, preferably 75-100 parts by weight;

[0020] The curing agent solvent is 0-30 parts by weight, preferably 0-25 parts by weight.

[0021] The hydroxyl acrylic resin can be any existing hydroxyl acrylic resin suitable for use in varnishes. Preferably, the hydroxyl acrylic resin has a hydroxyl value of 150 or higher; the hydroxyl value is defined as the number of milligrams of potassium hydroxide equivalent to the hydroxyl groups in 1g of sample. Specifically, at least one of the following can be used: Zhanxin 2155 acrylic resin, Zhanxin 4266 acrylic resin, Zhanxin 2810 acrylic resin, and Mitsubishi Chemical 7908 acrylic resin.

[0022] The anti-sagging agent can be any existing anti-sagging agent that can be used in varnishes. As a preferred embodiment, the anti-sagging agent is at least one of modified polyamide solution-based anti-sagging agents (such as anti-sagging additive BYK 430) and modified urea-based anti-sagging agents (such as anti-sagging agents BYK410, VOK-7410ET, etc.).

[0023] The defoamer can be any existing defoamer that can be used in varnishes. As a preferred embodiment, the defoamer is at least one of a defoaming polymer solution (such as defoamer BYK054, BYK057, etc.) or a polysiloxane solution (such as defoamer BYK024).

[0024] The leveling agent can be any existing leveling agent that can be used in varnishes. As a preferred embodiment, the leveling agent is at least one of the following: polyether-modified silicone leveling agent (e.g., leveling agent BYK333), acrylate leveling agent (e.g., leveling agent BYK354), or fluorocarbon-modified polyacrylate polymer (e.g., leveling agent AFCONA-3700).

[0025] The light stabilizer can be any existing light stabilizer that can be used in varnishes. As a preferred embodiment, the light stabilizer is at least one of hindered amine light stabilizers (such as light stabilizers UV-292, UV-123, etc.) or composite light stabilizers (such as light stabilizer UV-791).

[0026] The UV absorber can be any existing UV absorber suitable for use in varnishes. Preferably, the UV absorber is at least one of a triazine UV absorber (e.g., UV-1164) or a benzotriazole UV absorber (e.g., UV-326, UV-328, etc.). The combination of UV absorbers with different mechanisms of action and UV-resistant additives can significantly improve UV aging resistance.

[0027] The base solvent can be any existing base solvent that can be used in varnishes. As a preferred embodiment, the base solvent is one or more of butyl acetate, methyl isobutyl ketone, and propylene glycol methyl ether acetate.

[0028] The curing agent can be any existing curing agent suitable for varnishes. Preferably, the curing agent is an aliphatic isocyanate compound with good weather resistance, more preferably a hexamethylene diisocyanate biuret curing agent or an HDI trimer curing agent; for example, Desmodur N75, Desmodur N100, Desmodur N3375, Desmodur N3390, etc.

[0029] The curing agent solvent can be any existing curing agent solvent that can be used for varnishes. As a preferred embodiment, the curing agent solvent is at least one selected from ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, and methyl isobutyl ketone.

[0030] The diluent can be any existing diluent suitable for use in varnishes. Preferably, the diluent contains butyl acetate, and more preferably is composed of ethyl acetate, butyl acetate, methyl isobutyl ketone, and propylene glycol methyl ether acetate in a mass ratio of (0.1-2):(4-6):(0.1-3):(0.1-3).

[0031] The silicone-modified polyurethane resin is a self-made product of this invention. The silicone-modified polyurethane resin is obtained by stepwise polymerization of raw materials including hydroxyl-terminated polydimethylsiloxane, polycaprolactone polyol, diisocyanate, chain extender, and catalyst, followed by the addition of a solvent.

[0032] The preparation method of the organosilicon-modified polyurethane resin includes the following steps:

[0033] (1) Mix polycaprolactone polyol, diisocyanate and hydroxyl-terminated polydimethylsiloxane thoroughly and react at 75-85℃ for 1.5-2h under nitrogen protection;

[0034] (2) Cool down to 40-50℃, add chain extender and catalyst, and mix thoroughly;

[0035] (3) Heat to 70-80℃ and react for 2-3 hours;

[0036] (4) Cool down to 50-60℃, add solvent, stir evenly, and obtain the organosilicon modified polyurethane resin.

