Preparation method of lead selenide colloid quantum dot film based on trimethylaluminum doping

By doping trimethylaluminum gas in the lead selenide colloidal quantum dot film, the problems of high dark current and low mobility of lead-based colloidal quantum dot detectors are solved, and the detector performance is improved.

CN119768000AActive Publication Date: 2025-04-04HUAZHONG UNIV OF SCI & TECH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411780332.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-05
Publication Date
2025-04-04
Estimated Expiration
2044-12-05

AI Technical Summary

Technical Problem

The existing lead-based colloidal quantum dot detectors have high dark current, resulting in high shot noise, which limits further optimization of the detector imaging performance, and its low mobility, limiting the ultimate detection performance.

Method used

The preparation method of lead selenide colloidal quantum dot film based on trimethylaluminum doping is adopted. By doping lead selenide colloidal quantum dots and trimethylaluminum gas in a vacuum environment, the mobility of the film is improved.

Benefits of technology

It significantly improves the mobility of the colloidal quantum dot detector, improves the device's ultimate detection performance, and reduces dark current and shot noise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119768000A_ABST
    Figure CN119768000A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a lead selenide colloidal quantum dot film based on doping of trimethylaluminum. The preparation method of the lead selenide colloidal quantum dot film based on doping of trimethylaluminum comprises the following steps: obtaining a fifth mixed solution; spin-coating a target sample with the fifth mixed solution, and performing annealing treatment for a preset annealing duration to obtain an initial lead selenide colloidal quantum dot film; putting the initial lead selenide colloid quantum dot film into a cabin, vacuumizing the cabin until the air pressure reaches a preset pressure intensity, and heating the initial lead selenide colloid quantum dot film to a preset temperature; and introducing trimethylaluminum gas into the cabin to obtain the lead selenide colloid quantum dot film based on trimethylaluminum doping. The mobility of the colloidal quantum dot detector can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film. Background Art

[0002] Short-wave infrared refers to light with a wavelength from 900nm to 2.5um. Light in this band has higher intensity than visible light even in night environments, and has a longer penetration depth in clouds and fog. Therefore, the short-wave infrared band carries more information about object contours, surface textures, dimensions, etc. and is widely observed. Colloidal quantum dots are a type of zero-dimensional material synthesized in liquid phase. The band gap and wavelength of the material can be controlled by regulating the size. They are studied for their light absorption properties in the short-wave infrared band. The current mainstream colloidal quantum dots used for short-wave infrared detection are lead-based colloidal quantum dots. The electrons in the valence band of the quantum dots absorb photon energy and transition to the conduction band to form free electrons, increasing the current of the detector, thereby detecting the light signal through the detection of the current. The current mainstream lead-based colloidal quantum dot photodetector adopts a PIN-type structure, that is, a lead-based colloidal quantum dot layer (light-absorbing layer) with light-absorbing function is sandwiched between a highly doped functional layer, and a built-in electric field is formed through the high doping concentration of the functional layer to penetrate the light-absorbing layer; under the action of the built-in electric field, the electron-hole pairs generated by light absorption are separated to form efficient carrier extraction. In actual devices, oxide semiconductors such as zinc oxide and tin oxide are mostly used as N-type functional layers, and quantum dot films treated with ethanedithiol are used as P-type functional layers. Lead-based colloidal quantum dot devices based on this structure have the advantages of high responsiveness and high dynamic range and have also been widely reported. However, the shot noise caused by the dark current of colloidal quantum dots is large, which limits the further optimization of the imaging performance of colloidal quantum dot detectors. The high dark current is caused by the reverse saturation current, which is mainly limited by the low mobility. Compared with the mobility of classic semiconductors such as silicon, which is 480cm 2 / V*s, the mobility of lead-based colloidal quantum dot films is only 2*10 -3 -3*10 -3 cm 2 / V*s, 10 lower 5 This determines and limits the ultimate performance of lead-based colloidal quantum dot devices to be 2-3 orders of magnitude lower than that of silicon, and is also the main reason for the poor weak light performance of quantum dot detectors. Improving the mobility of colloidal quantum dot detectors is crucial. Summary of the invention

[0003] The present application aims to solve at least one of the above-mentioned technical problems by providing a method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film, thereby improving the mobility of a colloidal quantum dot detector.

