Continuous self-supporting electrostatic spinning nanofiber membrane preparation method

By regulating the electrospinning, drying and peeling units, combined with the conveying device, the continuous preparation of self-supported nanofiber membranes is achieved, solving the problems of low degree of automation and high production costs in the prior art, and improving production efficiency and yield.

CN120119402APending Publication Date: 2025-06-10INST OF URBAN ENVIRONMENT CHINESE ACAD OF SCI

Patent Information

Application Number
CN202510559143.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-30
Publication Date
2025-06-10

AI Technical Summary

Technical Problem

The existing flexible self-supported nanofiber membrane preparation technology has low degree of automation, and cannot be continuously produced. The post-processing steps are cumbersome, resulting in increased production costs and decreased yield.

Method used

By controlling the fine regulation of the receiving substrate electrospinning unit, the drying unit and the peeling winding unit, the coupling of the conveying device and multiple units is adopted to achieve continuous preparation of self-supported nanofiber membranes.

Benefits of technology

The single-step process is achieved to produce self-supported nanofiber membranes with excellent mechanical properties, which simplifies the production process, improves production efficiency, reduces production costs, and improves yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120119402A_ABST
    Figure CN120119402A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a continuous self-supporting electrostatic spinning nanofiber membrane, which is characterized by comprising the following steps: S1, preparing a polymer and the like into a to-be-spun solution, and putting the to-be-spun solution into a liquid pushing system; s2, the base material is arranged on a conveying device, and nanofibers are received; s3, adjusting the voltage and the rotating speed of the transmission device to a proper interval; s4, the drying unit starts to dry and remove the solvent of the base material and the nanofiber membrane; and S5, after passing through the stripping unit, the fiber membranes are collected by the winding unit. According to the method, the function of processing the composite nanofiber membrane material is realized by utilizing a set of technological process, and synchronous stripping of the nanofiber membrane and the base material is completed; and meanwhile, the recycled base material can be repeatedly used, so that the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical fields of nanofibers and textile machinery, and particularly relates to a method for preparing a continuous self-supporting electrospun nanofiber membrane. Background Art

[0002] With the progress of technology and the development of nanotechnology, nanofibers, as a new type of nanomaterial, have broad application potential in the fields of environmental protection, biomedicine, energy, etc. Compared with micron-scale fibers, nanofibers have a larger specific surface area, higher porosity, and are easier to be surface-functionalized, showing more excellent interfacial effects and application values. Among various processes for preparing nanofibers, electrospinning is a technique that uses high voltage to eject polymer solutions or melts into fibers. Under the action of an electric field, the polymer solution is ejected from the spinneret to form fine filaments, and the solvent evaporates during flight, finally forming nanofibers.

[0003] However, at present, most flexible nanofiber membranes need a substrate or backing to support the above nanofiber membranes. However, the presence of the substrate material usually affects the overall performance of the nanofiber membrane material. For example, in the field of electronic sensing, the substrate material increases the elastic modulus of the overall sensor to several hundred megapascals (MPa), far exceeding the level of most soft tissues in the body (in the range of KPa - MPa), resulting in a serious mechanical mismatch between the electronic sensor and body tissues; in the field of indoor ventilation, a transparent nanofiber window screen with a substrate material may reduce the light transmittance of the fiber membrane, affecting the indoor brightness. Therefore, there is an urgent need to develop innovative processes to develop flexible self-supporting nanofiber membranes.

[0004] Self-supporting flexible nanofiber membranes refer to nanofiber membranes that can exist independently without the support of a substrate, and have good flexibility and mechanical strength. At present, some researchers have prepared self-supporting nanofiber membranes by adjusting the process parameters of electrospinning (such as voltage, receiving distance, solution concentration, etc.) and combining different polymer types. Patent No. CN114858877 A discloses a super-soft self-supporting nano-network electrode and its preparation method and application, which improves the conductivity and cell compatibility of the material while ensuring the self-supporting performance of the nanofiber electrode material; CN 116288925 A discloses a self-supporting nanofiber membrane and its preparation method and application, and a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure is obtained by using the sacrificial template method, reducing the production cost and the complexity of subsequent application processing technology. CN118166479 A discloses a preparation method of a flexible self-supporting transparent porous micro-nanofiber membrane, and a flexible self-supporting transparent porous micro-nanofiber membrane is prepared by pressing a mold along the direction perpendicular to the surface of the micro-nanofiber membrane for a certain time, and the light transmittance reaches more than 70%. CN202210495678.6 discloses a self-supporting nanofiber anti-haze window screen and its preparation method, which is formed by thermocompression lamination of a self-supporting nanofiber filter layer and a support layer. However, this method cannot continuously produce nanofiber membranes, and manual stripping and thermocompression of the fiber membrane are required during the process, which is not suitable for large-scale production.

