A method for preparing modified lithium manganese iron phosphate using manganese iron ammonium phosphate as a matrix
By preparing a precursor of manganese iron ammonium phosphate through a reverse co-precipitation method and introducing divalent doped metal ions, the problems of difficult preparation and insufficient performance of lithium manganese iron phosphate were solved, and a modified lithium manganese iron phosphate material with high energy density and good cycle stability was realized, which is suitable for lithium-ion battery cathode materials.
Patent Information
- Application Number
- CN202510052209.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-01-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-01-14
AI Technical Summary
Existing methods for preparing lithium manganese iron phosphate suffer from difficulties in preparation, poor electrochemical performance, unstable crystal structure, and insufficient rate performance and cycle stability of lithium manganese iron phosphate with high Mn atomic ratio, making it difficult to achieve large-scale industrial production.
A precursor of manganese iron ammonium phosphate was prepared by reverse coprecipitation. Divalent doped metal ions were introduced, and atomic-level distribution of metal ions was achieved through coprecipitation reaction. The precursor was then mixed with lithium salt and carbon source, followed by sand milling, spray drying and sintering to obtain modified lithium manganese iron phosphate.
It improves the energy density and cycle stability of lithium manganese iron phosphate, enhances its rate performance and cycle stability, and makes it suitable for large-scale industrial production.
Smart Images

Figure CN119841301B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of lithium-ion battery material preparation technology, and in particular relates to a method for preparing modified lithium manganese iron phosphate using manganese iron ammonium phosphate as a matrix. Background Technology
[0002] Lithium iron phosphate has become the mainstream cathode material in the energy field due to its advantages such as stable structure, low cost and environmental friendliness. However, its low voltage platform (3.4V) can no longer meet the market's demand for energy density. Lithium manganese iron phosphate inherits its advantages and greatly improves energy density. It is the next generation product of lithium iron phosphate and will surely occupy a huge market share in the future.
[0003] However, due to Mn 3+ Manganese iron phosphate (MFP) readily undergoes disproportionation reactions in aqueous solutions, making it impossible to directly prepare it using the traditional co-precipitation route, and subsequently, lithium manganese iron phosphate (LMP). Using organic solvents increases the risks and production costs. Solid-state methods are simple, but they cannot achieve uniform elemental distribution, resulting in poor electrochemical performance of the prepared LMP. The more studied solvothermal method is limited by high equipment requirements and the solubility limitations of many raw materials, resulting in small-scale production and requiring an excess lithium source, making it unsuitable for industrial production. Therefore, it is necessary to develop a route that can utilize traditional LFP equipment to produce LMP, enabling large-scale production and accelerating the industrialization of LMP.
[0004] Besides the difficulty in preparation, lithium manganese iron phosphate cathode materials also suffer from low intrinsic electronic conductivity and low Mn content. 3+ The Jahn-Teller effect leads to crystal structure instability, which in turn results in a significant decline in rate performance and cycle stability, thus limiting the development of lithium manganese iron phosphate with a high Mn atomic ratio. Summary of the Invention
[0005] To address the technical deficiencies in existing methods for preparing lithium manganese iron phosphate, this application provides a method for preparing modified lithium manganese iron phosphate using ammonium manganese iron phosphate as a matrix. This method improves the purity of the ammonium manganese iron phosphate precursor through a reverse co-precipitation method, and simultaneously introduces divalent doped metal ions during the co-precipitation reaction stage to achieve atomic-level distribution of metal ions, effectively improving the energy density and cycle stability of lithium manganese iron phosphate. The method includes the following steps:
[0006] S100. Prepare a mixed metal ion solution, a phosphate solution, and a precipitant solution. The mixed metal ion solution contains manganese salt, iron salt, and dopant salt. The manganese salt is one or more of manganese sulfate monohydrate, manganese chloride tetrahydrate, or manganese acetate tetrahydrate. The iron salt is one or more of ferrous sulfate heptahydrate or ferrous chloride tetrahydrate. The dopant salt is one or more of nickel sulfate, nickel chloride, cobalt sulfate, cobalt chloride, magnesium sulfate, or magnesium chloride. The phosphate solution is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or ammonium phosphate. The precipitant solution is one or more of ammonia water or sodium hydroxide solution.