[0037] In the raw materials for preparing the silicone-modified polyurethane resin, the hydroxyl-terminated polydimethylsiloxane can be selected from a wide range. Variations in the molecular weight of the hydroxyl-terminated polydimethylsiloxane affect the performance of the prepared silicone-modified polyurethane resin in high-gloss varnishes. Preferably, the number-average molecular weight of the hydroxyl-terminated polydimethylsiloxane is 500-3500, more preferably 1000-3000.

[0038] In the raw materials for preparing the silicone-modified polyurethane resin, the polycaprolactone polyol can be selected within a wide range. Variations in the molecular weight of the polycaprolactone polyol affect the performance of the prepared silicone-modified polyurethane resin in high-gloss varnishes. Preferably, the number-average molecular weight of the polycaprolactone polyol is 300-2500, more preferably 1000-2000.

[0039] In the raw materials for preparing the silicone-modified polyurethane resin, the diisocyanate is one or more of dicyclohexylmethane diisocyanate or isoflurane diisocyanate. Both dicyclohexylmethane diisocyanate and isoflurane diisocyanate are aliphatic isocyanates and do not contain benzene rings in their structure, which can increase the anti-yellowing properties of the silicone-modified polyurethane resin in high-gloss clear varnishes. The selected HMDI and IPDI both contain cyclohexane structures similar to benzene rings and have good reactivity, enabling the prepared silicone-modified polyurethane resin to exhibit excellent impact and tear resistance in high-gloss clear varnishes.

[0040] In the raw materials for preparing the silicone-modified polyurethane resin, the chain extender can be any chain extender suitable for the synthesis of silicone-modified resins. Preferably, the chain extender is either 1,4-butanediol or ethylene glycol.

[0041] In the raw materials for preparing the organosilicon-modified polyurethane resin, the catalyst can be any catalyst suitable for the synthesis of organosilicon-modified resins. As a preferred embodiment, the catalyst is dibutyltin dilaurate (DBTDL).

[0042] In the raw materials for preparing the organosilicon-modified polyurethane resin, the solvent can be any solvent suitable for the synthesis of organosilicon-modified resin. As a preferred embodiment, the solvent is composed of ethyl acetate, butyl acetate, and methyl isobutyl ketone in a mass ratio of (1-3):(4-6):(1-3).

[0043] The amounts of raw materials used in preparing the silicone-modified polyurethane resin can be selected within a wide range. Variations in the proportions of the raw materials used in preparing the silicone-modified polyurethane resin will affect the performance of the prepared silicone-modified polyurethane resin in high-gloss clear varnishes. As a preferred embodiment, based on 100% of the total weight of raw materials and solvents: 30%-55% polycaprolactone polyol, 5%-25% hydroxyl-terminated polydimethylsiloxane, 20%-40% diisocyanate, 5%-15% chain extender, and 0.5%-1% catalyst. More preferably, based on 100% of the total weight of raw materials: 35%-55% polycaprolactone polyol, 10%-20% hydroxyl-terminated polydimethylsiloxane, 20%-35% diisocyanate, 5%-12% chain extender, and 0.1%-0.5% catalyst.

[0044] Compared with existing silicone-modified resins, the silicone-modified polyurethane resin prepared in this invention has a higher crosslinking density, and its hardness is significantly improved after forming a film with high-hydroxy acrylate and curing agent. Normally, increasing the crosslinking density of silicone-modified resin can improve the hardness of the paint film, but it also reduces the elasticity and toughness of the paint film, making it brittle. This invention selects polycaprolactone polyol as the soft segment of the silicone-modified polyurethane resin, which improves both the crosslinking density and the toughness and impact resistance of the silicone-modified polyurethane resin. Therefore, when the prepared silicone-modified polyurethane resin is used in high-gloss clear varnishes, it can significantly improve the hardness, abrasion resistance, scratch resistance, elasticity, toughness, impact resistance, and tear resistance of the paint film.

[0045] The organosilicon-modified polyurethane resin prepared by this invention does not contain benzene rings in its structure, which can increase the anti-yellowing performance of the organosilicon-modified polyurethane resin in high-gloss clear varnishes. This invention selects polycaprolactone polyol as the chain segment of the organosilicon-modified polyurethane resin, which enables the prepared organosilicon-modified polyurethane resin to exhibit excellent anti-yellowing performance in high-gloss clear varnishes.