[0004] On the one hand, the present application provides a method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film, and the method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film comprises:

[0005] Preserving lead selenide colloidal quantum dots in an n-octane solvent to obtain a quantum dot n-octane solution, wherein the ligand on the surface of the lead selenide colloidal quantum dots is oleic acid;

[0006] Dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution;

[0007] The quantum dot n-octane solution and the first mixed solution are filtered and then mixed to obtain a second mixed solution;

[0008] Oscillating the second mixed solution for a first oscillation time and standing until the second mixed solution is separated into an upper and lower solution, removing the upper solution of the second mixed solution and adding a preset volume of n-octane solvent to obtain a third mixed solution;

[0009] Oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into an upper and lower solution layer, and removing the upper solution of the third mixed solution to obtain a fourth mixed solution;

[0010] Treating the fourth mixed solution to obtain a DMF solution of lead selenide quantum dots with iodide ions and bromide ions as ligands;

[0011] The lead selenide quantum dot DMF solution is placed in a centrifuge and the upper yellow liquid is poured out, and vacuum extraction is performed for a preset extraction time to remove the residual DMF solution on the surface to obtain lead selenide quantum dots;

[0012] Dissolving lead selenide quantum dots in a mixed solvent of n-butylamine and DMF to obtain a fifth mixed solution;

[0013] Spin coating the fifth mixed solution on the target sample and annealing the sample for a preset annealing time to obtain an initial lead selenide colloidal quantum dot film;

[0014] Putting the initial lead selenide colloidal quantum dot film into a chamber, evacuating the chamber until the air pressure reaches a preset pressure, and heating the initial lead selenide colloidal quantum dot film to a preset temperature;

[0015] Trimethylaluminum gas is introduced into the chamber to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film.

[0016] Optionally, the concentration of the lead selenide colloidal quantum dots in the quantum dot n-octane solution is 10 mg / mL.

[0017] Optionally, dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution comprises:

[0018] 0.92 g of lead iodide and 0.58 g of lead bromide were dissolved in 10 ml of DMF solution to obtain a first mixed solution.

[0019] Optionally, the first oscillation duration is 40 seconds, and the second oscillation duration is 40 seconds.

[0020] Optionally, the preset volume is 10 ml.

[0021] Optionally, the preset extraction time is one hour.

[0022] Optionally, the step of placing the lead selenide quantum dot DMF solution in a centrifuge and discarding the upper yellow liquid comprises:

[0023] The lead selenide quantum dot DMF solution was placed in a centrifuge and centrifuged at a speed of 9000 rpm for 4 minutes.

[0024] Optionally, in the mixed solvent of n-butylamine and DMF, the volume ratio of n-butylamine to DMF is 1:1.

[0025] Optionally, the preset annealing time is 10 minutes, and the preset pressure is 10 -6 pa-10 -4 pa, the preset temperature is 20 degrees Celsius to 100 degrees Celsius.

[0026] Optionally, the step of introducing trimethylaluminum gas into the chamber to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film comprises:

[0027] Trimethylaluminum gas is introduced into the chamber in a pulse pumping manner to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film, wherein during pulse pumping, a single pumping time is 10 ms, a pumping time interval is 60s-150s, the number of pumpings is 10 times-100 times, and the gas pressure of the trimethylaluminum gas is 15Pa-25Pa.