[0007] S200. Place the prepared phosphate solution in a reaction vessel, add the precipitant under stirring and control the temperature and pH of the solution in the reaction vessel to be constant, then add the prepared metal ion mixed solution and precipitant solution in parallel to the reaction vessel, maintain the pH of the solution to be constant until the solution is completely drained, and then obtain the manganese iron ammonium phosphate suspension after stirring and aging.
[0008] S300. The obtained manganese iron ammonium phosphate suspension is subjected to solid-liquid separation. The supernatant is removed and the solid is repeatedly washed with deionized water and anhydrous ethanol until the conductivity of the washing solution drops below 500 μS / cm. Then, it is dried under vacuum to obtain the doped manganese iron ammonium phosphate monohydrate precursor. S400. The obtained doped manganese iron ammonium phosphate monohydrate precursor is mixed with lithium salt and carbon source and subjected to sanding treatment to obtain a uniformly mixed lithium manganese iron phosphate suspension. S500. The obtained lithium manganese iron phosphate suspension is spray-dried to obtain dry spherical powder. Then, the dry spherical powder is sintered under an inert atmosphere to obtain modified lithium manganese iron phosphate.
[0009] In some embodiments, in step S100, the total concentration of manganese salt, iron salt and doped salt in the metal ion mixed solution is 0.5-2 mol / L, the concentration of phosphate solution is 0.5-4 mol / L, and the concentration of precipitant is 1-15 mol / L.
[0010] In some embodiments, in step S200, the stirring intensity is 200-1000 r / min, the pH value of the solution in the reaction vessel is controlled at 4-10, the temperature of the solution in the reaction vessel is 20-80℃, the feeding rate of the manganese-iron mixed solution is 20-200 ml / min, the stirring time after the manganese-iron mixed solution is exhausted is 1-5 h, and the aging time is 4-20 h.
[0011] In some embodiments, in step S300, the drying temperature under vacuum is 60-100℃, the drying time is 12-36h, the vacuum pressure is -0.8MPa to -1MPa, and the molecular formula of the dried manganese ferric ammonium phosphate monohydrate precursor is NH4Mn. x Fey M 1-x-y PO4·H2O, wherein the atomic ratio (Mn+Fe+M) / P is 0.95-1.05, and the specific surface area is 15-25 m². 2 / g. In some embodiments, the lithium salt is one or more of lithium carbonate, lithium hydroxide, lithium oxalate, and lithium citrate.
[0012] In some embodiments, the carbon source is one or more of glucose, sucrose, phenolic epoxy resin, polyvinylpyrrolidone, and asphalt.
[0013] In some embodiments, in step S500, the sintering temperature is 600-800℃ and the sintering time is 4-8h.
[0014] In some embodiments, the inert atmosphere is one or more of nitrogen, argon, or helium.
[0015] Compared with existing technologies, this application prepares a precursor of manganese iron ammonium phosphate monohydrate by mixing manganese source, iron source, dopant ion source and phosphorus source through a reverse addition coprecipitation method. The reverse addition method can greatly reduce the formation of impurity phases, thereby improving the purity of the manganese iron ammonium phosphate precursor. At the same time, divalent doped metal ions are introduced in the coprecipitation reaction stage to achieve atomic-level distribution of metal ions, which effectively improves the energy density and cycle stability of lithium manganese iron phosphate. The prepared manganese iron ammonium phosphate monohydrate precursor is then mixed evenly with lithium salt and carbon source, followed by sand milling, spray drying and sintering to finally obtain carbon-coated modified lithium manganese iron phosphate with good crystallinity and excellent electrochemical performance. Attached Figure Description
[0016] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0017] Figure 1 This is a flowchart of a method for preparing modified lithium manganese iron phosphate using ammonium manganese phosphate as a matrix, as described in this application.
