Heat-stripping-resistant insulating brick and preparation method thereof

By using the reinforcement components and gradient heating technology of composite fiber toughening in insulation bricks, the problem of thermal peeling in the cold and emergency hot environment is solved, and efficient thermal peeling and insulation effects are achieved.

CN120172734APending Publication Date: 2025-06-20JIANGSU KUANYUAN NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510317165.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-18
Publication Date
2025-06-20

AI Technical Summary

Technical Problem

In the cold and hot environment, insulation bricks are prone to thermal peeling defects, resulting in surface damage.

Method used

The reinforcement components of composite fiber toughening are adopted and gradient heating technology are combined to ensure the full formation of the mullite phase, and the thermal peeling resistance of the insulation brick is improved through the coordination of macropores and micropores.

Benefits of technology

It achieves lightweight insulation while effectively taking into account the thermal peeling effect, improving the thermal stability and shock resistance of insulation bricks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120172734A_ABST
    Figure CN120172734A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of insulating bricks, and particularly relates to an anti-thermal-stripping insulating brick and a preparation method thereof, the preparation method comprises the following steps: S1, raw material pretreatment: pre-sintering lightweight aggregate at 600-800 DEG C for a certain time to obtain activated and impurity-removed lightweight aggregate; step S2, wet ball-milling and mixing, namely ball-milling and mixing the activated and impurity-removed lightweight aggregate, a reinforcing component, a binding component, a binder, a pore-forming agent, a sintering aid and deionized water in proportion until uniform slurry is obtained; s3, vacuum extrusion forming: injecting the uniform slurry into a mold, and then performing pressure forming to obtain a precast block; s4, gradient drying is conducted, specifically, the prefabricated block is heated to 110 DEG C from 50 DEG C in a gradient mode, and a to-be-sintered block is obtained; step S5, sintering in stages: preheating the to-be-sintered block at a low temperature of 400 DEG C, and then gradually raising the temperature in an environment of 1000-1200 DEG C to obtain the insulating brick; the mullite phase is fully formed by arranging the reinforcing component toughened by the composite fiber in cooperation with gradient heating, and by means of cooperation of the macro holes and the micro holes, the heat-resistant stripping effect is taken into account while the light heat preservation effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of thermal insulation bricks, and particularly relates to a thermal insulation brick with heat spalling resistance and a preparation method thereof. Background Art

[0002] A thermal insulation brick is a new type of building material synthesized using polymer materials, a new product that can replace ceramic tiles, and is mainly applicable to scenarios such as bathrooms, kitchens, TV background walls, bedrooms, exterior walls, etc.; moreover, it has bright colors, various specifications, can be cut arbitrarily, and the cut surface is neat.

[0003] However, when there is a large temperature difference between indoors and outdoors, such as in an environment where the outdoor temperature is -20 to -30 °C in winter, the excessive temperature difference on both sides of the surface of the thermal insulation brick is likely to generate internal stress, resulting in heat spalling and causing damage to the surface layer of the thermal insulation brick.

[0004] Therefore, how to provide a thermal insulation brick that can overcome the defect of heat spalling in a rapid cooling and heating environment is a technical problem that urgently needs to be solved in this field.

[0005] It should be noted that the above information disclosed in this background art section is only used to understand the background art of the concept of this application. Therefore, the above description is not considered as information on the prior art. Summary of the Invention

[0006] The embodiments of the present disclosure at least provide a thermal insulation brick with heat spalling resistance and a preparation method thereof.

[0007] In a first aspect, the embodiments of the present disclosure provide a preparation method of a thermal insulation brick with heat spalling resistance, including the following steps: Step S1, raw material pretreatment, that is, pre-burning lightweight aggregate at 600 - 800 °C for a certain period of time to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, that is, ball milling and mixing the activated and impurity-removed lightweight aggregate, reinforcing component, binding component, binder, pore-forming agent, sintering aid, and deionized water in proportion until a uniform slurry is obtained; Step S3, vacuum extrusion molding, that is, injecting the uniform slurry into a mold and pressing to form a preform; Step S4, gradient drying, heating the preform from 50 °C to 110 °C in a gradient manner to obtain a block to be sintered; Step S5, segmented sintering, preheating the block to be sintered at a low temperature of 400 °C and then gradually heating it in an environment of 1000 - 1200 °C to obtain a thermal insulation brick.

[0008] In an optional embodiment, the lightweight aggregate includes any one or a combination of fly beads, expanded perlite, and aluminum silicate fiber.

[0009] In an optional embodiment, the reinforcing component includes 3 - 8 parts by mass of mullite fiber and 2 - 5 parts by mass of glass fiber; wherein, the mullite fiber and glass fiber are surface-modified by a silane coupling agent.

[0010] In an alternative embodiment, the binding component comprises 6-9 parts by mass of high-purity alumina and 4-6 parts by mass of silica sol.

[0011] In an alternative embodiment, the components in the step S2 include the following parts by mass: 50-65 parts of activated and impurity-removed lightweight aggregate, 5-10 parts of reinforcing component, 10-15 parts of binding component, 5-8 parts of binder, 3-5 parts of pore former, and 1-2 parts of sintering aid.