[0028] In the preparation method of trimethylaluminum-doped lead selenide colloidal quantum dot film of the present application, the preparation method of trimethylaluminum-doped lead selenide colloidal quantum dot film includes: preserving lead selenide colloidal quantum dots in an n-octane solvent to obtain a quantum dot n-octane solution, wherein the ligand on the surface of the lead selenide colloidal quantum dots is oleic acid; dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution; filtering the quantum dot n-octane solution and the first mixed solution separately and then mixing them to obtain a second mixed solution; oscillating the second mixed solution for a first oscillation time and standing until the second mixed solution is separated into two layers of upper and lower solutions, removing the upper layer of the second mixed solution and adding a preset volume of n-octane solvent to obtain a third mixed solution; oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into two layers of upper and lower solutions, removing the third mixed solution The upper solution is obtained to obtain a fourth mixed solution; the fourth mixed solution is treated to obtain a DMF solution of lead selenide quantum dots with iodine ions and bromide ions as ligands; the DMF solution of lead selenide quantum dots is placed in a centrifuge for treatment and the upper yellow liquid is poured out, and the DMF solution remaining on the surface is removed by vacuum extraction for a preset extraction time to obtain lead selenide quantum dots; the lead selenide quantum dots are dissolved in a mixed solvent of n-butylamine and DMF to obtain a fifth mixed solution; the fifth mixed solution is spin-coated on the target sample and annealed for a preset annealing time to obtain an initial lead selenide colloidal quantum dot film; the initial lead selenide colloidal quantum dot film is placed in a cabin, the cabin is vacuumed until the air pressure reaches a preset pressure, and the initial lead selenide colloidal quantum dot film is heated to a preset temperature; trimethylaluminum gas is introduced into the cabin to obtain a lead selenide colloidal quantum dot film based on trimethylaluminum doping. The present application can improve the mobility of colloidal quantum dot detectors. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic flow chart of an embodiment of a method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film according to an embodiment of the present application;

[0030] Figure 2 It is a schematic diagram of disposing a trimethylaluminum-doped lead selenide colloidal quantum dot film on a target sample provided in an embodiment of the present application;

[0031] Figure 3 is a graph showing the relationship between the gate voltage and drain current of the target sample before trimethylaluminum doping;

[0032] Figure 4 It is a curve diagram showing the relationship between the gate voltage and drain current of the target sample after trimethylaluminum doping. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0034] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0035] In this application, the word "exemplary" is used to mean "used as an example, illustration, or description." Any embodiment described in this application as "exemplary" is not necessarily to be construed as being preferred or advantageous over other embodiments. The following description is given to enable any technician in the field to implement and use the present application. In the following description, details are listed for the purpose of explanation. It should be understood that a person of ordinary skill in the art can recognize that the present application can be implemented without using these specific details. In other instances, well-known structures and processes will not be elaborated in detail to avoid obscuring the description of the present application with unnecessary details. Therefore, the present application is not intended to be limited to the embodiments shown, but is consistent with the widest scope consistent with the principles and features disclosed in the present application.

[0036] Lead-based colloidal quantum dot films have shown excellent performance in the field of short-wave infrared detection. However, due to the amorphous material structure of colloidal quantum dot films, their film mobility is limited to only 10 -3 cm 2 / (V*s), which is much lower than similar short-wave infrared detection materials. PN junction infrared detection devices made of low-mobility semiconductor materials face the disadvantages of low responsivity and high dark current, which limits their ultimate detection performance. How to improve the mobility of lead-based colloidal quantum dots and thus enhance the ultimate detection performance of the device is particularly important.