[0046] For decorative coatings, gloss and saturation are very important. When general silicone-modified resins are used in varnishes, the gloss performance of the varnish will be somewhat reduced, making it difficult to achieve a gloss of over 90°. The silicone-modified polyurethane resin prepared in this invention, when used in high-gloss varnishes, can ensure that the gloss of the coating is above 90° while achieving high hardness and high toughness.

[0047] The second objective of this invention is to provide a method for preparing a high-gloss varnish with high resistance to ultraviolet aging and abrasion, as described in one objective of this invention.

[0048] The preparation method includes: mixing the components of the base material according to the specified weight parts to obtain the base material; mixing the components of the curing material according to the specified weight parts to obtain the curing material; and mixing the base material, curing material, and diluent according to the specified dosage to obtain the high-gloss clear varnish.

[0049] The preparation method can specifically adopt the following scheme:

[0050] Preparation of base material:

[0051] Prepare the paint mixing tank, weigh the raw materials according to the formula, and add them to the mixing tank in sequence. After all the raw materials have been added, disperse and stir them using a high-speed disperser. The stirring speed should be controlled at (600-900) r / min, and the stirring time should be sufficient to stir evenly, usually around 30 minutes. After dispersion, mix the paint and adjust the non-volatile matter content to within the range of 60±2%. After the product performance test is qualified, filter and package it.

[0052] Preparation of curing material:

[0053] Prepare the paint mixing tank, weigh the raw materials according to the formula, and add them to the paint mixing tank in sequence; after all the raw materials have been added, disperse and stir them with a high-speed disperser; control the stirring speed at (200-400) r / min, and the stirring time should be sufficient to stir evenly, usually around 20 minutes; filter and package the product after the product performance test is qualified.

[0054] Preparation of diluent:

[0055] Prepare the paint mixing tank, weigh the raw materials according to the formula, and add them to the paint mixing tank in sequence; after all the raw materials have been added, disperse and stir them with a high-speed disperser; control the stirring speed at (100-300) r / min, and the stirring time should be sufficient to stir evenly, usually around 10 minutes; filter and package the product after the product performance test is qualified.

[0056] A third objective of this invention is to provide the application of a high-gloss varnish with high UV aging resistance and abrasion resistance, as described in one objective of this invention, in a protective coating.

[0057] The application involves mixing the base material, curing agent, and diluent according to the stated amounts, stirring thoroughly, allowing it to stand and mature until the application viscosity is reached, then coating and curing. Preferably, the standing and maturation time is 15-30 minutes, the application viscosity is 12-28 seconds, the coating method is spraying, and the thickness of the cured dry film is 25-40 μm.

[0058] The application can specifically adopt the following scheme:

[0059] One of the objectives of the invention is to use the high-gloss clear varnish with high UV aging resistance and abrasion resistance in combination with the color paint. The initial substrate treatment mainly involves sanding the color paint to activate the surface. Fine sanding is done with sandpaper of 800 grit or higher to improve the wetting ability of the high-gloss clear varnish to the color paint. After sanding, the surface is cleaned with ethyl acetate or butyl acetate to ensure that there is no oil or powder residue on the surface.

[0060] The high-gloss clear varnish of this invention comprises three components: base material, hardener, and thinner. Before application, the base material, hardener, and thinner are mixed and stirred in proportion, and then allowed to stand for 15-30 minutes to mature. The general application viscosity is between 12-28 s. It is recommended to filter the varnish with a filter cloth of 100 mesh or higher before spraying. The dry film thickness should be controlled at 25-40 μm. Pneumatic spraying is recommended, with a nozzle diameter of 1.0-1.5 mm and an atomization pressure controlled at 0.3-0.5 MPa. During spraying, the spray gun should be moved perpendicular to the spraying surface at a uniform speed. After the varnish film is sprayed, it can be surface dry in 2 hours and fully dry in 24 hours at room temperature. Complete curing takes 7 days. The varnish film can also be cured by heat, but it needs to be placed at room temperature for at least 2 hours and then placed in a 60°C oven for at least 4 hours.

[0061] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0062] The organosilicon-modified polyurethane resin prepared in this invention is combined with a high-hydroxyl acrylic resin and crosslinked with a curing agent to form a film. This approach offers several advantages: first, the migration of organosilicon segments to the surface provides a shielding effect, increasing weather resistance and media resistance; second, the high-hydroxyl groups form a film with the trimer, increasing the crosslinking density and significantly enhancing film hardness and abrasion resistance, together with the organosilicon segments; and third, by controlling the content of organosilicon groups, a relatively large number of polar groups remain on the coating surface, thus not affecting the recoating performance of the film and maintaining gloss.