[0018] Figure 2 Scanning electron microscope (SEM) images of the modified lithium manganese iron phosphate prepared in Example 1 of this application are provided.
[0019] Figure 3 The charge-discharge curves of the modified lithium manganese iron phosphate prepared in Example 1 of this application at a rate of 0.1C are shown.
[0020] Figure 4The charge-discharge curves of the modified lithium manganese iron phosphate prepared in Example 1 of this application at a 1C rate are shown.
[0021] Figure 5 The rate performance diagram of the modified lithium manganese iron phosphate prepared in Example 1 of this application is given;
[0022] Figure 6 The cycling performance of the modified lithium manganese iron phosphate prepared in Example 1 of this application at 1C rate is shown in the figure.
[0023] Figure 7 Scanning electron microscope (SEM) images of the modified lithium manganese iron phosphate prepared in Example 2 of this application are provided.
[0024] Figure 8 The charge-discharge curves of the modified lithium manganese iron phosphate prepared in Example 2 of this application at a rate of 0.1C are shown.
[0025] Figure 9 The charge-discharge curves of the modified lithium manganese iron phosphate prepared in Example 2 of this application at a 1C rate are shown.
[0026] Figure 10 The rate performance diagram of the modified lithium manganese iron phosphate prepared in Example 2 of this application is given;
[0027] Figure 11 The cycling performance of the modified lithium manganese iron phosphate prepared in Example 2 of this application at 1C rate is shown in the figure.
[0028] Figure 12 Scanning electron microscope (SEM) images of the modified lithium manganese iron phosphate prepared in Example 3 of this application are provided.
[0029] Figure 13 The charge-discharge curves of the modified lithium manganese iron phosphate prepared in Example 3 of this application at a rate of 0.1C are shown.
[0030] Figure 14 The charge-discharge curves of the modified lithium manganese iron phosphate prepared in Example 3 of this application at a 1C rate are shown.
[0031] Figure 15 The rate performance diagram of the modified lithium manganese iron phosphate prepared in Example 3 of this application is given;
[0032] Figure 16 The cycling performance of the modified lithium manganese iron phosphate prepared in Example 3 of this application at 1C rate is shown in the figure.
[0033] Figure 17 A scanning electron microscope image of lithium manganese iron phosphate prepared in Comparative Example 1 of this application is provided;
[0034] Figure 18The charge-discharge curves of lithium manganese iron phosphate prepared in Comparative Example 1 of this application at a rate of 0.1C are shown.
[0035] Figure 19 The charge-discharge curves of lithium manganese iron phosphate prepared in Comparative Example 1 of this application at 1C rate are shown.
[0036] Figure 20 The rate performance diagram of lithium manganese iron phosphate prepared in Comparative Example 1 of this application is given;
[0037] Figure 21 The cycling performance of lithium manganese iron phosphate prepared by Comparative Example 1 of this application at a 1C rate is shown in the figure. Detailed Implementation
[0038] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values 1 and 2 are listed, and if maximum range values 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0039] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0040] refer to Figure 1 As shown in the embodiments of this application, a method for preparing modified lithium manganese iron phosphate using ammonium manganese phosphate as a matrix is provided. The method includes the following steps:
[0041] S100. Prepare a mixed metal ion solution, a phosphate solution, and a precipitant solution. The mixed metal ion solution contains manganese salt, iron salt, and dopant salt. The manganese salt is one or more of manganese sulfate monohydrate, manganese chloride tetrahydrate, or manganese acetate tetrahydrate. The iron salt is one or more of ferrous sulfate heptahydrate or ferrous chloride tetrahydrate. The dopant salt is one or more of nickel sulfate, nickel chloride, cobalt sulfate, cobalt chloride, magnesium sulfate, or magnesium chloride. The phosphate solution is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or ammonium phosphate. The precipitant solution is one or more of ammonia water or sodium hydroxide solution.