[0037] In order to solve the above problems, the present application provides a preparation method of a trimethylaluminum-doped lead selenide colloidal quantum dot film, and the preparation method of the trimethylaluminum-doped lead selenide colloidal quantum dot film comprises: preserving the lead selenide colloidal quantum dots in an n-octane solvent to obtain a quantum dot n-octane solution, wherein the ligand on the surface of the lead selenide colloidal quantum dots is oleic acid; dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution; filtering the quantum dot n-octane solution and the first mixed solution respectively and then mixing them to obtain a second mixed solution; oscillating the second mixed solution for a first oscillation time and standing until the second mixed solution is separated into an upper and lower solution, removing the upper solution of the second mixed solution and adding a preset volume of n-octane solvent to obtain a third mixed solution; oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into an upper and lower solution, removing the first mixed solution, and adding a preset volume of n-octane solvent to obtain a third mixed solution; oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into an upper and lower solution, removing the first mixed solution, and mixing the first mixed solution. The upper solution of the three mixed solutions is used to obtain a fourth mixed solution; the fourth mixed solution is treated to obtain a DMF solution of lead selenide quantum dots with iodine ions and bromide ions as ligands; the DMF solution of lead selenide quantum dots is placed in a centrifuge for treatment and the upper yellow liquid is poured out, and the DMF solution remaining on the surface is removed by vacuum extraction for a preset extraction time to obtain lead selenide quantum dots; the lead selenide quantum dots are dissolved in a mixed solvent of n-butylamine and DMF to obtain a fifth mixed solution; the fifth mixed solution is spin-coated on the target sample and annealed for a preset annealing time to obtain an initial lead selenide colloidal quantum dot film; the initial lead selenide colloidal quantum dot film is placed in a cabin, the cabin is vacuumed until the air pressure reaches a preset pressure, and the initial lead selenide colloidal quantum dot film is heated to a preset temperature; trimethylaluminum gas is introduced into the cabin to obtain a lead selenide colloidal quantum dot film based on trimethylaluminum doping. The present application can improve the mobility of colloidal quantum dot detectors.

[0038] See also Figure 1 In the embodiment of the present application, the preparation method of trimethylaluminum-doped lead selenide colloidal quantum dot film comprises:

[0039] 201. Preserving lead selenide colloidal quantum dots in n-octane solvent to obtain quantum dot n-octane solution.

[0040] Among them, the ligand on the surface of lead selenide colloidal quantum dots is oleic acid.

[0041] In the embodiment of the present application, the concentration of lead selenide colloidal quantum dots in the quantum dot n-octane solution is 10 mg / mL. Specifically, lead selenide (PbSe) colloidal quantum dots are stored in n-octane solvent at a concentration of 10 mg / mL, and the ligand on the surface of the quantum dots is oleic acid.

[0042] 202. Dissolve lead iodide and lead bromide in DMF solution to obtain a first mixed solution.

[0043] In an embodiment of the present application, lead iodide and lead bromide are dissolved in a DMF solution to obtain a first mixed solution, including: dissolving 0.92 g of lead iodide and 0.58 g of lead bromide in 10 ml of a DMF solution to obtain a first mixed solution.

[0044] 203. Filter the quantum dot n-octane solution and the first mixed solution separately and then mix them to obtain a second mixed solution.

[0045] Specifically, ligand exchange is first required, and the whole process is carried out in a nitrogen environment (oxygen <0.01ppm water <0.01ppm) in a glove box. The specific operation is as follows: First, measure 10mL of PbSe quantum dot n-octane solution; then, weigh 0.92g of lead iodide (PbI2) and 0.58g of lead bromide (PbBr2) and fully dissolve them in 10ml of DMF (N,N-dimethylformamide) solution to obtain a first mixed solution. Filter 10mL of PbSe quantum dot n-octane solution and the first mixed solution (PbI2, PbBr-DMF solution) separately, and mix them in a container to obtain a second mixed solution.

[0046] 204. Oscillating the second mixed solution for a first oscillation time and standing until the second mixed solution is separated into an upper and lower solution layer, removing the upper solution of the second mixed solution and adding a preset volume of n-octane solvent to obtain a third mixed solution.

[0047] Since polar DMF and non-polar n-octane are separated, the upper layer of the second mixed solution is a black quantum dot n-octane solution, and the lower layer is a yellow DMF solution of PbI2 and PbBr2. The second mixed solution is oscillated for the first oscillation time and allowed to stand until the second mixed solution is separated into an upper and lower solution, the upper solution of the second mixed solution is removed and a preset volume of n-octane solvent is added to obtain a third mixed solution.

[0048] Specifically, the first oscillation time is 40 seconds, and the preset volume is 10 ml. The second mixed solution is oscillated for 40 seconds and then allowed to stand until the upper layer becomes transparent and the lower layer becomes black, the upper clear liquid is discarded, and 10 mL of n-octane is added to obtain a third mixed solution.