[0063] The high-gloss clear varnish provided by this invention possesses excellent resistance to ultraviolet aging and abrasion. When applied to the surface of colored paint, it effectively enhances the coating's anti-aging and scratch resistance, while also exhibiting good impact toughness, high and low temperature alternating performance, and excellent adhesion to the colored paint. It boasts advantages such as high gloss, strong ultraviolet resistance, excellent abrasion resistance, and good recoatability. It can be widely applied to equipment and transportation vehicles operating in outdoor environments with strong sunlight and wind and sand, possessing considerable application and economic value. Detailed Implementation

[0064] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0065] The raw materials used in the following examples and comparative examples are all commercially available products.

[0066] Polycaprolactone polyol is derived from Aladdin reagent, Mn1000-2000;

[0067] The hydroxyl-terminated polydimethylsiloxane is derived from Aladdin reagent, Mn1000-2000.

[0068] Example 1

[0069] (1) Preparation of silicone-modified polyurethane resin:

[0070] 15g of hydroxyl-terminated polydimethylsiloxane was ultrasonically dispersed in 20g of solvent methyl isobutyl ketone to obtain a hydroxyl-terminated polydimethylsiloxane solution. 35g of polycaprolactone polyol and 30g of dicyclohexylmethane diisocyanate (Aladdin reagent, isomer mixture) were added to a flask equipped with a stirrer, thermometer, condenser, and nitrogen protection device and mixed thoroughly. The hydroxyl-terminated polydimethylsiloxane solution was then added to the flask, and the mixture was stirred thoroughly for 30 minutes. Under nitrogen protection, the temperature was raised to 80℃ and reacted for 2 hours. After cooling to 50℃, 5g of chain extender 1,4-butanediol and 0.2g of catalyst dibutyltin dilaurate were added, and the mixture was thoroughly mixed. The temperature was then raised to 70℃ and reacted for 3 hours. After cooling to 60℃, a solvent (composed of ethyl acetate, butyl acetate, and methyl isobutyl ketone in a mass ratio of 2:2:1) was added. After cooling, the mixture was discharged to obtain an organosilicon-modified polyurethane resin.

[0071] (2) Preparation of base material:

[0072] The raw material formula of the base material is as follows: 25g of silicone-modified polyurethane resin prepared in step (1), 46g of hydroxyl acrylic resin (Zhanxin 2810), 2g of anti-sagging agent (BYK410), 0.3g of defoamer (BYK054), 0.7g of leveling agent (AFCONA3700), 3g of light stabilizer (UV-791), 3g of ultraviolet absorber (UV-1164), 10g of butyl acetate, and 10g of propylene glycol methyl ether acetate.

[0073] The base material preparation process is as follows: Prepare a mixing tank, and add all the base material raw materials into the mixing tank according to the formula. After all raw materials have been added, disperse and stir them using a high-speed disperser, then filter and package. The stirring speed is controlled at 600 r / min, and the stirring time is 30 min.

[0074] (3) Preparation of curing material:

[0075] The raw material formula for the curing agent is: Desmodur N3390 78g, butyl acetate 22g.

[0076] The preparation process of the cured material is as follows: Prepare a mixing tank, and add the raw materials of the cured material into the mixing tank according to the formula. After all the raw materials have been added, disperse and stir them using a high-speed disperser, then filter and package. The stirring speed is controlled at 200 r / min, and the stirring time is 20 min.

[0077] (4) Preparation of diluent:

[0078] The raw material formula of the diluent is: 50g of butyl acetate, 30g of ethyl acetate, and 20g of propylene glycol methyl ether acetate.

[0079] The preparation process of the thinner is as follows: Prepare a paint mixing tank, and add all the raw materials into the tank according to the formula. After all the raw materials have been added, disperse and stir them using a high-speed disperser, then filter and package. The stirring speed is controlled at 100 r / min, and the stirring time is 10 min.

[0080] (5) Preparation of high-gloss varnish:

[0081] The weight ratio of base material, curing agent and diluent is 2:1.2:2.