[0042] In this step, the total concentration of manganese salt, iron salt and doped salt in the metal ion mixed solution is 0.5-2 mol / L, the concentration of phosphate solution is 0.5-4 mol / L, and the concentration of precipitant is 1-15 mol / L.
[0043] S200. Place the prepared phosphate solution in a reaction vessel, add the precipitant under stirring and control the temperature and pH of the solution in the reaction vessel to be constant, then add the prepared metal ion mixed solution and precipitant solution in parallel to the reaction vessel, maintain the pH of the solution to be constant until the solution is completely drained, and then obtain the manganese iron ammonium phosphate suspension after stirring and aging.
[0044] In this step, the reaction vessel is a reaction kettle, the stirring intensity is 200-1000 r / min, the pH value of the solution in the reaction vessel is controlled at 4-10, the temperature of the solution in the reaction vessel is 20-80℃, the feeding rate of the manganese-iron mixed solution is 20-200 ml / min, the stirring time after the manganese-iron mixed solution is exhausted is 1-5 h, and the aging time is 4-20 h.
[0045] S300. The obtained manganese iron ammonium phosphate suspension is subjected to solid-liquid separation. The supernatant is removed and the solid is repeatedly washed with deionized water and anhydrous ethanol until the conductivity of the washing solution drops to below 500 μS / cm. Then, it is dried under vacuum to obtain the doped manganese iron ammonium phosphate monohydrate precursor.
[0046] In this step, the drying temperature under vacuum is 60-100℃, the drying time is 12-36h, and the vacuum pressure is -0.8MPa. The molecular formula of the dried manganese ferric ammonium phosphate monohydrate precursor is NH4Mn. x Fe y M 1-x-y The dried manganese iron ammonium phosphate precursor, prepared by PO4·H2O, exhibits a uniform two-dimensional plate-like morphology, with an atomic ratio (Mn+Fe+M) / P of 0.95-1.05 and a specific surface area of 15-25 m². 2 / g.
[0047] S400. The obtained doped manganese iron ammonium phosphate precursor is mixed with lithium salt and carbon source and then subjected to sanding treatment to obtain a uniformly mixed lithium manganese iron phosphate suspension.
[0048] In this step, the lithium salt is one or more of lithium carbonate, lithium hydroxide, lithium oxalate, and lithium citrate, and the carbon source is one or more of glucose, sucrose, phenolic epoxy resin, polyvinylpyrrolidone, and asphalt.
[0049] S500. The obtained lithium manganese iron phosphate suspension is spray-dried to obtain dry spherical powder. Then, the dry spherical powder is sintered under an inert atmosphere to obtain modified lithium manganese iron phosphate.
[0050] In this step, the lithium manganese iron phosphate suspension is dried under vacuum conditions at a temperature of 60-100℃ for 12-36 hours and a vacuum pressure of -0.8MPa to -1MPa. The sintering temperature is 600-800℃ for 4-8 hours, and the inert atmosphere is one or more of nitrogen, argon, or helium.
[0051] In the above embodiments, a precursor of manganese iron ammonium phosphate monohydrate is first prepared by mixing manganese source, iron source, dopant ion source and phosphorus source through a reverse addition coprecipitation method. The reverse addition method can greatly reduce the formation of impurity phases, thereby effectively improving the purity of the manganese iron ammonium phosphate precursor. At the same time, the introduction of divalent dopant metal ions in the coprecipitation reaction stage achieves atomic-level distribution of metal ions, effectively improving the energy density and cycle stability of lithium manganese iron phosphate. Then, the prepared manganese iron ammonium phosphate monohydrate precursor is mixed evenly with lithium salt and carbon source, followed by sand milling, spray drying and sintering to obtain carbon-coated modified lithium manganese iron phosphate with good crystallinity. This method is simple and the prepared lithium manganese iron phosphate has good rate performance.
[0052] To further illustrate the technical principles and effects of this application, the following describes the disclosure of this application in more detail with several embodiments. These embodiments are merely illustrative, as various modifications and variations within the scope of the disclosure of this application will be apparent to those skilled in the art. Unless otherwise stated, all reagents and raw materials used in the embodiments are commercially available or synthesized by conventional methods, and the instruments and equipment used in the embodiments are commercially available.