[0049] 205. Oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into an upper and lower solution layer, removing the upper solution of the third mixed solution to obtain a fourth mixed solution.

[0050] The second oscillation time is 40 seconds. 10 mL of n-octane is added to obtain a third mixed solution, which is further oscillated for 40 seconds. After standing for stratification, the upper layer of the solution is removed to obtain a fourth mixed solution.

[0051] 206. Treat the fourth mixed solution to obtain a DMF solution of lead selenide quantum dots with iodide ions and bromide ions as ligands.

[0052] In a specific embodiment, the fourth mixed solution is used as a DMF solution of lead selenide quantum dots with iodide ions and bromide ions as ligands.

[0053] In another specific embodiment, the fourth mixed solution is oscillated for the second oscillation time and allowed to stand until the fourth mixed solution is separated into two layers of solution, and the upper layer of the fourth mixed solution is removed to obtain a DMF solution of lead selenide quantum dots with iodide ions and bromide ions as ligands. Finally, the lower layer is a DMF solution of PbSe quantum dots with iodide ions and bromide ions as ligands.

[0054] 207. Place the lead selenide quantum dot DMF solution in a centrifuge and pour off the upper yellow liquid, vacuum extract for a preset extraction time, remove the residual DMF solution on the surface, and obtain lead selenide quantum dots.

[0055] In the embodiment of the present application, the preset extraction time is one hour. The lead selenide quantum dot DMF solution is placed in a centrifuge and the upper yellow liquid is poured out, including: placing the lead selenide quantum dot DMF solution in a centrifuge and centrifuging the lead selenide quantum dot DMF solution at a speed of 9000 rpm for 4 minutes.

[0056] Specifically, the lead selenide quantum dot DMF solution was placed in a centrifuge and centrifuged at 9000 rpm for 4 minutes. The upper yellow liquid was poured off, and vacuum extraction was performed for one hour to remove the residual DMF solution on the surface, thereby obtaining black powdered lead selenide quantum dots.

[0057] 208. Dissolve the lead selenide quantum dots in a mixed solvent of n-butylamine and DMF to obtain a fifth mixed solution.

[0058] In the embodiment of the present application, in the mixed solvent of n-butylamine and DMF, the volume ratio of n-butylamine to DMF is 1:1. According to the concentration of 50 μg / μL-600 μg / μL, lead selenide quantum dots are dissolved in the mixed solvent of n-butylamine and DMF in a volume ratio of 1:1 to obtain a fifth mixed solution. Among them, n-butylamine is used to dissolve the quantum dots, and DMF is used to increase the boiling point of the solvent to prevent volatilization from affecting the concentration.

[0059] 209. Spin-coat the fifth mixed solution on the target sample and anneal the sample for a preset annealing time to obtain an initial lead selenide colloidal quantum dot film.

[0060] In the embodiment of the present application, the preset annealing time is 10 minutes. After the quantum dots are completely dissolved, a certain amount of the fifth mixed solution is sucked with a pipette and spin-coated on the surface of the target sample, and finally an annealing treatment is performed for 10 minutes.

[0061] 210. Place the initial lead selenide colloidal quantum dot film into a chamber, evacuate the chamber until the air pressure reaches a preset pressure, and heat the initial lead selenide colloidal quantum dot film to a preset temperature.

[0062] In the embodiment of the present application, the preset annealing time is 10 minutes and the preset pressure is 10 -6 -10 -4 pa, the preset temperature is 20 degrees Celsius to 100 degrees Celsius. The doping of trimethylaluminum is carried out in a vacuum chamber. The initial lead selenide colloidal quantum dot film prepared in the previous step is placed in the chamber and evacuated to 10 -6 pa-10 -4 pa. The sample substrate is heated to 20-100 degrees Celsius and the temperature is stabilized.

[0063] 211. Trimethylaluminum gas is introduced into the chamber to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film.