[0082] The construction process is as follows: First, mix and stir the base material, hardener, and thinner according to the specified ratio, then let it stand for 15 minutes to mature, achieving a working viscosity of 15s. Filter the mixture through a 100-mesh or finer filter cloth before spraying. Use pneumatic spraying with a 1.2mm nozzle diameter and atomization pressure controlled at 0.4MPa. During spraying, the spray gun should be moved perpendicular to the spray surface at a uniform speed. After spraying, the paint film will be surface dry in 2 hours at room temperature, completely dry in 24 hours, and fully cured in 7 days. The dry film thickness is 25-40μm.

[0083] Example 2

[0084] (1) Preparation of silicone-modified polyurethane resin:

[0085] 10g of hydroxyl-terminated polydimethylsiloxane was ultrasonically dispersed in 20g of solvent methyl isobutyl ketone to obtain a hydroxyl-terminated polydimethylsiloxane solution. 50g of polycaprolactone polyol and 35g of dicyclohexylmethane diisocyanate (Aladdin reagent) were added to a flask equipped with a stirrer, thermometer, condenser, and nitrogen protection device and mixed thoroughly. The hydroxyl-terminated polydimethylsiloxane solution was then added to the flask, and the mixture was stirred thoroughly for 30 minutes. Under nitrogen protection, the temperature was raised to 75℃ and reacted for 2 hours. After cooling to 50℃, 10g of chain extender ethylene glycol and 0.5g of catalyst dibutyltin dilaurate were added, and the mixture was thoroughly mixed. The temperature was then raised to 70℃ and reacted for 3 hours. After cooling to 60℃, a solvent (composed of ethyl acetate, butyl acetate, and methyl isobutyl ketone in a mass ratio of 2:2:1) was added. After cooling, the mixture was discharged to obtain an organosilicon-modified polyurethane resin.

[0086] (2) Preparation of base material:

[0087] The raw material formula of the base material is as follows: 35g of silicone-modified polyurethane resin prepared in step (1), 40g of acrylic resin (Mitsubishi 7908), 2.5g of anti-sagging agent (BYK430), 0.2g of defoamer (BYK054), 1.3g of leveling agent (BYK354), 5g of light stabilizer (UV-292), 5g of ultraviolet absorber (UV-328), 6g of butyl acetate, and 5g of methyl isobutyl ketone.

[0088] The base material preparation process is the same as in Example 1.

[0089] (3) Preparation of curing material:

[0090] Raw material formula for curing agent: Desmodur N100 70g, butyl acetate 30g.

[0091] The preparation process of the cured material is the same as that in Example 1.

[0092] (4) Preparation of diluent:

[0093] The raw material formula of the diluent is: 50g butyl acetate, 30g propylene glycol methyl ether acetate, and 20g methyl isobutyl ketone.

[0094] The diluent preparation process is the same as in Example 1.

[0095] (5) Preparation of high-gloss varnish:

[0096] The weight ratio of the base material, curing agent, and diluent is 2:1:2.

[0097] The construction process is the same as in Example 1.

[0098] Example 3

[0099] (1) Preparation of silicone-modified polyurethane resin:

[0100] 15g of hydroxyl-terminated polydimethylsiloxane was ultrasonically dispersed in 20g of methyl isobutyl ketone solvent to obtain a hydroxyl-terminated polydimethylsiloxane solution. 50g of polycaprolactone polyol and 20g of isoflurane diisocyanate (Aladdin reagent) were added to a flask equipped with a stirrer, thermometer, condenser, and nitrogen protection device and mixed thoroughly. The hydroxyl-terminated polydimethylsiloxane solution was then added to the flask, and the mixture was stirred thoroughly for 30 minutes. Under nitrogen protection, the temperature was raised to 85℃ and reacted for 2 hours. After cooling to 50℃, 10g of 1,4-butanediol chain extender and 0.5g of dibutyltin dilaurate catalyst were added, and the mixture was thoroughly mixed. The temperature was then raised to 80℃ and reacted for 3 hours. After cooling to 60℃, a solvent (composed of ethyl acetate, butyl acetate, and methyl isobutyl ketone in a mass ratio of 2:2:1) was added. After cooling, the mixture was discharged to obtain an organosilicon-modified polyurethane resin.