[0005] In summary, many studies on flexible self-supporting nanofiber membranes and their preparation methods have been carried out. However, the preparation of flexible self-supporting nanofiber membranes poses higher requirements for electrospinning equipment and auxiliary equipment. However, the existing equipment has a low degree of automation and cannot continuously prepare self-supporting nanofiber membranes in the same process; at the same time, the post-treatment steps are cumbersome, time-consuming and laborious, and the production cost will increase by 35-50%; in addition, the use of manual stripping and winding in the existing technology will cause the yield of self-supporting nanofiber membranes to decrease by more than 20%, and frequent shutdowns will also cause 70% of the needles to become blocked, and the annual loss of production capacity at the million-square-meter level is > 3 million yuan. Therefore, this patent discloses a preparation method for improving the mechanical strength and flexibility of nanofiber membranes, thereby promoting the industrialization and application development of self-supporting nanofiber membranes. Summary of the Invention

[0006] The purpose of the present invention is to provide a preparation method of a self-supporting flexible electrospun nanofiber membrane in view of the deficiencies of flexible self-supporting nanofiber membrane materials and their preparation technologies. Using the present invention, a self-supporting nanofiber membrane material with excellent mechanical properties and flexibility can be obtained, and the preparation technology is simple, controllable, has good stability and a high yield.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A preparation method of a self - supporting electrospun nanofiber membrane, which finely regulates the electrospinning unit, drying unit and peeling and winding unit of the receiving substrate, then dries the substrate and the nanofiber membrane, and finally peels to obtain the self - supporting nanofiber membrane. It includes a conveying device, an electrospinning unit, a drying unit, a peeling unit and a winding unit arranged around the conveying device, and the steps are as follows: S1: Prepare a spinning solution by mixing a polymer, a solvent and an additive, and place the solution in the liquid - pushing system in the electrospinning unit; S2: Select a suitable substrate and place it on the conveying device to receive the nanofibers produced by electrospinning; S3: Turn on the power supplies of the high - voltage system, the conveying device and the liquid - pushing system. Connect the positive high - voltage system to the spinning needle, and connect the negative high - voltage system to the conveying device and the substrate. The electrospinning unit sprays the spinning solution onto the substrate to obtain the electrospun nanofiber membrane with the substrate; S4: The electrospun nanofiber membrane with the substrate is conveyed to the drying unit, and the drying unit starts to dry and remove the solvent of the substrate and the nanofiber membrane; S5: After passing through the peeling unit, the substrate and the nanofiber membrane are respectively collected by their own winding units to obtain a separated self - supporting electrospun nanofiber membrane and the substrate.

[0008] In a preferred embodiment, there are several nozzles at the top of the electrospinning unit, and the continuous movement of the conveying device matches the rate of the nozzles. When the liquid - pushing rate of the nozzles is greater than 2.5 ml / h, the movement speed of the conveyor belt is greater than 15 cm / s.

[0009] In a preferred embodiment, when the liquid - pushing rate of the nozzles is 0.2 ml / h - 1 ml / h, the rotation speed of the conveying device is 5 - 30 cm / s.

[0010] In a preferred embodiment, when a low - conductivity substrate (resistivity greater than 10 -8 Ω·m) is selected, the positive voltage range is 15 kV - 60 kV, the negative voltage range is - 15 - 0 kV, and the rotation speed range of the conveyor belt is 1 cm / s - 30 cm / s.

[0011] In a preferred embodiment, when a high - conductivity substrate (resistivity less than 10 -8 Ω·m) is selected, the positive voltage range is 15 kV - 30 kV, the negative voltage range is - 5 - 0 kV, and the rotation speed range of the conveyor belt is 5 cm / s - 100 cm / s.

