An ultra-thin photosensitive resin coating

By preparing a copper fiber film and electrostatically spraying photosensitive resin and a water and oxygen barrier layer on the eyeglass frame, the problems of insignificant color change and aging of the eyeglass frame were solved, achieving the effects of photosensitive color change and resistance to yellowing.

CN120041040BActive Publication Date: 2026-11-17张勇军
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510028830.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-11
Publication Date
2026-11-17
Estimated Expiration
2042-04-11

AI Technical Summary

Technical Problem

Existing eyeglass frames have insufficient color variation, low aesthetic appeal, and are prone to aging due to ultraviolet rays and moisture in the air, resulting in loss of luster, discoloration, and darkening, as well as a short lifespan.

Method used

Copper fiber membranes were prepared by ion beam-assisted spinning, and combined with electrostatic field spraying of photosensitive resin and water-oxygen barrier layer to form an ultra-thin photosensitive resin coating. The photosensitive material changes color under light, and the resistance to yellowing is improved by alumina and silica films.

Benefits of technology

It achieves a photosensitive color-changing effect on the eyeglass frames, enhancing their aesthetics, and extends their lifespan by using a water-oxygen barrier layer to prevent yellowing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses an ultrathin photosensitive resin coating and its preparation method, relating to the field of coating materials technology. First, this invention utilizes 3-hydroxy-1-naphthylamine, 5-chloro-1,3,3-trimethyl-2-methyleneindoline, 3-aminophthalate, and silver chloride to modify epoxy resin, forming a photosensitive resin that allows the coating to change with light exposure. Then, using ion beam-assisted spinning, a copper fiber film is formed on the surface of an eyeglass frame. This film serves as the cathode, and a high-voltage electric field is used to ionize the photosensitive resin, depositing it onto the frame. Finally, electrostatic field-assisted spraying is used to grow layer-by-layer alumina and silica films, effectively blocking water and oxygen. The ultrathin photosensitive resin coating prepared by this invention exhibits photosensitive color-changing and yellowing-resistant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating materials technology, specifically to an ultrathin photosensitive resin coating. Background Technology

[0002] Most existing eyeglass frames are single-color. Some eyeglass frames with color-changing function are simply made by spraying thermochromic or photochromic powder onto the surface of the frame. Because the frame itself is dark, the color after spraying the color-changing powder is not bright enough, and the color change is not obvious enough, resulting in low aesthetic appeal. In addition, the temperature change is often very slow. For example, when you are out and about, the temperature generally does not change much. It is also easy to fall off when exposed to sweat or rain, resulting in a short service life.

[0003] Since eyeglasses are products that people carry with them, they are frequently exposed to outdoor ultraviolet rays and are in contact with oxygen and moisture in the air for extended periods. This causes ordinary eyeglass frames to age, resulting in defects such as loss of luster, discoloration, and darkening over time. The surface color will turn yellow, which is more noticeable on some light-colored frames, seriously affecting the appearance of the eyeglasses and limiting their daily use. Summary of the Invention

[0004] The purpose of this invention is to provide an ultrathin photosensitive resin coating and its preparation method, so as to solve the problems existing in the prior art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: an ultra-thin photosensitive resin coating, wherein the ultra-thin photosensitive resin coating is prepared by the following method: using ion beam-assisted spinning on an eyeglass frame to obtain a copper fiber film eyeglass frame; then using the copper fiber film eyeglass frame as the cathode of the electric field and a nozzle as the anode, a photosensitive resin is sprayed to obtain a substrate coating; and then electrostatic field-assisted spraying is used to obtain a water and oxygen barrier layer.

[0006] Furthermore, the photosensitive resin is prepared from epoxy resin, 3-hydroxy-1-naphthylamine, 5-chloro-1,3,3-trimethyl-2-methyleneindoline, 3-aminophthalate and silver chloride.

[0007] Furthermore, the water-oxygen barrier layer comprises an aluminum oxide film and a silicon dioxide film.

[0008] Furthermore, a method for preparing an ultrathin photosensitive resin coating includes the following preparation steps: (1) Place the pretreated eyeglass frame in an ion thinning instrument and evacuate it to 3.2 × 10⁻⁶. -3 ~5.6×10 -3Under an argon atmosphere, the film is bombarded at 15-23° for 15-27 seconds, then bombarded at 3-9° for 8-17 seconds. Using copper paste as the spinning solution, the film is spun to a thickness of 10-30 μm. After drying at 40-50°C for 4-10 hours, the film is heated to 400-600°C at 2-5°C / min under a hydrogen atmosphere and held for 2-5 hours. Then, the film is heated to 650-800°C at 1-3°C / min and held for 1-3 hours. Finally, the film is cooled to 500°C at 4-9°C / min and allowed to cool naturally to room temperature to obtain a copper fiber film eyeglass frame. (2) Using a copper fiber film eyeglass frame as the cathode and a nozzle as the anode, spray 0.3 to 0.7 times the weight of the copper fiber film eyeglass frame with photosensitive resin, and cure at 30 to 50°C for 40 to 50 hours to obtain a base coating; (3) Place the substrate coating in an electrostatic field with an electric field voltage of 10~30kV, heat it to 280~330℃, spray the alumina precursor solution at 20~30mL / h, spray the distance at 30~40mm, spray for 60~120s, with an interval of 180s, spray for a total of 12~24min, dry at 90~120℃ for 4~6h, place it in a tube furnace, react at 300~360℃ for 1~3h under a hydrogen atmosphere, then place it in the same electrostatic field, spray the silica sol at the same speed for 10~22min, heat to 100~130℃, dry for 1~5min, then heat to 400~450℃, and keep warm for 2~5h to obtain an ultrathin photosensitive resin coating.

[0009] Further, in step (1), the pre-treatment of the eyeglass frame is carried out by washing the eyeglass frame with acetone and anhydrous ethanol for 5 to 11 minutes at 25 to 35 kHz.