[0101] (2) Preparation of base material:

[0102] The raw material formula of the base material is as follows: 40g of silicone-modified polyurethane resin prepared in step (1), 35g of acrylic resin (Zhanxin 2155), 3g of anti-sagging agent (BYK430), 0.3g of defoamer (BYK024), 1.5g of leveling agent (BYK333), 2g of light stabilizer (UV-124), 3.2g of ultraviolet absorber (UV-326), and 15g of methyl isobutyl ketone.

[0103] The base material preparation process is the same as in Example 1.

[0104] (3) Preparation of curing material:

[0105] The raw material formula for the curing agent is: Desmodur N3390 78g, butyl acetate 23g.

[0106] The preparation process of the cured material is the same as that in Example 1.

[0107] (4) Preparation of diluent:

[0108] The raw material formula of the diluent is: 60g of butyl acetate, 20g of ethyl acetate, and 20g of methyl isobutyl ketone.

[0109] The diluent preparation process is the same as in Example 1.

[0110] (5) Preparation of high-gloss varnish:

[0111] The weight ratio of base material, curing agent and diluent is 2:1.2:2.

[0112] The construction process is the same as in Example 1.

[0113] Comparative Example 1

[0114] The raw material formula of the base material is as follows: 75g of Zhanxin 2810 resin, 2.5g of anti-sagging agent (BYK430), 0.2g of defoamer (BYK054), 1.3g of leveling agent (BYK354), 5g of light stabilizer (UV-292), 5g of ultraviolet absorber (UV-328), 6g of butyl acetate, and 5g of methyl isobutyl ketone.

[0115] The base material preparation process is the same as in Example 1.

[0116] Raw material formula of the curing agent:

[0117] Desmodur N100 70g, butyl acetate 30g.

[0118] The preparation process of the cured material is the same as that in Example 1.

[0119] Diluent raw material formula:

[0120] 50g butyl acetate, 30g propylene glycol methyl ether acetate, 20g methyl isobutyl ketone.

[0121] The diluent preparation process is the same as in Example 1.

[0122] The weight ratio of base material, curing agent and diluent is 2:0.6:2.

[0123] The construction process is the same as in Example 1.

[0124] Comparative Example 2

[0125] The raw material formula of the base material is as follows: 75g of Xin Sihai Chemical SH-024 silicone resin, 2g of anti-sagging agent (BYK410), 0.3g of defoamer (BYK057), 1.3g of leveling agent (BYK354), 5g of light stabilizer (UV-292), 5g of ultraviolet absorber (UV-328), 6g of butyl acetate, and 5g of methyl isobutyl ketone.

[0126] The base material preparation process is the same as in Example 1.

[0127] Raw material formula of the curing agent:

[0128] Desmodur N100 70g, butyl acetate 30g.

[0129] The preparation process of the cured material is the same as that in Example 1.

[0130] Diluent raw material formula:

[0131] 50g butyl acetate, 30g propylene glycol methyl ether acetate, 20g methyl isobutyl ketone.

[0132] The diluent preparation process is the same as in Example 1.

[0133] The weight ratio of the base material, curing agent, and diluent is 3:1:3.

[0134] The construction process is the same as in Example 1.

[0135] Performance testing

[0136] The properties of the paint films formed in Examples 1-3 and Comparative Examples 1-2 were tested, requiring the varnish to be applied to the surface of the colored paint. The test standards, test methods, and technical requirements for the varnish are shown in Table 1. The test results are shown in Table 2.

[0137] Table 1

[0138]

[0139] In Table 1, A, B, and C represent the base material, curing material, and diluent, respectively.

[0140] Specific coating properties:

[0141] Table 2

[0142]

[0143] As can be seen from the test results shown in Table 2, the paint films prepared in Examples 1-3 have good mechanical properties. Their flexibility, impact adhesion, etc. all meet the index requirements. They not only have good UV aging resistance and wear resistance, but also excellent mechanical properties, good recoatability, high gloss characteristics, and excellent high and low temperature alternating performance.

[0144] Compared with Comparative Examples 1 and 2, Examples 1-3 use different resin components. Examples 1-3 use a self-made silicone-modified polyurethane resin and acrylic resin as the resin component of the high-gloss clear varnish, Comparative Example 1 uses a non-silicone-modified resin as the resin component of the clear varnish, and Comparative Example 2 uses an existing silicone-modified resin as the resin component of the clear varnish.