[0053] Example 1
[0054] 1. Weigh 172.55g (1.5mol) of ammonium dihydrogen phosphate and dissolve it in 1000ml of deionized water. Transfer the solution to a reaction vessel and stir at 600r / min. Pump 13.38mol / L concentrated ammonia into the reaction vessel and control the pH of the solution in the reaction vessel to 6. Adjust the solution temperature to 40℃.
[0055] 2. Weigh 105.64g (0.38mol) ferrous sulfate heptahydrate, 101.412g (0.6mol) manganese sulfate monohydrate and 5.26g (0.02mol) nickel sulfate hexahydrate and dissolve them in 1000ml of deionized water. Pump the solution into the reaction vessel at a rate of 40ml / min and adjust the stirring speed of the reaction vessel to 500r / min. At the same time, pump concentrated ammonia water to control the pH value of the solution to be constant at 6. After the metal ion mixture has been completely drained, stir for 3 hours and age for 12 hours to obtain a suspension of manganese iron ammonium phosphate.
[0056] 3. The obtained manganese ferric ammonium phosphate suspension was placed in a centrifuge for solid-liquid separation. After repeated washing with deionized water and anhydrous ethanol until the conductivity of the washing solution decreased to below 500 μS / cm, it was dried under vacuum to obtain the nickel-doped manganese ferric ammonium phosphate monohydrate precursor with the molecular formula NH4Mn. 0.6 Fe 0.38 Ni 0.02 PO4·H2O;
[0057] 4. Weigh 1.57g of sucrose and dissolve it in 100ml of deionized water. Then add 18.63g (0.1mol) of dried nickel-doped manganese iron ammonium phosphate monohydrate precursor and 3.79g (0.105mol) of lithium carbonate and stir to disperse evenly. Then transfer it to a sand mill and mill until the particle size is less than 400nm to obtain a uniformly mixed manganese iron lithium phosphate suspension. The sand mill speed is 2000r / min and the milling time is 30min.
[0058] 5. The milled lithium manganese iron phosphate suspension is spray-dried at a feed rate of 650 ml / h and an inlet temperature of 220℃. The dried powder is then placed in a tube furnace and heated to 350℃ at a rate of 5℃ / min, held for 5 hours, and then heated to 700℃ and held for 4 hours to obtain nickel-doped modified lithium manganese iron phosphate with the molecular formula LiMn. 0.6 Fe 0.38 Ni 0.02 PO4 / C.
[0059] Example 2
[0060] 1. Weigh 172.55g (1.5mol) of ammonium dihydrogen phosphate and dissolve it in 1000ml of deionized water. Transfer the solution to a reaction vessel and stir at 600r / min. Pump 13.38mol / L concentrated ammonia into the reaction vessel and control the pH of the solution in the reaction vessel to 6. Adjust the solution temperature to 60℃.
[0061] 2. Weigh 105.64g (0.38mol) ferrous sulfate heptahydrate, 101.412g (0.6mol) manganese sulfate monohydrate and 5.62g (0.02mol) cobalt sulfate heptahydrate and dissolve them in 1000ml of deionized water. Pump the solution into the reaction vessel at a rate of 80ml / min and adjust the reaction vessel speed to 1000r / min. At the same time, pump concentrated ammonia water to control the pH value of the solution to be constant at 6. After the metal ion mixture has been completely drained, stir for 3 hours and age for 12 hours to obtain a suspension of manganese iron ammonium phosphate.