[0012] In a preferred embodiment, the drying unit is located on one side of the substrate conveyor belt. When a low-conductivity substrate is selected, the drying temperature is 60 - 80 °C, and the air-blowing speed is 5 - 100 cm / s; when a high-conductivity substrate is selected, the drying temperature is 40 - 60 °C, and the air-blowing speed is 0 - 40 cm / s; when a patterned substrate is selected, the drying temperature is 40 - 80 °C, and the air-blowing speed is 0 - 200 cm / s.

[0013] In a preferred embodiment, the drying unit is a batch-type heat pump blower unit.

[0014] In a preferred embodiment, the peeling unit is a columnar metal with an adjustable diameter, and its cross-section is an arc cone. The transition between the arc and the cone is treated with a rounded corner. The radius range of the arc is 2 - 8 cm, and the side length range is 4 - 14 cm.

[0015] In a preferred embodiment, the diameter of the drum of the winding unit is adjustable, and the adjustable range is 3 cm - 20 cm.

[0016] In a preferred embodiment, the mass ratio of the polymer, solvent, and additive in step S1 is (5 - 20):(75 - 95):(0.5 - 5).

[0017] The nanofiber membrane with good mechanical properties and flexibility prepared by the present invention is produced by an electrospinning process. The diameter range of the fibers is between 50 nm and 1000 nm, and the thickness range of the fiber layer is between 5 μm and 400 μm.

[0018] In addition, the flexible self-supporting electrospun nanofiber membrane of the present invention can be applied to a variety of application scenarios, such as air filtration, biomedicine, oil-water separation, and electronic sensing. For example: (1) Transparent anti-haze window screen: Fix the flexible self-supporting electrospun nanofiber membrane with a magnetic frame and cut it into the required window screen grid size for installation; (2) Aerosol protective clothing: Cut the flexible self-supporting electrospun nanofiber membrane with a slicing machine and then thermally fuse it with the fabric layer using a hot press. The inert gas is nitrogen, the thermal fusion temperature is 120 - 170 °C, and the thermal fusion time is 60 - 150 s; (3) Medical dressing: Immerse the flexible self-supporting electrospun nanofiber membrane in a solution containing an anti-inflammatory component. The solvent is one or both of water and ethanol, the soaking time is 3 - 12 h, and then it is dried at room temperature for 3 - 5 days.

[0019] The above technical solutions have the following beneficial effects: The present invention relates to a method for preparing a self - supporting flexible electrospun nanofiber membrane, providing a one - step method for producing a self - supporting nanofiber membrane with excellent mechanical properties, simplifying the production process and improving production efficiency. At the same time, in the present invention, by adjusting the speeds of the conveyor belt and the roller and selecting different substrates and spinning solution systems, the thickness and structure of the nanofiber membrane can be flexibly adjusted to meet different performance requirements, and it is applicable to a variety of application scenarios, such as air filtration, biomedicine, oil - water separation, and electronic sensing. Further, the present invention can achieve synchronous deposition and peeling in the same production process, further simplifying the production process and meeting the requirements of batch preparation. In addition, the substrate in the present invention can be re - wound for reuse, significantly reducing the production cost and improving the economy. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic flow chart of the method for preparing the self - supporting flexible electrospun nanofiber membrane.

[0021] Figure 2 It is a cross - sectional view of the peeling device.

[0022] Figure 3 It is a physical map and a microscopic morphology map of the self - supporting flexible electrospun nanofiber membrane prepared by the present invention (corresponding to specific embodiment 1).

[0023] Figure 4 It is a morphology map of the self - supporting flexible electrospun nanofiber membrane prepared by the present invention (corresponding to specific embodiment 2).

[0024] Figure 5 It is a mechanical property map of the self - supporting flexible electrospun nanofiber membrane prepared by the present invention (corresponding to specific embodiment 3). DETAILED DESCRIPTION OF THE EMBODIMENTS

[0025] In order to make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be elaborated in detail below in conjunction with the drawings and preferred embodiments.

[0026] A continuous method for preparing a self - supporting electrospun nanofiber membrane includes a conveying device, a suitable substrate is disposed on the substrate conveyor belt for receiving the nanofibers generated by electrospinning, and an electrospinning unit, a drying unit, a peeling unit, and a winding unit are disposed around the conveying device.