[0010] Furthermore, in step (1), the bombardment energy of the ion thinning instrument is 1~6keV, the argon flow rate is 20~30sccm, the size of the spinning head is 2~3mm, the flow rate is 22~34mL / min, and the air gap is 18~30cm.

[0011] Further, the copper paste in step (1) is prepared by mixing polyethersulfone, N-methylpyrrolidone and polyvinylpyrrolidone in a mass ratio of 1:4:0.2 to 1:4:0.4, grinding at 14 to 36 rpm for 4 to 9 hours, adding copper powder at 6 to 11 times the mass of polyethersulfone, grinding at the same speed for 44 to 50 hours, and then vacuuming for 33 to 59 minutes.

[0012] Furthermore, the photosensitive resin in step (2): A. Mix E-44 epoxy resin, ethylene glycol monobutyl ether, and anhydrous ethanol in a mass ratio of 1:0.3:0.2~1:0.5:0.3. Under nitrogen protection, heat to 60~75℃ and stir until dissolved. Then add 0.4~0.7 times the mass of E-44 epoxy resin of 3-hydroxy-1-naphthylamine. After reacting for 12~15 hours, add 0.6~2.1 times the mass of E-44 epoxy resin of an aqueous ethanol solution. The mass ratio of ethanol to water in the aqueous ethanol solution is 0.25:1. Let stand for 18~34 minutes to obtain the photosensitive resin matrix. B. Mix photosensitive resin matrix, sodium hydroxide, and deionized water in a mass ratio of 1:0.3:8~1:0.6:15. Cool the mixture in a salt bath to -5~0℃. Then add 0.4~0.7 times the mass of the photosensitive resin matrix containing sodium nitrite. While stirring at 50~100 rpm, add 2~6 times the mass of the photosensitive resin matrix containing 42% sulfuric acid. After reacting for 57~71 min, filter the mixture and wash it with deionized water until the solution pH reaches 6~7. Then add 21~30 times the mass of the photosensitive resin matrix containing methanol. Under nitrogen protection, heat the mixture to 66~80℃ and add 0.6~1 times the mass of the photosensitive resin matrix containing methanol. 5-chloro-1,3,3-trimethyl-2-methyleneindoline was reacted at 0.3 times its volume for 8-14 hours, and then concentrated at 200-300 rpm and 60-80 °C for 2-4 hours to obtain a spiroxazine compound. 3-aminophthalic acid ester, pyridine, and the spiroxazine compound were mixed at a mass ratio of 1:6:1 to 1:14:2, stirred at 100-200 rpm for 6-10 hours, and then concentrated at 80-100 °C under vacuum of 0.04-0.08 MPa for 2-5 hours. The mixture was then washed 5-10 times successively with ethyl acetate, distilled water, and saturated brine, and dried at 40-60 °C for 5-10 hours to obtain a modified resin. C. Mix the modified resin with 4-10 times its weight of methanol. At 20-30℃, add 0.7-1.4 times its weight of 25-28% ammonia solution (by mass) at a rate of 0.5-1.5 mL / min. Stir at 50-100 rpm for 6-9 hours. Then cool to 0-5℃ and maintain this temperature for 0.5-1.5 hours. Filter the mixture. Next, add 1.0-2.1 times its weight of triethylamine and 4-8 times its weight of tetrahydrofuran (by mass) of the modified resin. Mix thoroughly and then cool to -10-0℃. Stir at 0.6-1.2 mL / min. Add 1.2 to 2.6 times the mass of the modified resin of trifluoroacetic anhydride at a rate of L / min, and react at -10 to 0℃ for 58 to 71 min. Then, raise the temperature to 30 to 40℃ and react for 2 to 5 h. Distill at 50 to 65℃ under a vacuum of 0.04 to 0.08 MPa for 3 to 6 h. Then, add 2 to 4 times the mass of the modified resin of deionized water and 3 to 6 times the mass of the modified resin of ethyl acetate. Separate the mixture, wash with distilled water 3 to 7 times, and distill at 60 to 71℃ under a vacuum of 0.05 to 0.1 MPa for 2 to 4 h to obtain the nitrile compound. D. A nitrile compound, silver chloride, dimethylacetamide, and 1,8-diazabicyclo[5.4.0]undec-7-ene are mixed in a mass ratio of 1:0.3:5:0.001 to 1:0.6:9:0.001. The mixture is microwaved at 180-310°C for 8-20 minutes, washed 4-10 times with deionized water, anhydrous ethanol, and acetone, centrifuged at 8000-10000 rpm for 1-5 minutes, filtered, and dried at 60-73°C for 2-6 hours to obtain a photosensitive resin precursor. The photosensitive resin precursor, diethylenetriamine, polydimethylsiloxane, n-butanol, and xylene are mixed in a mass ratio of 1:0.08:0.6:0.6 to 1:0.22:0.9:0.9 to obtain the photosensitive resin.

[0013] Further, the alumina precursor solution in step (3) is prepared by mixing aluminum nitrate, urea and sodium chloride in a mass ratio of 1:8:3 to 1:13:7.

[0014] Further, in step (3), the silica sol is prepared by mixing tetraethyl orthosilicate, anhydrous ethanol, deionized water, and nitric acid with a mass fraction of 58% in a mass ratio of 1:1:0.2:0.02 to 1:2:1.0:0.05, heating to 50-60°C, and refluxing for 3-5 hours to obtain a tetraethyl orthosilicate mixture; adding 17-20 times the volume of anhydrous ethanol to the tetraethyl orthosilicate mixture to obtain a silica sol.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: This invention uses photosensitive resin as a base material and coats it with a water and oxygen barrier layer to prepare a coating for eyeglass frames, thereby achieving the effects of photosensitive color change and resistance to yellowing.