[0062] 3. The suspension of ferric ammonium manganese phosphate was centrifuged for solid-liquid separation. After repeated washing with deionized water and anhydrous ethanol until the conductivity of the washing solution decreased to below 500 μS / cm, it was dried under vacuum to obtain the cobalt-doped ferric ammonium manganese phosphate monohydrate precursor, with the molecular formula NH4Mn. 0.6 Fe 0.38 Co 0.02 PO4 / C·H2O;
[0063] 4. Weigh 1.57g of sucrose and dissolve it in 100ml of deionized water. Then add 18.63g (0.1mol) of dried cobalt-doped manganese iron ammonium phosphate monohydrate precursor and 3.79g of lithium carbonate and stir to disperse evenly. Then transfer it to a sand mill and mill until the particle size is less than 400nm to obtain a uniformly mixed manganese iron lithium phosphate suspension. The sand mill speed is 2000r / min and the milling time is 30min.
[0064] 5. The milled lithium manganese iron phosphate suspension is spray-dried at a feed rate of 650 ml / h and an inlet temperature of 220℃. The dried powder is then placed in a tube furnace and heated to 350℃ at a rate of 5℃ / min, held for 5 hours, and then heated to 800℃ and held for 4 hours to obtain cobalt-doped modified lithium manganese iron phosphate with the molecular formula LiMn. 0.6 Fe 0.38 Co 0.02 PO4 / C.
[0065] Example 3
[0066] 1. Weigh 172.55g (1.5mol) of ammonium dihydrogen phosphate and dissolve it in 1000ml of deionized water. Transfer the solution to a reaction vessel and stir at 600r / min. Pump 13.38mol / L concentrated ammonia into the reaction vessel to control the pH of the solution in the reaction vessel to 6 and adjust the solution temperature to 40℃.
[0067] 2. Weigh 105.64g (0.38mol) ferrous sulfate heptahydrate, 101.412g (0.6mol) manganese sulfate monohydrate and 2.41g (0.02mol) anhydrous magnesium sulfate and dissolve them in 1000ml of deionized water. Pump the solution into the reaction vessel at a rate of 100ml / min and adjust the reaction vessel speed to 800r / min. At the same time, pump concentrated ammonia water to control the pH value of the solution to be constant at 6. After the metal ion mixture has been completely drained, stir for 3 hours and age for 12 hours to obtain a suspension of manganese ferric ammonium phosphate.
[0068] 3. The suspension of ferric ammonium manganese phosphate was centrifuged for solid-liquid separation. After repeated washing with deionized water and anhydrous ethanol until the conductivity of the washing solution decreased to below 500 μS / cm, it was dried under vacuum to obtain the magnesium-doped ferric ammonium manganese phosphate precursor, with the molecular formula NH4Mn. 0.6 Fe 0.38 Mg 0.02 PO4·H2O;
[0069] 4. Weigh 1.57g of sucrose and dissolve it in 100ml of deionized water. Then add 18.63g (0.1mol) of dried magnesium-doped manganese iron ammonium phosphate monohydrate precursor and 3.79g of lithium carbonate and stir to disperse evenly. Then transfer it to a sand mill and mill until the particle size is less than 400nm to obtain a uniformly mixed lithium manganese iron ammonium phosphate suspension. The sand mill speed is 2000r / min and the milling time is 30min.
[0070] 5. The milled lithium manganese iron phosphate suspension is spray-dried at a feed rate of 650 ml / h and an inlet temperature of 220℃. The dried powder is then placed in a tube furnace and heated to 350℃ at a rate of 5℃ / min, held for 5 hours, and then heated to 500℃ and held for 4 hours to obtain magnesium-doped modified lithium manganese iron phosphate with the molecular formula LiMn. 0.6 Fe 0.38 Mg 0.02 PO4 / C.
[0071] Comparative Example 1
[0072] 1. Weigh 172.55g (1.5mol) of ammonium dihydrogen phosphate and dissolve it in 1000ml of deionized water. Transfer the solution to a reaction vessel and stir at 600r / min. Pump 13.38mol / L concentrated ammonia into the reaction vessel and control the pH of the solution in the reaction vessel to 6. Adjust the solution temperature to 40℃.