[0027] There are several nozzles at the top of the electrospinning unit. The movement trajectory of the nozzles is fixed to ensure that the nanofiber material is evenly sprayed onto the conveyor belt. The continuous movement of the conveying device matches the rate of the nozzles. When the liquid pushing rate of the nozzles is greater than 2.5 ml / h, the movement speed of the conveyor belt should be greater than 15 cm / s. Otherwise, there will be a rate mismatch, resulting in damage to the fiber membrane due to mechanical strength problems when the subsequent fiber membrane passes through the peeling device, reducing the yield rate of the fiber membrane.

[0028] Turn on the high-voltage system. The positive high-voltage system is connected to the spinning needle, and the negative high-voltage system is connected to the conveying device and the substrate. When a low-conductivity substrate (resistivity greater than 10 -8 Ω·m) is selected, the positive voltage range is 15 kV - 60 kV, the negative voltage range is -15 - 0 kV, and the conveyor belt rotation speed range is 1 cm / s - 30 cm / s; when a high-conductivity substrate (resistivity less than 10 -8 Ω·m) is selected, the positive voltage range is 15 kV - 30 kV, the negative voltage range is -5 - 0 kV, the conveyor belt rotation speed range is 5 cm / s - 100 cm / s, and the conveyor belt width range is between 20 cm - 200 cm.

[0029] The substrate after passing through the electrospinning unit is conveyed to the drying unit 3. The drying unit is located on one side of the conveying device. The self-supporting electrospun nanofiber membrane with the substrate is conveyed to the drying unit, and the drying unit starts to dry and remove the solvent of the substrate and the nanofiber membrane; when the nanofiber material passes through the zone-controlled drying area on the conveying device, it is cured by precisely controlling the temperature and time to ensure that the material is properly processed at this stage.

[0030] The drying unit is a hot air drying system. The type of the drying system is, for example, a batch-type heat pump blower unit, and the distance from the conveyor belt is 20 - 60 cm. When a low-conductivity substrate is selected, the drying temperature is 60 - 80 °C, and the air blowing speed is 5 - 100 cm / s; when a high-conductivity substrate is selected, the drying temperature is 40 - 60 °C, and the air blowing speed is 0 - 40 cm / s; when a patterned substrate is selected, the drying temperature is 40 - 80 °C, and the air blowing speed is 0 - 200 cm / s.

[0031] After that, the self-supporting electrospun nanofiber membrane with the substrate after drying is transported to the peeling unit and then collected by their respective winding units, obtaining a separated self-supporting electrospun nanofiber membrane and the substrate. The peeling unit and the winding unit are used to sort out the dried nanofiber material and the substrate, ensuring that the materials are collected or further processed in the required form. The peeling unit is a columnar metal with adjustable diameter, and its cross-section is an arc cone. The arc and the cone are rounded. The radius range of the arc is 2 - 8 cm, and the side length range is 4 - 14 cm. This design can effectively separate the substrate from the nanofibers, and at the same time avoid the damage of the metal to the nanofibers and the substrate, enabling the peeled substrate to be reused, further reducing the cost. The diameter of the roller of the winding unit is adjustable, and the adjustable range is 3 cm - 20 cm.

[0032] Furthermore, with the drying unit as the regional center, the distance ratios between the drying unit and the electrospinning unit, and between the drying unit and the peeling unit are set to 0.6 - 1.2. By regulating the regional distribution among the various module units of the system, the spinning solution is evenly sprayed onto the substrate and then transported through the conveying device, and then enters the drying unit for sufficient drying. In this way, through the fine regulation of various steps such as the rates of electrospinning, the drying unit, and the conveying device, the nanofiber membrane can be fully dried, ensuring the mechanical strength of the nanofiber membrane, thus ensuring the subsequent mechanical peeling of the nanofiber membrane, and maintaining the yield of the self-supporting nanofiber membrane above 80%.