[0016] First, the amino group of 3-hydroxy-1-naphthylamine is grafted onto the epoxy resin molecule through a ring-opening reaction. Then, under the action of sodium nitrosamine, a nitrosyl group is introduced at the ortho position of the hydroxyl group, and it forms a spirooxazine compound with 5-chloro-1,3,3-trimethyl-2-methyleneindoline, giving the coating photosensitivity. The polyhydroxyl nature of the epoxy resin increases the polarity of the spirooxazine compound, resulting in more hydrogen bonds between molecules, increasing its rigidity, making the light-exposed ring-opening structure more stable, and extending the photosensitive lifetime of the coating. Next, the amino group of 3-aminophthalate reacts with the spirooxazine... The chloride ions of the compound combine, and after its ester group is amidated and nitrified, it coordinates with silver chloride. Through the attraction of hydrogen bonds, it self-assembles into an organic-inorganic amorphous composite network structure and is embedded therein to obtain a photosensitive resin. When exposed to light, the ring-opening organic matter undergoes intermolecular transitions under the further induction of light, generating colored free radicals, which promote the oxidation and valence change of silver ions, achieving a color-changing effect. This allows the color of the eyeglass frame coated with this material to change with the intensity of light, increasing its interest. At the same time, the addition of silver ions can improve the light fatigue resistance of the coating, and it can also fade quickly in an air-isolated environment.

[0017] Secondly, this invention uses copper powder as a raw material to spin a copper fiber film onto an eyeglass frame. Before spinning, the eyeglass frame is bombarded with an ion beam. The enormous energy transferred by the incident particles activates the surface atoms, causing lattice depressions to appear on the surface, allowing the copper fiber film to embed into the frame. This serves as the cathode of an electric field, with the anode connected to a nozzle, forming a high-voltage electrostatic field that ionizes the photosensitive resin, causing it to electrodeposit onto the frame surface, forming a continuous, uniform, and dense structure. Simultaneously, during the drying and curing of the photosensitive resin surface, moisture evaporation creates pores, which interact with the metal particles in the photosensitive resin. The particles form an uneven structure, increasing the surface roughness of the coating and giving it better hydrophobicity. This isolates water vapor from contacting the metal frame, giving the coating resistance to yellowing. Then, using an electrostatic field-assisted spraying method, an alumina precursor solution and silica sol are sprayed sequentially to form charged particles. These particles decompose in the gas phase and deposit on the surface of the photosensitive resin. The film is formed layer by layer. The presence of the layered structure increases the pathway for the diffusion of small molecules such as water and oxygen in the film layer, prolonging the penetration time of small molecules, thereby achieving a barrier effect and improving the coating's resistance to yellowing. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] To more clearly illustrate the method provided by the present invention, the following embodiments are provided in detail. The testing methods for various indicators of the ultrathin photosensitive resin coating prepared in the following embodiments are as follows: Photochromic properties: The same mass of the example and the comparative example were used to test the photochromic effect. After irradiating with 365nm ultraviolet light for 3 minutes, the color change was observed.

[0020] Photosensitive color-changing fatigue test: Take the same mass of the example and the comparative example to test the photosensitive color-changing fatigue effect. Irradiate with 365nm ultraviolet light continuously for 8 hours, with an interval of 10 hours, and cycle for 5 times. Observe whether there is color change.

[0021] Yellowing resistance: Take the same mass of the example and comparative examples to test the yellowing resistance effect. Place the sample in a pure oxygen environment with a relative humidity of 90% for 30 days and observe whether the surface turns yellow.