[0012] In an alternative embodiment, after the uniform slurry is injected into the mold degassed under vacuum in the step S3, it is pressure-molded at 20-30 MPa and kept under pressure for 5-10 min.

[0013] In an alternative embodiment, the gradient drying in the step S4 specifically includes: drying for 4-6 h in an environment of 50-60 °C, drying for 6-8 h in an environment of 70-80 °C, and drying for 2-4 h at 100-110 °C.

[0014] In an alternative embodiment, the segmented sintering in the step S5 specifically includes: keeping the sintering block at 400-450 °C for 2-3 h, at 1000-1100 °C for 3-4 h, and at 1100-1200 °C for 2-3 h, and then cooling with the furnace.

[0015] In a second aspect, the embodiments of the present disclosure further provide a heat-resistant spalling-resistant insulating brick prepared by the method as described above, including: a lightweight porous inner layer and a high-alumina dense outer layer; the lightweight porous inner layer includes internal macropores with a pore size range of 100-300 μm; the high-alumina dense outer layer includes surface micropores with a pore size range of 10-50 μm.

[0016] In an alternative embodiment, the thermal conductivity of the insulating brick is not higher than 0.15 W / (m·K).

[0017] The beneficial effects of the present invention are that the heat-resistant spalling-resistant insulating brick and its preparation method ensure the full formation of mullite phase by setting a reinforcing component with composite fiber toughening and gradient heating. Moreover, the gradient heating can remove organic impurities at low temperature, form stable crystal phases at medium and high temperatures, and form a dense layer on the surface at high temperature. By using the combination of macropores and micropores, while achieving lightweight insulation, the heat-resistant spalling effect is also taken into account.

[0018] Other features and advantages of the present invention will be described in the following specification, and, in part, will be obvious from the specification, or will be understood by implementing the present invention. The objectives and other advantages of the present invention are achieved and obtained by the structures specifically pointed out in the specification and the drawings.

[0019] To make the above objects, features, and advantages of the present invention more obvious and understandable, the following provides preferred embodiments in conjunction with the accompanying drawings for detailed description as follows. Description of the Drawings

[0020] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following will briefly introduce the drawings required for use in the description of the specific embodiments or the prior art. Obviously, the drawings in the following description are some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can also be obtained based on these drawings.

[0021] Figure 1 It is a process flow diagram for the preparation of a heat-resistant spalling insulation brick provided by an embodiment of the present disclosure. Specific Embodiments

[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the following will clearly and completely describe the technical solutions of the present invention in conjunction with the drawings. Obviously, the described embodiments are some, but not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative efforts fall within the scope of protection of the present invention.

[0023] As used herein, phrases such as "in one embodiment", "according to one embodiment", "in some embodiments", etc. generally refer to the fact that the specific features, structures, or characteristics after the phrase can be included in at least one embodiment of the present disclosure. Therefore, specific features, structures, or characteristics can be included in more than one embodiment of the present disclosure, such that these phrases do not necessarily refer to the same embodiment. As used herein, terms such as "example", "exemplary", etc. are used "as an example, instance, or illustration. Any embodiment, aspect, or design described herein as "example" or "exemplary" is not necessarily to be construed as preferred or superior to other embodiments, aspects, or designs. Instead, the use of terms such as "example", "exemplary", etc. is intended to present concepts in a specific manner.

[0024] In this document, the exemplary embodiments of the present disclosure will be described in more detail with reference to the drawings. As used herein, expressions such as "at least one of..." modify the entire list of elements when following a list of elements, rather than modifying individual elements in the list. For example, the expression "at least one of a, b, and c" should be understood to include only a, only b, only c, both a and b, both a and c, both b and c, or all of a, b, and c.

[0025] The terms used herein are for describing specific exemplary configurations only and are not intended to be limiting. As used herein, the singular articles "a", "an", and "the" may also be intended to include the plural forms, unless clearly stated otherwise in the context. The terms "comprising", "including", and "having" are inclusive, thus specifying the presence of the features, steps, operations, elements, and / or components, but not precluding the presence or addition of one or more other features, steps, operations, elements, components, and / or their combinations. The method steps, processes, and operations described herein should not be construed as necessarily requiring them to be performed in the specific order discussed or shown, unless specifically identified as the order of execution. Additional or alternative steps may be employed.

[0026] The following will, with reference to the accompanying drawings, elaborate on some embodiments of the present invention. Without conflict, the following embodiments and the features in the embodiments may be combined with each other.

[0027] Please refer to Figure 1 , as Figure 1 shown, an embodiment of the present disclosure provides a method for preparing a heat-resistant spalling insulation brick, including the following steps: Step S1, raw material pretreatment, that is, pre-burning lightweight aggregate at 600 - 800 °C for a certain time to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, that is, ball milling and mixing the activated and impurity-removed lightweight aggregate, reinforcing component, binding component, binder, pore-forming agent, sintering aid, and deionized water in proportion until a uniform slurry is obtained; Step S3, vacuum extrusion molding, that is, injecting the uniform slurry into a mold and pressing to form a preform; Step S4, gradient drying, heating the preform from 50 °C to 110 °C in a gradient manner to obtain a block to be sintered; Step S5, segmented sintering, preheating the block to be sintered at a low temperature of 400 °C and then gradually heating it in an environment of 1000 - 1200 °C to obtain the insulation brick.