[0145] Table 2 shows that, compared with Comparative Example 1, Examples 1-3 showed improvements in hardness by two grades, adhesion by one grade, corrosion resistance, UV aging resistance (gloss retention increased by 11-13%, color retention increased by 58-65%), and abrasion resistance by 77-86%. This indicates that, compared with existing resins (non-silicone modified), the present invention uses a self-made silicone-modified polyurethane resin compounded with acrylic resin as the resin component of the varnish, which improves the varnish's hardness, adhesion, corrosion resistance, UV aging resistance (gloss retention, color retention), and abrasion resistance. A possible reason is that the silicone-modified polyurethane resin synthesized in this invention moves silicone segments to the surface during film formation, effectively shielding the coating and increasing both corrosion resistance and UV aging resistance. Furthermore, the acrylic resin contains a large number of hydroxyl groups, which form a network cross-linked structure with the curing agent during film formation, increasing both the coating's corrosion resistance and hardness. Combined with the effect of silicone segments, the film hardness and abrasion resistance are significantly increased.

[0146] Table 2 shows that, compared with Comparative Example 2, Examples 1-3 showed improvements in recoatability by one grade, gloss by 11-13%, hardness by one grade, flexibility by one grade, adhesion by one grade, impact adhesion, high and low temperature alternating performance (low temperature impact resistance) by two grades, and abrasion resistance by 47-67%. This indicates that, compared with existing silicone-modified resins, the present invention uses a self-made silicone-modified polyurethane resin compounded with acrylic resin as the resin component of the clear varnish, which can improve the clear varnish's recoatability, gloss, hardness, flexibility, adhesion, impact adhesion, high and low temperature alternating performance, UV aging resistance, and abrasion resistance. A possible reason is that the hydroxyl acrylic resin in Examples 1-3 increases the polarity of the coating surface, correspondingly increasing the coating's toughness and improving its mechanical properties. This also avoids the problem of poor recoatability caused by silicone resins, and the gloss of the paint film is also guaranteed.

[0147] Table 2 shows that compared with Comparative Example 1, Comparative Example 2 exhibits significantly increased hardness and decreased flexibility; compared with Comparative Example 1, Examples 1-3 show significantly increased hardness and comparable flexibility; compared with Comparative Example 2, Examples 1-3 show significantly increased hardness and flexibility. This indicates that while using existing silicone-modified resins as resin components in clear varnishes can increase hardness, it also makes the varnish film brittle and reduces its flexibility. However, using the self-made silicone-modified polyurethane resin and acrylic resin compounded in this invention as resin components in high-gloss clear varnishes not only significantly increases the hardness of the clear varnish but also avoids making the varnish film brittle due to increased hardness; that is, it can significantly increase the hardness of the clear varnish while maintaining good flexibility.

Claims

1. A high-gloss varnish with high resistance to UV aging and abrasion, characterized in that, The high-gloss varnish comprises a base material, a curing agent, and a diluent; the weight ratio of the base material, curing agent, and diluent is 2:(1.0-1.3):(1.2-2.4). Based on a total weight of 100 parts by weight, the base material comprises the following components: 20-40 parts by weight of silicone-modified polyurethane resin; 30-60 parts by weight of hydroxyl acrylic resin; Anti-sagging agent: 1.0-3.5 parts by weight; Defoamer 0.1-0.5 parts by weight; Leveling agent 0.5-2.0 parts by weight; Light stabilizer 1-10 parts by weight; 1-10 parts by weight of ultraviolet absorber; Base solvent 5-25 parts by weight; Based on 100 parts by weight of the cured material, the cured material comprises the following components: 70-100 parts by weight of curing agent; Curing agent solvent: 0-30 parts by weight; The organosilicon-modified polyurethane resin is obtained by stepwise polymerization of raw materials including hydroxyl-terminated polydimethylsiloxane, polycaprolactone polyol, diisocyanate, chain extender, and catalyst, followed by the addition of a solvent; based on the total weight of the raw materials (100%): polycaprolactone polyol 30%-55%, hydroxyl-terminated polydimethylsiloxane 5%-25%, diisocyanate 20%-40%, chain extender 5%-15%, and catalyst 0.5%-1%. The preparation method of the organosilicon-modified polyurethane resin includes the following steps: (1) Mix polycaprolactone polyol, diisocyanate and hydroxyl-terminated polydimethylsiloxane thoroughly and react at 75-85℃ for 1.5-2h under nitrogen protection; (2) Cool down to 40-50℃, add chain extender and catalyst, and mix thoroughly; (3) Heat to 70-80℃ and react for 2-3 hours; (4) Cool down to 50-60℃, add solvent, stir evenly, and obtain the organosilicon-modified polyurethane resin; The number-average molecular weight of the hydroxyl-terminated polydimethylsiloxane is 500-3500; The number-average molecular weight of the polycaprolactone polyol is 300-2500; The hydroxyl value of the hydroxyl acrylic resin is 150 or higher; The curing agent is selected from aliphatic isocyanate compounds; The diluent contains butyl acetate.