[0073] 2. Weigh 111.20g (0.4mol) ferrous sulfate heptahydrate and 101.412g (0.6mol) manganese sulfate monohydrate and dissolve them in 1000ml of deionized water. Pump the solution into the reaction vessel at a rate of 40ml / min. Adjust the stirring speed of the reaction vessel to 500r / min. At the same time, pump in concentrated ammonia water to keep the pH value constant at 6. After the metal ion mixture has been completely drained, stir for 3 hours and age for 12 hours to obtain a suspension of manganese ferric ammonium phosphate.
[0074] 3. The precursor suspension was centrifuged for solid-liquid separation. The solution was repeatedly washed with deionized water and anhydrous ethanol until the conductivity of the washing solution decreased to below 500 μS / cm. After drying under vacuum, the precursor, ferric ammonium manganese phosphate monohydrate, was obtained, with the molecular formula NH4Mn. 0.6 Fe 0.4 PO4·H2O;
[0075] 4. Weigh 1.57g of sucrose and dissolve it in 100ml of deionized water. Then add 18.63g (0.1mol) of dried doped manganese iron ammonium phosphate monohydrate precursor and 3.79g of lithium carbonate and stir to disperse evenly. Then transfer it to a sand mill and mill until the particle size is less than 400nm to obtain a uniformly mixed manganese iron ammonium phosphate suspension. The sand mill speed is 2000r / min and the milling time is 30min.
[0076] 5. The milled lithium manganese iron phosphate suspension was spray-dried at a feed rate of 650 ml / h and an inlet temperature of 220℃. The dried powder was then placed in a tube furnace and heated to 350℃ at a rate of 5℃ / min, held for 5 hours, and then heated to 700℃ and held for 4 hours to obtain lithium manganese iron phosphate with the molecular formula LiMn. 0.6 Fe 0.4 PO4 / C.
[0077] The lithium manganese iron phosphate cathode materials prepared in Examples 1-3 and Comparative Example 1 were tested by scanning electron microscopy, energy-dispersive X-ray spectroscopy, rate performance, and cycle performance, as shown in Table 1 and... Figure 2-21 As shown, all the prepared materials are well-dispersed spherical particles, indicating that doping does not affect their spherical morphology. The energy spectrum shows that the distribution of each constituent element and dopant element is relatively uniform, demonstrating the advantages of co-precipitation method and in-situ doping.
[0078] Table 1. Test data of the modified lithium manganese iron phosphate prepared in Examples 1-3 and Comparative Example 1, including discharge specific capacity, discharge voltage, and capacity retention after 100 cycles at 0.1C and 1C rates.
[0079]
[0080] As shown in the electrochemical performance diagram and Table 1, the lithium manganese iron phosphate material prepared in Comparative Example 1 has a discharge specific capacity of 147.0 mAh / g and a discharge voltage of 3.864 V at a 0.1C rate, and a discharge specific capacity of 128.0 mAh / g and a discharge voltage of 3.612 V at a 1C rate, indicating that its performance is average.
[0081] The modified lithium manganese iron phosphate materials prepared in Examples 1-3 all exhibited discharge specific capacities greater than 151 mAh / g at 0.1C rate and discharge voltages above 3.9V. At 1C rate, their discharge specific capacities were all above 131 mAh / g and discharge voltages above 3.63V. Compared to Comparative Example 1, the modified lithium manganese iron phosphate materials prepared in Examples 1-3 demonstrated superior rate performance and higher discharge voltages.
[0082] Meanwhile, the modified lithium manganese iron phosphate prepared in Examples 1-3 all had a capacity retention rate of more than 90.8% after 100 cycles at 1C rate, with the highest being 94.6% in Example 3; while the cycle retention rate of Comparative Example 1 was only 84.4%. This shows that the modified lithium manganese iron phosphate material has better cycle stability.
[0083] In summary, by doping divalent metal ions during the preparation of manganese iron ammonium phosphate precursor by the reverse coprecipitation method, atomic-level distribution of metal ions can be achieved, thereby improving the energy density and cycle stability of modified manganese iron ammonium phosphate, and enabling the modified manganese iron ammonium phosphate material to have better rate performance at 0.1C and 1C rates.