[0033] The specific steps of the present invention are as follows: S1: Prepare a spinning solution by mixing a polymer, a solvent, and an additive, and place the solution in the liquid pushing system of the electrospinning unit. Among them, the mass ratio of the polymer, the solvent, and the additive is (5 - 20):(75 - 95):(0.5 - 5); the types of the polymer can be one or more of polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polycaprolactone (PCL), polylactic acid (PLA), polystyrene (PS), polyurethane (TPU), polyvinylidene fluoride (PVDF), polyamide (PA), chitosan (CS), silk fibroin (SF), cellulose and its derivatives, sodium alginate (Alginate), etc. The additive can be one or more of components such as a surface-active spinning aid, an inorganic salt, and a functional additive; S2: Select a suitable substrate and lay it on the conveying device for receiving the nanofibers generated by electrospinning; among them, the substrate can be a conductive substrate (resistivity is between 10 -6 -10 -8 Ω·m), such as copper foil, aluminum foil, and a non-conductive substrate (resistivity is greater than 10 6One of the 3D printing substrates with customized patterns of conductive and non-conductive phases, such as silicon oil paper, gauze, non-woven fabric, etc., and having a resistivity of 10³ - 10¹² Ω·m; S3: Turn on the power supplies of the high-voltage system, the conveying device, and the liquid-pushing system. Connect the positive high-voltage system to the spinning needle, and connect the negative high-voltage system to the conveying device and the substrate. The electrospinning unit sprays the liquid to be spun onto the substrate to obtain the self-supporting electrospun nanofiber membrane with the substrate. S4: Transfer the self-supporting electrospun nanofiber membrane with the substrate to the drying unit, and the drying unit starts to dry and remove the solvents of the substrate and the nanofiber membrane. S5: After passing through the peeling unit, the substrate and the nanofibers are respectively collected by their respective winding units to obtain a separated self-supporting electrospun nanofiber membrane and the substrate.

[0034] The present invention prepares a self-supporting nanofiber membrane by regulating the cooperation of the conveying device, the electrospinning device, and the drying unit, and prepares a self-supporting nanofiber membrane with excellent properties that meets different applications. At the same time, the prepared self-supporting nanofiber membrane can be peeled off by mechanical force and directly subjected to subsequent winding operations.

[0035] During the process of preparing nanofibers by electrospinning, the electric field distribution and surface morphology of the substrate for receiving nanofibers have a significant impact on the morphology and planar distribution of the nanofibers. When using a non-conductive substrate, its surface potential is higher; during the deposition of nanofibers onto the substrate, the residual charges on the fibers will rapidly accumulate on the non-conductive receiving device, making it more difficult for subsequent fibers to deposit on it, reducing the packing density of the nanofibers, and making it easier to obtain a self-supporting nanofiber membrane with a fluffy structure. A substrate with a high degree of conductivity can make the deposition of nanofibers more compact, increase the number of fibers per unit area, and improve the mechanical strength of the fiber membrane. On the other hand, when using a substrate with a large roughness for receiving, the number of contact points between the nanofibers and the substrate decreases, which is beneficial to the rapid peeling of the fiber membrane. When using a substrate with a small roughness for receiving, the flatness of the nanofibers is better. At the same time, with the development of material surface manufacturing processes such as 3D printing, electromagnetic sputtering, and laser etching, it has become possible to prepare flexible substrates with different roughnesses, conductivities, and surface patterns to control the electrospinning electric field and potential distribution. Therefore, by combining the substrate material, the flexibility and mechanical properties of the electrospun nanofiber membrane material can be improved by adjusting the types, concentrations, and electric field strengths of electrospinning polymers, etc., so as to obtain the self-supporting flexible electrospun nanofiber membrane. At the same time, by adopting a roll-to-roll production and winding method, combined with an auxiliary drying and peeling device, continuous preparation of fiber membranes can be realized, improving the production efficiency of nanofiber membranes in actual processes.

[0036] The present invention provides a preparation method for continuously producing a self-supporting nanofiber membrane with excellent mechanical properties in a single step, which simplifies the production process and improves production efficiency. The present invention can achieve synchronous deposition and peeling in the same production process, further simplifying the production process and meeting the requirements of batch preparation. In addition, the substrate in the present invention can be rewound for reuse, significantly reducing the production cost and improving the economy. The entire device can be combined with sensors and control systems to monitor parameters such as the spinning amount, conveying speed, and drying temperature in real time, and automated control ensures the stability and consistency of the production process. At the same time, in the present invention, by adjusting the speeds of each unit and selecting different substrates and spinning solution systems, the thickness and structure of the nanofiber membrane can be flexibly adjusted to meet different performance requirements and are applicable to a variety of application scenarios, such as air filtration, biomedicine, oil-water separation, and electronic sensing.