[0064] In an embodiment of the present application, trimethylaluminum gas is introduced into the chamber to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film, including: introducing trimethylaluminum gas into the chamber in a pulse pumping manner to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film, wherein during pulse pumping, a single pumping time is 10 ms, a pumping time interval is 60s-150s, the number of pumpings is 10 times-100 times, and the gas pressure of the trimethylaluminum gas is 15Pa-25Pa.

[0065] In an embodiment of the present application, a method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film comprises:

[0066] Preliminary preparation of colloidal quantum dot films:

[0067] Lead selenide (PbSe) colloidal quantum dots are stored in n-octane solvent at a concentration of 10 mg / mL, and the ligand on the surface of the quantum dots is oleic acid. First, ligand exchange is required, and the whole process is carried out in a nitrogen environment (oxygen <0.01ppm water <0.01ppm) in a glove box. The specific operation is as follows: First, measure 10mL of PbSe quantum dot n-octane solution; then, weigh 0.92g of lead iodide (PbI2) and 0.58g of lead bromide (PbBr2) and fully dissolve them in 10ml of DMF (N,N-dimethylformamide) solution to obtain a first mixed solution. Filter 10mL of PbSe quantum dot n-octane solution and the first mixed solution (PbI2, PbBr-DMF solution) separately, mix them in a container, and obtain a second mixed solution. Due to the polar DMF and non-polar n-octane stratification, the upper layer of the second mixed solution is a black quantum dot n-octane solution, and the lower layer is a yellow Pb I2, PbBr2 DMF solution. The second mixed solution was vibrated for 40 seconds and then allowed to stand. After the upper layer became transparent and the lower layer turned black, the upper clear liquid was discarded and 10 mL of n-octane was added to obtain a third mixed solution. 10 mL of n-octane was added to obtain a third mixed solution, which was continued to vibrate for 40 seconds. After standing and stratifying, the upper solution was removed, and the fourth mixed solution was repeated twice. Finally, the lower layer was a PbSe quantum dot DMF solution with iodide ions and bromide ions as ligands. The lead selenide quantum dot DMF solution was placed in a centrifuge and centrifuged at a speed of 9000 rpm for 4 minutes. The upper yellow liquid was poured out, vacuum extracted for one hour, and the residual DMF solution on the surface was removed to obtain a black powder of lead selenide quantum dots. Lead selenide quantum dots are dissolved in a mixed solvent of n-butylamine and DMF at a volume ratio of 1:1 at a concentration of 50 μg / μL-600 μg / μL to obtain a fifth mixed solution. Among them, n-butylamine is used to dissolve the quantum dots, and DMF is used to increase the boiling point of the solvent to prevent volatilization from affecting the concentration. After the quantum dots are completely dissolved, a certain amount of the fifth mixed solution is taken with a pipette and spin-coated on the surface of the target sample, and finally annealed for 10 minutes.

[0068] Doping with trimethylaluminum:

[0069] The doping of trimethylaluminum is carried out in a vacuum chamber. The initial lead selenide colloidal quantum dot film prepared in the previous step is placed in the chamber and evacuated to 10 -6 pa-10 -4pa. The sample substrate is heated to 20-100 degrees Celsius and the temperature is stabilized. Trimethylaluminum gas is introduced into the chamber by pulse pumping to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film, wherein during pulse pumping, the single pumping time is 10ms, the pumping time interval is 60s-150s, the number of pumpings is 10-100 times, and the gas pressure of trimethylaluminum gas is 15Pa-25Pa.