[0022] Example 1 A method for preparing an ultrathin photosensitive resin coating, the method comprising the following steps: (1) The eyeglass frame was washed with acetone and anhydrous ethanol for 11 min at 25 kHz to obtain a pretreated eyeglass frame; the pretreated eyeglass frame was placed in an ion thinning instrument with a bombardment energy of 1 keV and evacuated to 3.2 × 10⁻⁶ kHz. -3 Argon gas was introduced at 20 sccm, and the mixture was bombarded at 15° for 15 s under an argon atmosphere, followed by bombardment at 3° for 8 s. Polyethersulfone, N-methylpyrrolidone, and polyvinylpyrrolidone were mixed at a mass ratio of 1:4:0.2 and ground at 14 rpm for 9 h. Then, copper powder with a mass of 6 times that of polyethersulfone was added and ground at the same speed for 50 h. After vacuuming for 33 min, copper paste was obtained. The copper paste was used as the spinning solution and spun to a film thickness of 10 μm. After drying at 40°C for 10 h, the temperature was increased to 400°C at 2°C / min and held for 5 h under a hydrogen atmosphere. Then, the temperature was increased to 650°C at 1°C / min and held for 3 h. After cooling to 500°C at 4°C / min, the temperature was allowed to drop naturally to room temperature to obtain a copper fiber film eyeglass frame. During the spinning process, the spinneret size was 2 mm, the flow rate was 22 mL / min, and the air gap was 18 cm. (2) E-44 epoxy resin, ethylene glycol monobutyl ether and anhydrous ethanol are mixed in a mass ratio of 1:0.3:0.23. Under nitrogen protection, the mixture is heated to 60°C and stirred until dissolved. Then, 3-hydroxy-1-naphthylamine with a mass ratio of 0.4 times that of E-44 epoxy resin is added. After reacting for 12 minutes, an ethanol aqueous solution with a mass ratio of 0.6 times that of E-44 epoxy resin is added. The mass ratio of ethanol to water in the ethanol aqueous solution is 0.25:1. The mixture is allowed to stand for 18 minutes to obtain the photosensitive resin matrix. (3) Mix photosensitive resin matrix, sodium hydroxide, and deionized water at a mass ratio of 1:0.3:8, cool in a salt bath to -5℃, then add sodium nitrite at 0.4 times the mass of the photosensitive resin matrix. While stirring at 50 rpm, add sulfuric acid with a mass fraction of 42% at 2 times the mass of the photosensitive resin matrix. After reacting for 57 min, filter, wash with deionized water until the solution pH is 6, then add methanol at 21 times the mass of the photosensitive resin matrix. Under nitrogen protection, heat to 66℃, then add the photosensitive resin matrix... 5-chloro-1,3,3-trimethyl-2-methyleneindoline (0.6 times its bulk weight) was reacted for 8 hours, then concentrated at 200 rpm and 60 °C for 4 hours to obtain a spiroxazine compound. 3-aminophthalate, pyridine, and the spiroxazine compound were mixed at a mass ratio of 1:6:1, stirred at 100 rpm for 10 hours, concentrated at 80 °C under vacuum of 0.04 MPa for 2 hours, and then washed five times successively with ethyl acetate, distilled water, and saturated brine, and dried at 40 °C for 10 hours to obtain a modified resin. (4) Mix the modified resin and methanol at 4 times the mass of the modified resin. Add 0.7 times the mass of the modified resin and 25% ammonia water at 0.5 mL / min at 20°C. Stir at 50 rpm for 9 h. Then cool down to 0°C and keep warm for 0.5 h. Filter. Add 1.0 times the mass of the modified resin and 4 times the mass of the modified resin and tetrahydrofuran. Mix evenly. Cool down to -10°C. Add 1.2 times the mass of the modified resin and trifluoroacetic anhydride at 0.6 mL / min. Keep warm at -10°C for 58 min. Then heat up to 30°C and keep warm for 5 h. Distill at 50°C under vacuum of 0.04 MPa for 3 h. Add 2 times the mass of the modified resin and 3 times the mass of the modified resin and deionized water. Separate the contents and wash with distilled water 3 times. Distill at 60°C under vacuum of 0.05 MPa for 2 h to obtain the nitrile compound. (5) A nitrile compound, silver chloride, dimethylacetamide, and 1,8-diazabicyclo[5.4.0]undec-7-ene were mixed in a mass ratio of 1:0.3:5:0.001, microwaved at 180°C for 20 min, washed four times with deionized water, anhydrous ethanol, and acetone, centrifuged at 8000 rpm for 5 min, filtered, and dried at 60°C for 6 h to obtain a photosensitive resin raw material; the photosensitive resin raw material, diethylenetriamine, polydimethylsiloxane, n-butanol, and xylene were mixed in a mass ratio of 1:0.08:0.6:0.6 to obtain a photosensitive resin. (6) Using a copper fiber film eyeglass frame as the cathode and a nozzle as the anode, spray 0.3 times the weight of the copper fiber film eyeglass frame with photosensitive resin, cure at 30°C for 50 hours to obtain a base coating; (7) Aluminum nitrate, urea, and sodium chloride were mixed in a mass ratio of 1:8:3 to obtain an alumina precursor solution; the substrate coating was placed in an electrostatic field with an electric field voltage of 10kV and heated to 280℃. The alumina precursor solution was sprayed at a rate of 20mL / h, with a spraying distance of 30mm, a spraying time of 60s, an interval of 180s, and a total spraying time of 24min. After that, it was dried at 90℃ for 6h and placed in a tube furnace under a hydrogen atmosphere at 300℃ for 3h; tetraethyl orthosilicate, anhydrous ethanol, and other chemicals were added to the mixture. Ionized water and 58% nitric acid were mixed in a mass ratio of 1:1:0.2:0.02, heated to 50°C, and refluxed for 5 hours to obtain a tetraethyl orthosilicate mixture. Anhydrous ethanol, 17 times the volume of the tetraethyl orthosilicate mixture, was added to the tetraethyl orthosilicate mixture to obtain a silica sol. The silica sol was then placed in the same electrostatic field and sprayed at the same speed for 22 minutes. The temperature was then raised to 100°C, dried for 5 minutes, and then raised to 400°C and kept at that temperature for 5 hours to obtain an ultrathin photosensitive resin coating.