[0037] Example 1 (1) 30 g of TPU (average molecular weight = 100,000 - 120,000) and 70 g of a solvent (N,N-dimethylformamide:tetrahydrofuran = 1:1) with a mass ratio of 10:1 were placed in a conical flask, heated in a water bath at 60 °C for 3 h, and then magnetically stirred until a homogeneous solution was obtained to obtain a spinning solution. (2) An aqueous sandpaper with a mesh number of 2000 (average roughness Ra = about 0.3 microns, resistivity between 10 12 Ω·m - 10 15 Ω·m) was laid on the conveying device. The roughness of the sandpaper was used to reduce the number of bonding points between the fibers and the substrate, reducing the peeling difficulty for receiving the nanofibers generated by electrospinning. (3) The spinning solution was loaded onto the liquid pushing system. A 23-gauge spinning needle was used, the liquid pushing speed was 0.5 mL / h, and the linear distance between the spinning needle and the substrate was 12 cm. The positive high-voltage system was connected to the spinning needle, the negative high-voltage system was connected to the conveying device and the substrate, the positive voltage was adjusted to 15 kV, the receiving device was grounded with a potential of 0, the conveyor belt speed was 20 cm / s, and the high-voltage power supply was adjusted to 15 kV respectively. (4) The hot air drying system was turned on. The dryer temperature was 60 °C and the wind speed was 80 cm / s to remove the solvent from the nanofiber membrane with the substrate. (5) After drying, the substrate and the nanofibers were collected by their respective winding units after passing through the peeling unit, and a self-supporting electrospun nanofiber membrane was obtained, which can be used as a transparent anti-haze window screen. Among them, the radius of the peeling device = 2.5 cm, and the side length D = 6.2 cm.

[0038] As Figure 3As shown, the average fiber diameter of the self-supporting nanofiber membrane prepared in Example 1 is 380 nm, the fiber thickness is 5.5 μm, the porosity is 91.5%, the light transmittance is 70%, the filtration efficiency is 98.50%, and the maximum tensile strain is 150%. The yield rate is 85%.

[0039] Example 2 (1) Place 30 g of TPU (average molecular weight = 100,000 - 120,000) and 70 g of a solvent (N,N-dimethylformamide:tetrahydrofuran = 1:1) in a mass ratio of 10:1 in a conical flask. After heating in a water bath at 60°C for 3 h, stir magnetically until a homogeneous solution is obtained to get the spinning solution; (2) Select a mesh screen cloth (roughness > 10 microns, conductivity is 10 14 Ω·m) and lay it on the conveying device. Use the roughness of the mesh screen cloth to reduce the number of fiber-substrate bonding points and reduce the peeling difficulty for receiving the nanofibers generated by electrospinning; (3) Load the spinning solution onto the liquid pushing system. Use a No. 23 spinning needle, with a liquid pushing speed of 0.5 mL / h. The linear distance between the spinning needle and the substrate is 12 cm. Connect the positive high-voltage system to the spinning needle, connect the negative high-voltage system to the conveying device and the substrate, ground the receiving device with a potential of 0, and the conveyor belt speed range is 10 cm / s. Adjust the high-voltage power supply to 15 kV respectively; (4) Turn on the hot air drying system. The dryer temperature is 60°C and the wind speed is 100 cm / s to remove the solvent from the nanofiber membrane with the substrate; (5) After drying, the substrate and the nanofibers are collected by their respective winding units through the peeling unit, that is, a self-supporting electrospun nanofiber membrane is obtained. Among them, the radius R of the peeling device is 2.5 cm and the side length D is 6 cm.

[0040] As Figure 3 shown, the average fiber diameter of the self-supporting nanofiber membrane prepared in Example 2 is 380 nm, the fiber thickness is 10 μm, the porosity is 84%, the light transmittance is 82%, the filtration efficiency is 92.00%, the maximum tensile strain is 202%, and the yield rate is 98%.