2. The high-gloss clear varnish as described in claim 1, characterized in that, The weight ratio of the base material, curing agent and diluent is 2:(1.1-1.2):(1.8-2.4).

3. The high-gloss clear varnish as described in claim 1, characterized in that, Based on a total weight of 100 parts by weight, the base material comprises the following components: 25-35 parts by weight of silicone-modified polyurethane resin; 35-55 parts by weight of hydroxyl acrylic resin; Anti-sagging agent 2.0-3.0 parts by weight; Defoamer 0.1-0.3 parts by weight; Leveling agent 0.5-1.5 parts by weight; 2-5 parts by weight of light stabilizer; 2-5 parts by weight of ultraviolet absorber; Base solvent 10-20 parts by weight.

4. The high-gloss clear varnish as described in claim 1, characterized in that, Based on 100 parts by weight of the cured material, the cured material comprises the following components: 75-100 parts by weight of curing agent; Curing agent solvent: 0-25 parts by weight.

5. The high-gloss clear varnish as described in claim 1, characterized in that, The diluent is composed of ethyl acetate, butyl acetate, methyl isobutyl ketone, and propylene glycol methyl ether acetate in a mass ratio of (0.1-2):(4-6):(0.1-3):(0.1-3).

6. The high-gloss clear varnish as described in claim 1, characterized in that, The anti-sagging agent is at least one of modified polyamide solution-based anti-sagging agents and modified urea-based anti-sagging agents; or / and, The defoamer is at least one of a defoaming polymer solution or a polysiloxane solution; or / and The leveling agent is at least one of a polyether-modified silicone leveling agent and an acrylate leveling agent; or / and, The light stabilizer is at least one of hindered amine light stabilizers or composite light stabilizers; or / and, The ultraviolet absorber is at least one of triazine ultraviolet absorbers and benzotriazole ultraviolet absorbers; or / and, The base solvent is one or more of butyl acetate, methyl isobutyl ketone, and propylene glycol methyl ether acetate.

7. The high-gloss clear varnish according to claim 1, characterized in that, The curing agent is selected from hexamethylene diisocyanate biuret curing agent, HDI trimer curing agent; or / and, The curing agent solvent is at least one of ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, and methyl isobutyl ketone.

8. The high-gloss clear varnish as described in claim 1, characterized in that, The number-average molecular weight of the hydroxyl-terminated polydimethylsiloxane is 1000-3000; or / and The number-average molecular weight of the polycaprolactone polyol is 1000-2000; or / and, The diisocyanate is one or more of dicyclohexylmethane diisocyanate or isoflurane diisocyanate; or / and The chain extender is one of 1,4-butanediol or ethylene glycol; or / and, The catalyst is dibutyltin dilaurate; or / and, The solvent is composed of ethyl acetate, butyl acetate, and methyl isobutyl ketone in a mass ratio of (1-3):(4-6):(1-3).

9. A method for preparing a high-gloss varnish as described in any one of claims 1-8, characterized in that, The preparation method includes: The base material is obtained by stirring and mixing the components according to the stated weight proportions; the curing material is obtained by stirring and mixing the components according to the stated weight proportions; the high-gloss varnish is obtained by mixing the base material, curing material, and diluent according to the stated dosages.

10. The application of a high-gloss varnish as described in any one of claims 1-8 or a high-gloss varnish prepared by the preparation method as described in claim 9 in a protective coating.

Citation Information

Patent Citations

  • Solvent type skin coating varnish as well as preparation method and application thereof

    CN115477878A

  • High-temperature-resistant high-gloss varnish coating composition, preparation method thereof and high-temperature-resistant high-gloss varnish coating prepared from high-temperature-resistant high-gloss varnish coating composition