[0084] The above provides a detailed description of a method for preparing modified lithium manganese iron phosphate using ammonium manganese phosphate as a matrix, as provided in this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are merely for the purpose of helping to understand the core ideas of this application. It should be noted that those skilled in the art can make various improvements and modifications to this application without departing from the principles of this application, and these improvements and modifications also fall within the protection scope of the claims of this application.
Claims
1. A method for preparing modified lithium manganese iron phosphate using ammonium manganese phosphate as a matrix, characterized in that, The method includes the following steps: S100. Prepare a mixed metal ion solution, a phosphate solution, and a precipitant solution. The mixed metal ion solution contains manganese salt, iron salt, and dopant salt. The manganese salt is one or more of manganese sulfate monohydrate, manganese chloride tetrahydrate, or manganese acetate tetrahydrate. The iron salt is one or more of ferrous sulfate heptahydrate or ferrous chloride tetrahydrate. The dopant salt is one or more of nickel sulfate, nickel chloride, cobalt sulfate, cobalt chloride, magnesium sulfate, or magnesium chloride. The phosphate solution is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or ammonium phosphate. The precipitant solution is one or more of ammonia or sodium hydroxide solution. The total concentration of manganese salt, iron salt, and dopant salt in the mixed metal ion solution is 0.5-2 mol / L, the concentration of the phosphate solution is 0.5-4 mol / L, and the concentration of the precipitant is 1-15 mol / L. S200. Place the prepared phosphate solution in a reaction vessel, add a precipitant under stirring, and control the temperature and pH of the solution in the reaction vessel to be constant. Then, add the prepared metal ion mixed solution and precipitant solution in parallel to the reaction vessel, maintain the pH of the solution to be constant until the solution is completely drained, and then stir and age to obtain a manganese iron ammonium phosphate suspension. The stirring intensity is 200-1000 r / min, the pH of the solution in the reaction vessel is controlled to be constant at 6, the temperature of the solution in the reaction vessel is 40-80℃, the feeding rate of the manganese iron mixed solution is 20-200 ml / min, the stirring time after the manganese iron mixed solution is completely drained is 1-5 h, and the aging time is 4-20 h. S300. The obtained manganese ferric ammonium phosphate suspension is subjected to solid-liquid separation. The supernatant is removed, and the solid is repeatedly washed with deionized water and anhydrous ethanol until the conductivity of the washing solution drops below 500 μS / cm. Then, it is dried under vacuum to obtain the doped manganese ferric ammonium phosphate monohydrate precursor. The drying temperature under vacuum is 60-100℃, the drying time is 12-36 h, and the vacuum pressure is -0.8 MPa to -1 MPa. The molecular formula of the dried doped manganese ferric ammonium phosphate monohydrate precursor is NH4Mn. x Fe y M 1-x-y PO4·H2O, with an atomic ratio of (Mn+Fe+M) / P of 0.95-1.05 and a specific surface area of 15-25 m². 2 / g; S400. The obtained doped manganese iron ammonium phosphate precursor is mixed with lithium carbonate and a carbon source and then subjected to a sanding process to obtain a uniformly mixed lithium manganese iron phosphate suspension. The carbon source is one or more of glucose, sucrose, phenolic epoxy resin, polyvinylpyrrolidone, and asphalt. S500. The obtained lithium manganese iron phosphate suspension is spray-dried to obtain dry spherical powder. Then, the dry spherical powder is sintered in an inert atmosphere at a temperature of 600-800℃ for 4-8 hours to obtain modified lithium manganese iron phosphate.
2. The method according to claim 1, characterized in that, The inert atmosphere is one or more of nitrogen, argon, or helium.
Citation Information
Patent Citations
Ferromanganese phosphate precursor as well as preparation method and application thereof
CN117886292A
Preparation method of ammonium manganese iron phosphate precursor and lithium manganese iron phosphate
CN118164461A
Ferric manganese phosphate precursor, lithium ferric manganese phosphate and preparation method and application of ferric manganese phosphate precursor and lithium ferric manganese phosphate
CN118666263A