[0041] Example 3 (1) Place 30 g of PAN polymer and 1170 g of solvent DMF in a conical flask. After heating in a water bath at 70°C for 4 h, stir magnetically until a homogeneous solution is obtained to get the spinning solution; (2) Select a smooth flat aluminum foil (average roughness Ra is about 0.02 microns, resistivity is 2.65*10 -8 Ω·m) and lay it on the conveying device for receiving the nanofibers generated by electrospinning; (3) Load the spinning solution onto the liquid pushing system, use a No. 15 spinning needle, with a liquid pushing speed of 1 ml / h, and the linear distance between the spinning needle and the substrate is 12 cm. The positive high-voltage system is connected to the spinning needle, the negative high-voltage system is connected to the conveyor and the substrate, the positive voltage is adjusted to 30 kV, the negative voltage is -5 kV, the conveyor speed is 30 cm / s, and the conveyor width is 100 cm; (4) Turn on the hot air drying system, with the dryer temperature at 60 °C and the wind speed at 20 cm / s, to remove the solvent from the nanofiber membrane with the substrate; (5) After drying, the substrate and the nanofibers are collected by their respective winding units after passing through the peeling unit, and a self-supporting electrospun nanofiber membrane is obtained. Among them, the radius R of the peeling device is 3 cm, and the side length D is 7.2 cm.

[0042] The average fiber diameter of the self-supporting PAN nanofiber membrane prepared in Example 3 is 470 nm, the average fiber thickness is 12.5 μm, the porosity is 87%, and the yield rate is 99%.

[0043] Example 4 (1) Place 14 g of polyamic acid (synthesized by reacting monomer biphenyltetracarboxylic dianhydride (BPDA) and p-phenylenediamine (PDA)) and 86 g of solvent DMF in a 500 ml conical flask, heat it in a water bath at 80 °C for 4 h, and then stir magnetically until a homogeneous solution is obtained to get the spinning solution; (2) Select a smooth silicone oil paper (with an average roughness Ra of about 0.02 microns and a conductivity of 10 13 Ω·m) and place it on the conveyor for receiving the nanofibers generated by electrospinning; (3) Load the spinning solution onto the liquid pushing system, use a No. 23 spinning needle, with a liquid pushing speed of 0.2 mL / h, and the linear distance between the spinning needle and the substrate is 10 cm. The positive high-voltage system is connected to the spinning needle, the negative high-voltage system is connected to the conveyor and the substrate, the positive voltage is adjusted to 60 kV, the negative voltage is -10 kV, the conveyor speed is 5 cm / s, and the conveyor width range is 120 cm; (4) Turn on the hot air drying system, with the dryer temperature at 70 °C and the wind speed at 1 m / s, to remove the solvent from the nanofiber membrane with the substrate; (5) After drying, the substrate and the nanofibers are collected by their respective winding units after passing through the peeling unit, and a self-supporting electrospun nanofiber membrane is obtained. Among them, the radius R of the peeling device is 3 cm, and the side length D is 7.2 cm.

[0044] As Figure 4As shown, the average fiber diameter of the self-supporting nanofiber membrane prepared in this example is 221 nm, the fiber thickness is 20 μm, the porosity is 90%, the filtration efficiency is 92.00%, the maximum tensile strain is 15%, and it can be used to make a filtration layer for protective clothing with high efficiency and low resistance, and the yield rate is 90%.

[0045] Example 5 (1) Put 3 g of TPU, 2 g of ZIF-8 powder and 20 g of solvent (DMF:THF = 1:1) into a 100 ml conical flask, place it in a water bath at 80 °C and heat for 6 h, then stir magnetically until a homogeneous solution is obtained to get the spinning solution; (2) Select a rough copper foil (average roughness Ra is about 1 micron and the conductivity is 1.8*10 -6 Ω·m) and place it on the conveying device. Use the roughness of the copper foil to reduce the number of bonding points between the fiber and the substrate and reduce the peeling difficulty for receiving the nanofibers generated by electrospinning; (3) Load the spinning solution into the liquid pushing system, use a No. 20 spinning needle, the liquid pushing speed is 0.7 mL / h, and the linear distance between the spinning needle and the substrate is 15 cm. The positive high-voltage system is connected to the spinning needle, the negative high-voltage system is connected to the conveying device and the substrate, the positive voltage is adjusted to 30 kV, the negative voltage is -5 kV, the conveyor belt speed is 20 cm / s, and the conveyor belt width is 80 cm; (4) Turn on the hot air drying system, the dryer temperature is 60 °C, the wind speed is 30 cm / s, and remove the solvent from the nanofiber membrane with the substrate; (5) After drying, the substrate and the nanofibers are collected by their respective winding units through the peeling unit, and a self-supporting electrospun nanofiber membrane is obtained. Among them, the radius R of the peeling device is 2.5 cm and the side length D is 6.2 cm.