[0023] Example 2 A method for preparing an ultrathin photosensitive resin coating, the method comprising the following steps: (1) The eyeglass frame was washed with acetone and anhydrous ethanol for 8 min at 30 kHz to obtain a pretreated eyeglass frame; the pretreated eyeglass frame was placed in an ion thinning instrument with a bombardment energy of 3 keV and evacuated to 4.4 × 10⁻⁶. -3 Pa, argon gas is introduced at 25 sccm, and under argon atmosphere, it is bombarded at 19° for 21s, then at 6° for 12s; polyethersulfone, N-methylpyrrolidone and polyvinylpyrrolidone are mixed at a mass ratio of 1:4:0.3, and ground at 25 rpm for 6.5h, then copper powder with 8.5 times the mass of polyethersulfone is added, and ground at the same speed for 47h, then vacuumed for 46min to obtain copper paste; using copper paste as spinning solution, spinning is carried out to a film thickness of 230μm, dried at 45℃ for 7h, then heated to 500℃ at 3℃ / min under hydrogen atmosphere, held for 3.5h, then heated to 725℃ at 2℃ / min, held for 2h, then cooled to 500℃ at 6℃ / min, and then allowed to cool naturally to room temperature to obtain copper fiber film eyeglass frames; during the spinning process, the spinneret size is 3mm, the flow rate is 28mL / min, and the air gap is 24cm. (2) E-44 epoxy resin, ethylene glycol monobutyl ether and anhydrous ethanol were mixed in a mass ratio of 1:0.4:0.25. Under nitrogen protection, the mixture was heated to 68°C and stirred until dissolved. Then, 0.55 times the mass of E-44 epoxy resin and 3-hydroxy-1-naphthylamine were added. After reacting for 13.5 h, 1.35 times the mass of E-44 epoxy resin and an aqueous ethanol solution were added. The mass ratio of ethanol to water in the aqueous ethanol solution was 0.25:1. After standing for 26 min, the photosensitive resin matrix was obtained. (3) Mix photosensitive resin matrix, sodium hydroxide, and deionized water at a mass ratio of 1:0.45:11.5, cool in a salt bath to -2℃, then add sodium nitrite at 0.55 times the mass of the photosensitive resin matrix. While stirring at 70 rpm, add sulfuric acid with a mass fraction of 42% at 4 times the mass of the photosensitive resin matrix. After reacting for 64 min, filter, wash with deionized water until the solution pH is 6.5, then add methanol at 25.5 times the mass of the photosensitive resin matrix. Under nitrogen protection, heat to 73℃, then add photosensitive resin. 5-chloro-1,3,3-trimethyl-2-methyleneindoline (0.95 times the mass of the lipid matrix) was reacted for 11 h, and then concentrated at 250 rpm and 70 °C for 3 h to obtain a spiroxazine compound. 3-aminophthalate, pyridine, and the spiroxazine compound were mixed at a mass ratio of 1:10:1.5, stirred at 150 rpm for 8 h, concentrated at 0.06 MPa and 90 °C for 3 h, and then washed seven times successively with ethyl acetate, distilled water, and saturated brine, and dried at 50 °C for 7.5 h to obtain the modified resin. (4) Mix the modified resin and 7 times the mass of the modified resin with methanol. Add 1.05 times the mass of the modified resin with 26% ammonia water at 1.0 mL / min at 25°C. Stir at 70 rpm for 7.5 h. Then cool down to 2°C and keep warm for 1 h. Filter. Add 1.55 times the mass of the modified resin with triethylamine and 6 times the mass of the modified resin with tetrahydrofuran. Mix evenly. Cool down to -5°C. Add 1.9 times the mass of the modified resin with trifluoroacetic anhydride at 0.9 mL / min. Keep warm at -5°C for 64 min. Then heat up to 35°C and keep warm for 3.5 h. Distill at 58°C under vacuum of 0.06 MPa for 4.5 h. Add 3 times the mass of the modified resin with deionized water and 4.5 times the mass of the modified resin with ethyl acetate. Separate the mixture and wash with distilled water 5 times. Distill at 66°C under vacuum of 0.08 MPa for 3 h to obtain the nitrile compound. (5) A nitrile compound, silver chloride, dimethylacetamide, and 1,8-diazabicyclo[5.4.0]undec-7-ene were mixed in a mass ratio of 1:0.45:7:0.001, microwaved at 245°C for 14 min, washed 7 times with deionized water, anhydrous ethanol, and acetone, centrifuged at 9000 rpm for 3 min, filtered, and dried at 67°C for 4 h to obtain a photosensitive resin raw material; the photosensitive resin raw material, diethylenetriamine, polydimethylsiloxane, n-butanol, and xylene were mixed in a mass ratio of 1:0.15:0.75:0.75 to obtain a photosensitive resin. (6) Using a copper fiber film eyeglass frame as the cathode and a nozzle as the anode, spray 0.5 times the weight of the copper fiber film eyeglass frame with photosensitive resin, cure at 40°C for 45 hours to obtain a base coating; (7) Aluminum nitrate, urea and sodium chloride were mixed in a mass ratio of 1:10.5:5 to obtain an alumina precursor solution; the substrate coating was placed in an electrostatic field with an electric field voltage of 20kV and heated to 305℃. The alumina precursor solution was sprayed at a rate of 25mL / h, with a spraying distance of 35mm, a spraying time of 90s, an interval of 180s, and a total spraying time of 18min. After that, it was dried at 105℃ for 5h and placed in a tube furnace under a hydrogen atmosphere at 330℃ for 2h; tetraethyl orthosilicate, anhydrous ethanol, and deionized... Acid and nitric acid with a mass fraction of 58% were mixed in a mass ratio of 1:1.5:0.6:0.035, heated to 55°C, and refluxed for 4 hours to obtain a tetraethyl orthosilicate mixture. Anhydrous ethanol with a volume of 18.5 times that of the tetraethyl orthosilicate mixture was added to the tetraethyl orthosilicate mixture to obtain a silica sol. The silica sol was then placed in the same electrostatic field and sprayed at the same speed for 16 minutes. The temperature was then raised to 115°C, dried for 3 minutes, and then raised to 425°C and kept at that temperature for 3.5 hours to obtain an ultrathin photosensitive resin coating.