[0070] Mobility test:

[0071] The mobility of trimethylaluminum-doped lead selenide colloidal quantum dot films was characterized by field effect transistor (FET) method. The structure of the entire target sample is shown in Figure 1. Figure 2 As shown, the field effect transistor includes an n-heavy doped Si layer, a SiO2 layer, a source, a drain, and a gate. A lead selenide colloidal quantum dot film based on trimethylaluminum doping is set at the source and drain. A three-probe test platform is used to test the source, drain, and gate electrodes respectively. The test is carried out in a nitrogen environment (oxygen <0.01ppm water <0.01ppm) with no light (illuminance <30nW / cm2400 nm-1700nm) throughout the test. The gate voltage is fixed at 0V, the source voltage is scanned from 0V to 1V, and the drain current is measured to verify whether the electrode is in ohmic contact with the quantum dot film. On the basis of ohmic contact, the source voltage is fixed at 0.5V, the gate voltage is scanned from -40V to 40V, the drain current is measured, and the transfer characteristic curve of the quantum dot film is obtained. For the test results, the linear region near 0V is selected for fitting to obtain the mobility of the film.

[0072] Experimental results: Figure 3 and Figure 4 As shown, Figure 3 This is the relationship curve between gate voltage and drain current before trimethylaluminum doping. Figure 4 This is the relationship curve between gate voltage and drain current after trimethylaluminum doping. Figure 3 and Figure 4 In the figure, the horizontal axis is the gate voltage in V, and the vertical axis is the drain current in A. After trimethylaluminum doping, the slope of the test curve of the trimethylaluminum-doped lead selenide colloidal quantum dot film increased by 5 times, proving that trimethylaluminum doping can bring a 5-fold increase in mobility.

[0073] The strategy of this application is to achieve a certain degree of trimethylaluminum doping by post-treating the prepared colloidal quantum dot film with trimethylaluminum gas in a vacuum environment. By controlling the purge time and reaction temperature of trimethylaluminum, its doping effect in the quantum dot film can be more accurately controlled, and the mobility of the film after doping can be improved by 1-2 orders of magnitude. The technical solution of trimethylaluminum gas doping can improve the mobility of colloidal quantum dots by 1-2 orders of magnitude, thereby achieving an improvement in the ultimate performance of the detector prepared therefrom.

[0074] In the preparation method of trimethylaluminum-doped lead selenide colloidal quantum dot film of the present application, the preparation method of trimethylaluminum-doped lead selenide colloidal quantum dot film includes: preserving lead selenide colloidal quantum dots in an n-octane solvent to obtain a quantum dot n-octane solution, wherein the ligand on the surface of the lead selenide colloidal quantum dots is oleic acid; dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution; filtering the quantum dot n-octane solution and the first mixed solution separately and then mixing them to obtain a second mixed solution; oscillating the second mixed solution for a first oscillation time and standing until the second mixed solution is separated into two layers of upper and lower solutions, removing the upper layer of the second mixed solution and adding a preset volume of n-octane solvent to obtain a third mixed solution; oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into two layers of upper and lower solutions, removing the third mixed solution The upper solution is obtained to obtain a fourth mixed solution; the fourth mixed solution is treated to obtain a DMF solution of lead selenide quantum dots with iodine ions and bromide ions as ligands; the DMF solution of lead selenide quantum dots is placed in a centrifuge for treatment and the upper yellow liquid is poured out, and the DMF solution remaining on the surface is removed by vacuum extraction for a preset extraction time to obtain lead selenide quantum dots; the lead selenide quantum dots are dissolved in a mixed solvent of n-butylamine and DMF to obtain a fifth mixed solution; the fifth mixed solution is spin-coated on the target sample and annealed for a preset annealing time to obtain an initial lead selenide colloidal quantum dot film; the initial lead selenide colloidal quantum dot film is placed in a cabin, the cabin is vacuumed until the air pressure reaches a preset pressure, and the initial lead selenide colloidal quantum dot film is heated to a preset temperature; trimethylaluminum gas is introduced into the cabin to obtain a lead selenide colloidal quantum dot film based on trimethylaluminum doping. The present application can improve the mobility of colloidal quantum dot detectors.