[0046] As Figure 4 shown, the average fiber diameter of the self-supporting nanofiber membrane prepared in this example is 170 nm, the fiber thickness is 35 μm, the porosity is 91%, and the yield rate is 80%.

[0047] The above description is only the preferred embodiment of this application and the description of the applied technical principles. Those skilled in the art should understand that the scope of the invention involved in this application is not limited to the technical solutions formed by the specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the technical solutions formed by mutually replacing the above features with the (but not limited to) technical features with similar functions disclosed in this application.

Claims

1. A method for preparing a continuous self-supporting electrospun nanofiber membrane, characterized in that: The method comprises a conveying device, an electrospinning unit, a drying unit, a stripping unit and a winding unit arranged around the conveying device, and the steps are as follows: S1: preparing a solution to be spun by using a polymer, a solvent and an additive, and placing the solution in a liquid pushing system in the electrospinning unit; S2: Selecting a suitable substrate and placing it on the conveying device to receive the nanofibers produced by electrospinning; S3: Turn on the power of the high-voltage system, the conveying device, and the liquid pushing system, connect the positive high-voltage system to the spinning needle, connect the negative high-voltage system to the conveying device and the substrate, and the electrospinning unit sprays the spinning solution onto the substrate to obtain the electrospun nanofiber membrane with the substrate; S4: the electrospun nanofiber membrane with the substrate is transferred to the drying unit, and the drying unit starts to dry and remove the solvent of the substrate and the nanofiber membrane; S5: After passing through the stripping unit, the substrate and the nanofiber membrane are collected by respective winding units to obtain separated self-supporting electrospun nanofiber membrane and substrate.

2. A method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: There are several nozzles on the top of the electrospinning unit. The continuous movement of the conveyor matches the speed of the nozzles. When the nozzle liquid pushing speed is greater than 2.5 ml / h, the conveyor belt movement speed is greater than 15 cm / s.

3. The method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: When the liquid pushing rate of the nozzle is 0.2 ml / h~1 ml / h, the rotation speed of the conveying device is 5~30 cm / s.

4. The method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: When using a low conductivity substrate (resistivity greater than 10 -8 Ω·m), the forward voltage range is 15kV-60kV, the negative voltage range is -15-0kV, and the conveyor belt speed range is 1cm / s-30cm / s.

5. The method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: When a high conductivity substrate (resistivity less than 10 -8 Ω·m), the forward voltage range is 15kV-30kV, the negative voltage range is -5-0kV, and the conveyor belt speed range is 5cm / s-100cm / s.

6. The method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: The drying unit is located on one side of the substrate conveyor belt. When a low conductivity substrate is selected, the drying temperature is 60-80°C and the blast speed is 5-100 cm / s; when a high conductivity substrate is selected, the drying temperature is 40-60°C and the blast speed is 0-40 cm / s; when a patterned substrate is selected, the drying temperature is 40-80°C and the blast speed is 0-200 cm / s.

7. A method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: The stripping unit is a columnar metal with adjustable diameter, and the cross section is an arc cone. The arc and the cone are rounded. The radius of the arc is in the range of 2-8 cm, and the side length is in the range of 4-14 cm.

8. The method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: The drying unit is a batch type heat pump blower unit.

9. A method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: The diameter of the roller of the winding unit is adjustable, and the adjustable range is 3cm-20cm.

10. The method for preparing a continuous self-supporting electrospun nanofiber membrane according to claim 1, characterized in that: The mass ratio of the polymer, solvent and additive in step S1 is (5-20): (75-95): (0.5-5).

Citation Information

Patent Citations

  • Super-soft self-supporting nanometer net electrode and preparation method and application thereof

    CN114858877A

  • Self-supporting nanofiber membrane as well as preparation method and application thereof

    CN116288925A

  • Self-supporting nanofiber anti-haze screen window and preparation method thereof

    CN117071169A

  • Flexible self-supporting transparent porous micro-nanofiber membrane and preparation method thereof

    CN118166479A

Cited By

  • Electrostatic spinning process control method for directionally arranged silk fibers

    CN121161429A