[0024] Example 3 A method for preparing an ultrathin photosensitive resin coating, the method comprising the following steps: (1) The eyeglass frame was washed with acetone and anhydrous ethanol for 5 min at 35 kHz to obtain a pretreated eyeglass frame; the pretreated eyeglass frame was placed in an ion thinning instrument with a bombardment energy of 6 keV and evacuated to 5.6 × 10⁻⁶ kHz. -3 Argon gas was introduced at 30 sccm, and the mixture was bombarded at 23° for 27 s under an argon atmosphere, followed by bombardment at 9° for 17 s. Polyethersulfone, N-methylpyrrolidone, and polyvinylpyrrolidone were mixed at a mass ratio of 1:4:0.4 and ground at 36 rpm for 4 h. Then, copper powder with a mass of 11 times that of polyethersulfone was added and ground at the same speed for 44 h. After vacuuming for 59 min, copper paste was obtained. Using the copper paste as a spinning solution, the film was spun to a thickness of 30 μm. After drying at 50°C for 4 h, the film was heated to 600°C at 5°C / min under a hydrogen atmosphere and held for 2 h. Then, the film was heated to 800°C at 3°C / min and held for 1 h. After cooling to 500°C at 9°C / min, the film was allowed to cool naturally to room temperature to obtain a copper fiber film eyeglass frame. During the spinning process, the spinneret size was 3 mm, the flow rate was 34 mL / min, and the air gap was 30 cm. (2) E-44 epoxy resin, ethylene glycol monobutyl ether and anhydrous ethanol were mixed in a mass ratio of 1:0.5:0.3. Under nitrogen protection, the mixture was heated to 75°C and stirred until dissolved. Then, 0.7 times the mass of E-44 epoxy resin and 3-hydroxy-1-naphthylamine were added. After reacting for 15 hours, 2.1 times the mass of E-44 epoxy resin and an aqueous ethanol solution were added. The mass ratio of ethanol to water in the aqueous ethanol solution was 0.25:1. After standing for 34 minutes, the photosensitive resin matrix was obtained. (3) Mix photosensitive resin matrix, sodium hydroxide, and deionized water at a mass ratio of 1:0.6:15, cool to 0°C in a salt bath, then add sodium nitrite at a mass ratio of 0.7 times that of the photosensitive resin matrix. While stirring at 100 rpm, add sulfuric acid at a mass fraction of 42% at a mass ratio of 6 times that of the photosensitive resin matrix. After reacting for 71 min, filter, wash with deionized water until the solution pH reaches 7, then add methanol at a mass ratio of 30 times that of the photosensitive resin matrix. Under nitrogen protection, heat to 80°C, then add the photosensitive resin matrix... 5-Chloro-1,3,3-trimethyl-2-methyleneindoline (1.3 times its bulk weight) was reacted for 14 h, then concentrated at 300 rpm and 80 °C for 2 h to obtain a spiroxazine compound. 3-aminophthalate, pyridine, and the spiroxazine compound were mixed at a mass ratio of 1:14:2, stirred at 200 rpm for 6 h, concentrated at 100 °C under vacuum of 0.08 MPa for 5 h, and then washed 10 times successively with ethyl acetate, distilled water, and saturated brine, and dried at 60 °C for 5 h to obtain a modified resin. (4) Mix the modified resin and 10 times the mass of the modified resin with methanol. Add 1.4 times the mass of the modified resin with 28% ammonia water at 1.5 mL / min at 30°C. Stir at 100 rpm for 6 h. Then cool down to 5°C and keep warm for 1.5 h. Filter. Add 2.1 times the mass of the modified resin with triethylamine and 8 times the mass of the modified resin with tetrahydrofuran. Mix evenly. Cool down to 0°C. Add 2.6 times the mass of the modified resin with trifluoroacetic anhydride at 1.2 mL / min. Keep warm at 0°C for 71 min. Then heat up to 40°C and keep warm for 2 h. Distill at 65°C under vacuum of 0.08 MPa for 6 h. Add 4 times the mass of the modified resin with deionized water and 6 times the mass of the modified resin with ethyl acetate. Separate the contents and wash with distilled water 7 times. Distill at 71°C under vacuum of 0.1 MPa for 4 h to obtain the nitrile compound. (5) A nitrile compound, silver chloride, dimethylacetamide, and 1,8-diazabicyclo[5.4.0]undec-7-ene were mixed in a mass ratio of 1:0.6:9:0.001, microwaved at 310°C for 8 min, washed 10 times with deionized water, anhydrous ethanol, and acetone, centrifuged at 10000 rpm for 1 min, filtered, and dried at 73°C for 2 h to obtain a photosensitive resin raw material; the photosensitive resin raw material, diethylenetriamine, polydimethylsiloxane, n-butanol, and xylene were mixed in a mass ratio of 1:0.22:0.9:0.9 to obtain a photosensitive resin. (6) Using a copper fiber film eyeglass frame as the cathode and a nozzle as the anode, spray 0.7 times the weight of the copper fiber film eyeglass frame with photosensitive resin, cure at 50°C for 40 hours to obtain a base coating; (7) Aluminum nitrate, urea and sodium chloride were mixed in a mass ratio of 1:13:7 to obtain an alumina precursor solution; the substrate coating was placed in an electrostatic field with an electric field voltage of 30kV and heated to 330℃. The alumina precursor solution was sprayed at a rate of 30mL / h, with a spraying distance of 40mm, spraying for 120s, with an interval of 180s, for a total of 12min. After spraying, it was dried at 120℃ for 4h and placed in a tube furnace under a hydrogen atmosphere at 360℃ for 1h; tetraethyl orthosilicate and anhydrous ethanol were added. Deionized water and nitric acid with a mass fraction of 58% were mixed in a mass ratio of 1:2:1.0:0.05, heated to 60°C, and refluxed for 3 hours to obtain a tetraethyl orthosilicate mixture. Anhydrous ethanol with a volume of 20 times that of the tetraethyl orthosilicate mixture was added to the tetraethyl orthosilicate mixture to obtain a silica sol. The silica sol was then placed in the same electrostatic field and sprayed at the same speed for 10 minutes. The temperature was then raised to 130°C, dried for 2 minutes, and then raised to 450°C and kept at that temperature for 2 hours to obtain an ultrathin photosensitive resin coating.

[0025] Comparative Example 1 The only difference between Comparative Example 1 and Example 2 is step (2). Step (2) is changed to: E-44 epoxy resin, ethylene glycol monobutyl ether and anhydrous ethanol are mixed at a mass ratio of 1:0.4:0.25, heated to 68°C under nitrogen protection, and stirred until dissolved to obtain the photosensitive resin matrix. The remaining preparation steps are the same as in Example 2.

[0026] Comparative Example 2 The only difference between Comparative Example 2 and Example 2 is step (3). Step (3) is changed to: mixing 3-aminophthalate, pyridine, and photosensitive resin matrix in a mass ratio of 1:10:1.5, stirring at 150 rpm for 8 hours, concentrating under vacuum of 0.06 MPa and at 90°C for 3 hours, then washing with ethyl acetate, distilled water, and saturated brine seven times in sequence, and drying at 50°C for 7.5 hours to obtain the modified resin. The remaining preparation steps are the same as in Example 2.

[0027] Comparative Example 3 The difference between Comparative Example 3 and Example 2 is that steps (4) and (5) are omitted. Step (3) is changed to: mixing photosensitive resin matrix, sodium hydroxide, and deionized water in a mass ratio of 1:0.45:11.5, cooling to -2°C in a salt bath, adding sodium nitrite at 0.55 times the mass of the photosensitive resin matrix, adding sulfuric acid with a mass fraction of 42% at 4 times the mass of the photosensitive resin matrix while stirring at 70 rpm, reacting for 64 min, filtering, washing with deionized water until the solution pH is 6.5, then adding methanol at 25.5 times the mass of the photosensitive resin matrix, heating to 73°C under nitrogen protection, adding 5-chloro-1,3,3-trimethyl-2-methyleneindoline at 0.95 times the mass of the photosensitive resin matrix, reacting for 11 h, and then concentrating at 250 rpm and 70°C for 3 h to obtain the photosensitive resin. The remaining preparation steps are the same as in Example 2.