[0075] The above are only implementation methods of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a trimethylaluminum-doped lead selenide colloidal quantum dot film, characterized in that: The preparation method of the trimethylaluminum-doped lead selenide colloidal quantum dot film comprises: Preserving lead selenide colloidal quantum dots in an n-octane solvent to obtain a quantum dot n-octane solution, wherein the ligand on the surface of the lead selenide colloidal quantum dots is oleic acid; Dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution; The quantum dot n-octane solution and the first mixed solution are filtered and then mixed to obtain a second mixed solution; Oscillating the second mixed solution for a first oscillation time and standing until the second mixed solution is separated into an upper and lower solution, removing the upper solution of the second mixed solution and adding a preset volume of n-octane solvent to obtain a third mixed solution; Oscillating the third mixed solution for a second oscillation time and standing until the third mixed solution is separated into an upper and lower solution layer, and removing the upper solution of the third mixed solution to obtain a fourth mixed solution; treating the fourth mixed solution to obtain a DMF solution of lead selenide quantum dots with iodide ions and bromide ions as ligands; The lead selenide quantum dot DMF solution is placed in a centrifuge and the upper yellow liquid is poured off, and vacuum extraction is performed for a preset extraction time to remove the residual DMF solution on the surface to obtain lead selenide quantum dots; Dissolving lead selenide quantum dots in a mixed solvent of n-butylamine and DMF to obtain a fifth mixed solution; Spin coating the fifth mixed solution on the target sample and annealing the sample for a preset annealing time to obtain an initial lead selenide colloidal quantum dot film; Putting the initial lead selenide colloidal quantum dot film into a chamber, evacuating the chamber until the air pressure reaches a preset pressure, and heating the initial lead selenide colloidal quantum dot film to a preset temperature; Trimethylaluminum gas is introduced into the chamber to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film.

2. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 1, characterized in that: The concentration of the lead selenide colloidal quantum dots in the quantum dot n-octane solution is 10 mg / mL.

3. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 2, characterized in that: The step of dissolving lead iodide and lead bromide in a DMF solution to obtain a first mixed solution comprises: 0.92 g of lead iodide and 0.58 g of lead bromide were dissolved in 10 ml of DMF solution to obtain a first mixed solution.

4. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 3, characterized in that: The first oscillation duration is 40 seconds, and the second oscillation duration is 40 seconds.

5. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 4, characterized in that: The preset volume is 10 ml.

6. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 5, characterized in that: The preset extraction time is one hour.

7. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 6, characterized in that: The method of placing the lead selenide quantum dot DMF solution in a centrifuge and discarding the upper yellow liquid comprises: The lead selenide quantum dot DMF solution was placed in a centrifuge and centrifuged at a speed of 9000 rpm for 4 minutes.

8. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 7, characterized in that: In the mixed solvent of n-butylamine and DMF, the volume ratio of n-butylamine to DMF is 1:

1.

9. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 8, characterized in that: The preset annealing time is 10 minutes, and the preset pressure is 10 -6 pa-10 -4 pa, the preset temperature is 20 degrees Celsius to 100 degrees Celsius.

10. The method for preparing trimethylaluminum-doped lead selenide colloidal quantum dot film according to claim 9, characterized in that: The method of introducing trimethylaluminum gas into the chamber to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film comprises: Trimethylaluminum gas is introduced into the chamber in a pulse pumping manner to obtain a trimethylaluminum-doped lead selenide colloidal quantum dot film, wherein during pulse pumping, a single pumping time is 10 ms, a pumping time interval is 60s-150s, the number of pumpings is 10 times-100 times, and the gas pressure of the trimethylaluminum gas is 15Pa-25Pa.

Citation Information

Patent Citations

  • A method for obtaining an n-type doped metal chalcogenide quantum dot solid-state film, and an optoelectronic device comprising the obtained film

    CN111863985A

  • CdSe quantum dot, preparation method thereof and photoconductive diode

    CN113150785A

  • Method of manufacturing quantum dot-polymer composite and light source device having the quantum dot-polymer composite

    KR101605290B1

  • Quantum dot stabilized by halogen salt and method for manufacturing the same

    US20150291422A1

  • Method for obtaining an n-type doped metal chalcogenide quantum dot solid-state film, and an optoelectronic device comprising the obtained film