[0028] Comparative Example 4 The difference between Comparative Example 4 and Example 2 is that steps (1) and (6) are omitted, and step (7) is changed to: spraying photosensitive resin with 0.5 times the mass of the eyeglass frame onto the eyeglass frame to obtain a base coating; mixing aluminum nitrate, urea and sodium chloride in a mass ratio of 1:13:7 to obtain an alumina precursor solution; placing the base coating in an electrostatic field with an electric field voltage of 30kV, heating it to 330℃, spraying the alumina precursor solution at 30mL / h, with a spraying distance of 40mm, spraying for 120s, with an interval of 180s, spraying for a total of 12min, drying at 120℃ for 4h, and placing it in a tube furnace. In a hydrogen atmosphere, the reaction was carried out at 360°C for 1 hour. Tetraethyl orthosilicate, anhydrous ethanol, deionized water, and 58% nitric acid were mixed in a mass ratio of 1:2:1.0:0.05, heated to 60°C, and refluxed for 3 hours to obtain a tetraethyl orthosilicate mixture. Anhydrous ethanol, 20 times the volume of the tetraethyl orthosilicate mixture, was added to the mixture to obtain a silica sol. This sol was then placed in the same electrostatic field and sprayed at the same speed for 10 minutes. The temperature was then raised to 130°C, dried for 2 minutes, and then raised to 450°C and held for 2 hours to obtain an ultrathin photosensitive resin coating. The remaining preparation steps were the same as in Example 2.

[0029] Comparative Example 5 The difference between Comparative Example 5 and Example 2 lies in step (1). Step (1) is changed to: washing the eyeglass frame with acetone and anhydrous ethanol sequentially for 8 minutes at 30 kHz to obtain a pretreated eyeglass frame; mixing polyethersulfone, N-methylpyrrolidone and polyvinylpyrrolidone in a mass ratio of 1:4:0.3, grinding at 25 rpm for 6.5 hours, adding copper powder at 8.5 times the mass of polyethersulfone, grinding at the same speed for 47 hours, and then vacuuming for 46 minutes to obtain copper slurry. Using copper paste as the spinning solution, the film thickness was spun to 230 μm. After drying at 45°C for 7 hours, the film was heated to 500°C at a rate of 3°C / min under a hydrogen atmosphere and held for 3.5 hours. Then, the temperature was increased to 725°C at a rate of 2°C / min and held for 2 hours. Finally, the temperature was lowered to 500°C at a rate of 6°C / min and allowed to cool naturally to room temperature to obtain a copper fiber film eyeglass frame. During the spinning process, the spinneret size was 3 mm, the flow rate was 28 mL / min, and the air gap was 24 cm. The remaining preparation steps were the same as in Example 2.

[0030] Comparative Example 6 The only difference between Comparative Example 6 and Example 2 is that step (7) is omitted; the other preparation steps are the same as in Example 2.

[0031] Example of effect Table 1 below presents the performance analysis results of the ultrathin photosensitive resin coatings of Examples 1 to 3 and Comparative Examples 1 to 6 of the present invention.

[0032] Table 1 Color change under ultraviolet light Color change under prolonged ultraviolet light exposure Yellowing Example 1 Color change Color change No yellowing Example 2 Color change Color change No yellowing Example 3 Color change Color change No yellowing Comparative Example 1 No change No change No yellowing Comparative Example 2 No change No change No yellowing Comparative Example 3 No change No change Slightly yellowing Comparative Example 4 Color change Color change Turn yellow Comparative Example 5 Color change Color change Turn yellow Comparative Example 6 Color change Color change Turn yellow A comparison of experimental data on color change under ultraviolet light and over long periods of time in the examples and comparative examples reveals that this product utilizes 3-hydroxy-1-naphthylamine and 5-chloro-1,3,3-trimethyl-2-methyleneindoline to modify epoxy resin, introducing spiroxazine groups into the epoxy resin molecular chain. This imbues the coating with photosensitivity. Furthermore, the polyhydroxyl nature of the epoxy resin enhances the polarity of the spiroxazine groups, increasing rigidity and extending the coating's resistance to light fatigue. Further modification with 3-aminophthalate and coordination with silver chloride leads to intermolecular transitions under light induction, generating colored free radicals that promote the oxidation and valence change of silver ions, achieving the color-changing effect. Simultaneously, the addition of silver ions... The addition of ion beams can improve the light fatigue resistance of the coating. A comparison of the yellowing experimental data of the examples and comparative examples shows that the product first bombards and roughens the eyeglass frame with ion beams, which is beneficial for the copper fiber film to be embedded in the surface during the spinning process. This allows it to act as an electrode cathode. Using the electric field effect, photosensitive resin is electrodeposited on the surface of the eyeglass frame, filling the depressions and forming a tight bond. During curing, the pores left by the evaporation of moisture and the metal ions form a rough surface, making the coating hydrophobic and able to isolate moisture. Then, using an electrostatic field-assisted spraying method, aluminum oxide and silicon dioxide films are grown layer by layer on the surface to block the penetration of moisture and oxygen, effectively isolating water and oxygen and improving the yellowing resistance of the coating.

[0033] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.

Claims

1. An ultrathin photosensitive resin coating, characterized in that, The ultrathin photosensitive resin coating is prepared by the following method: using ion beam-assisted spinning on an eyeglass frame to obtain a copper fiber film eyeglass frame; then using the copper fiber film eyeglass frame as the cathode and a nozzle as the anode, photosensitive resin is sprayed to obtain a substrate coating; and then electrostatic field-assisted spraying is used to obtain a water and oxygen barrier layer. The preparation method of the ultrathin photosensitive resin coating includes the following preparation steps: The photosensitive resin is prepared as follows: The eyeglass frame is washed sequentially with acetone and anhydrous ethanol for 8 minutes at 30 kHz to obtain a pretreated eyeglass frame; the pretreated eyeglass frame is then placed in an ion thinning apparatus with a bombardment energy of 3 keV and evacuated to a vacuum of 4.4 × 10⁻⁶. -3 Pa, argon gas is introduced at 25 sccm, and under argon atmosphere, it is bombarded at 19° for 21s, then at 6° for 12s; polyethersulfone, N-methylpyrrolidone and polyvinylpyrrolidone are mixed at a mass ratio of 1:4:0.3, and ground at 25 rpm for 6.5h, then copper powder with 8.5 times the mass of polyethersulfone is added, and ground at the same speed for 47h, then vacuumed for 46min to obtain copper paste; using copper paste as spinning solution, spinning is carried out to a film thickness of 230μm, dried at 45℃ for 7h, then heated to 500℃ at 3℃ / min under hydrogen atmosphere, held for 3.5h, then heated to 725℃ at 2℃ / min, held for 2h, then cooled to 500℃ at 6℃ / min, and then allowed to cool naturally to room temperature to obtain copper fiber film eyeglass frames; during the spinning process, the spinneret size is 3mm, the flow rate is 28mL / min, and the air gap is 24cm. E-44 epoxy resin, ethylene glycol monobutyl ether, and anhydrous ethanol were mixed in a mass ratio of 1:0.4:0.

25. Under nitrogen protection, the mixture was heated to 68°C and stirred until dissolved. Then, 0.55 times the mass of E-44 epoxy resin and 3-hydroxy-1-naphthylamine were added. After reacting for 13.5 hours, 1.35 times the mass of E-44 epoxy resin and an aqueous ethanol solution were added. The mass ratio of ethanol to water in the aqueous ethanol solution was 0.25:

1. After standing for 26 minutes, the photosensitive resin matrix was obtained. A mixture of photosensitive resin matrix, sodium hydroxide, and deionized water at a mass ratio of 1:0.45:11.5 was prepared and cooled to -2°C in a salt bath. Then, sodium nitrite (0.55 times the mass of the photosensitive resin matrix) was added. While stirring at 70 rpm, 42% sulfuric acid (4 times the mass of the photosensitive resin matrix) was added. After reacting for 64 minutes, the mixture was filtered and washed with deionized water until the pH reached 6.

5. Then, methanol (25.5 times the mass of the photosensitive resin matrix) was added. Under nitrogen protection, the mixture was heated to 73°C, and then the photosensitive resin was added. 5-chloro-1,3,3-trimethyl-2-methyleneindoline (0.95 times the matrix mass) was reacted for 11 h, then concentrated at 250 rpm and 70 °C for 3 h to obtain a spiroxazine compound. 3-aminophthalate, pyridine, and the spiroxazine compound were mixed at a mass ratio of 1:10:1.5, stirred at 150 rpm for 8 h, concentrated at 90 °C under vacuum of 0.06 MPa for 3 h, and then washed seven times successively with ethyl acetate, distilled water, and saturated brine, and dried at 50 °C for 7.5 h to obtain the modified resin. The modified resin and 7 times its mass of methanol were mixed. At 25°C, 1.05 times its mass of 26% ammonia (by mass) was added at a rate of 1.0 mL / min. The mixture was stirred at 70 rpm for 7.5 h, then cooled to 2°C and kept at that temperature for 1 h. After filtration, 1.55 times its mass of triethylamine and 6 times its mass of tetrahydrofuran were added. After mixing thoroughly, the mixture was cooled to -5°C. 1.9 times its mass of trifluoroacetic anhydride (by mass of trifluoroacetic anhydride) was added at a rate of 0.9 mL / min. The mixture was kept at -5°C for 64 min, then heated to 35°C and kept at that temperature for 3.5 h. The mixture was then distilled at 58°C under a vacuum of 0.06 MPa for 4.5 h. 3 times its mass of deionized water and 4.5 times its mass of ethyl acetate were added. The mixture was separated, washed 5 times with distilled water, and then distilled at 66°C under a vacuum of 0.08 MPa for 3 h to obtain the nitrile compound. A nitrile compound, silver chloride, dimethylacetamide, and 1,8-diazabicyclo[5.4.0]undec-7-ene were mixed in a mass ratio of 1:0.45:7:0.001, microwaved at 245°C for 14 min, washed seven times sequentially with deionized water, anhydrous ethanol, and acetone, centrifuged at 9000 rpm for 3 min, filtered, and dried at 67°C for 4 h to obtain a photosensitive resin precursor. The photosensitive resin precursor, diethylenetriamine, polydimethylsiloxane, n-butanol, and xylene were mixed in a mass ratio of 1:0.15:0.75:0.75 to obtain the photosensitive resin. Using a copper fiber film eyeglass frame as the cathode and a nozzle as the anode, a photosensitive resin of 0.5 times the weight of the copper fiber film eyeglass frame is sprayed and cured at 40°C for 45 hours to obtain a base coating. Aluminum nitrate, urea, and sodium chloride were mixed in a mass ratio of 1:10.5:5 to obtain an alumina precursor solution. The substrate coating was placed in an electrostatic field with an electric field voltage of 20kV and heated to 305℃. An alumina precursor solution was sprayed at a rate of 25mL / h, with a spraying distance of 35mm, a spraying time of 90s followed by a 180s interval, for a total spraying time of 18min. Afterward, it was dried at 105℃ for 5h and then placed in a tube furnace under a hydrogen atmosphere at 330℃ for 2h. Tetraethyl orthosilicate, anhydrous ethanol, deionized water, and 58% nitric acid were mixed in a mass ratio of 1: Mix 1.5:0.6:0.035, heat to 55℃, and reflux for 4 hours to obtain a tetraethyl orthosilicate mixture; add 18.5 times the volume of anhydrous ethanol to the tetraethyl orthosilicate mixture to obtain a silica sol, then place it in the same electrostatic field and spray the silica sol at the same speed for 16 minutes, raise the temperature to 115℃, dry for 3 minutes, then raise the temperature to 425℃ and keep it at that temperature for 3.5 hours to obtain an ultrathin photosensitive resin coating.

Citation Information

Patent Citations

  • Photochromic spectacle frame processing method, photochromic spectacle frame and spectacles