[0028] Specifically, the pre-burning in Step S1 can remove impurities in the lightweight aggregate and activate the surface of the lightweight aggregate to improve the subsequent reaction rate.

[0029] In some embodiments, specifically, the lightweight aggregate includes any one or a combination of any of cenospheres, expanded perlite, and aluminum silicate fiber.

[0030] In some embodiments, specifically, the reinforcing component includes 3 - 8 parts by mass of mullite fiber and 2 - 5 parts by mass of glass fiber; wherein, the mullite fiber and glass fiber are surface-modified by a silane coupling agent to enhance the dispersibility.

[0031] In some embodiments, specifically, the binding component includes 6 - 9 parts by mass of high-purity alumina and 4 - 6 parts by mass of silica sol. The high-purity alumina can improve the temperature resistance stability, but excessive alumina will increase the sintering temperature and cause a decline in the performance of other components.

[0032] In some embodiments, specifically, the components in the step S2 include the following parts by mass: 50 - 65 parts of activated impurity-removed light aggregate, 5 - 10 parts of reinforcing component, 10 - 15 parts of binding component, 5 - 8 parts of binder, 3 - 5 parts of pore-forming agent, and 1 - 2 parts of sintering aid.

[0033] Specifically, the binder is preferably aluminum dihydrogen phosphate, which is used to improve the green body strength.

[0034] Specifically, the pore-forming agent is preferably polystyrene microspheres, which are used to control the uniform distribution of microspheres and macropores.

[0035] Specifically, the sintering aid is preferably borax, which is used to reduce the sintering reaction temperature.

[0036] In some embodiments, specifically, after the uniform slurry is injected into a vacuum-degassed mold in the step S3, it is pressed and formed under a pressure of 20 - 30 MPa and kept under pressure for 5 - 10 min.

[0037] In some embodiments, specifically, the gradient drying in the step S4 specifically includes: drying in an environment of 50 - 60 °C for 4 - 6 h, drying in an environment of 70 - 80 °C for 6 - 8 h, and drying at 100 - 110 °C for 2 - 4 h, so as to avoid cracking of the sintered ore caused by rapid drying.

[0038] In some embodiments, specifically, the segmented sintering in the step S5 specifically includes: keeping the blocks to be sintered at 400 - 450 °C for 2 - 3 h, at 1000 - 1100 °C for 3 - 4 h, and at 1100 - 1200 °C for 2 - 3 h, and cooling with the furnace; among them, the low-temperature sintering at 400 - 450 °C can discharge the pore-forming agent and other organic aids in the blocks to be sintered, the medium-high temperature sintering at 1000 - 1100 °C is used to form the mullite phase, and the high-temperature sintering at 1100 - 1200 °C can finally form a high-alumina dense outer layer on the surface of the insulating brick.

[0039] The embodiment of the present disclosure also provides a heat-resistant spalling-resistant insulating brick prepared by the method as described above, including: a light porous inner layer and a high-alumina dense outer layer; the light porous inner layer includes internal macropores with a pore size range of 100 - 300 μm; the high-alumina dense outer layer includes surface micropores with a pore size range of 10 - 50 μm; through the cooperation of macropores and micropores, the porosity of the insulating brick is improved, and while taking into account the heat conduction and heat preservation effects, the thermal shock resistance effect is also improved.

[0040] In some embodiments, specifically, the thermal conductivity of the insulating brick is not higher than 0.15 W / (m·K).

[0041] Example 1

[0042] A preparation method of heat-resistant spalling insulation bricks, comprising the following steps: Step S1, raw material pretreatment, namely pre-burning cenospheres at 600 °C for 1 h to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, namely ball milling 55 parts of activated and impurity-removed lightweight aggregate, 9 parts of reinforcing components (5 parts of mullite fiber and 4 parts of glass fiber), 15 parts of binding components (9 parts of high-purity alumina and 6 parts of silicon solution), 8 parts of binder (aluminum dihydrogen phosphate), 4 parts of pore-forming agent (polystyrene microspheres), 2 parts of sintering aid (borax) and deionized water in proportion for 4 h, where the amount of deionized water is appropriate to meet the requirements of slip casting to obtain a uniform slurry; Step S3, vacuum extrusion molding, namely injecting the uniform slurry into a mold and pressurizing to form a preform; Step S4, gradient drying, drying at 50 °C for 4 h, drying at 70 °C for 6 h, and drying at 100 °C for 2 h to obtain a block to be sintered; Step S5, segmented sintering, holding at 400 °C for 2 h, holding at 1000 °C for 3 h, holding at 1100 °C for 2 h, and cooling with the furnace to obtain the insulation bricks.

[0043] Example 2

[0044] A preparation method of heat-resistant spalling insulation bricks, comprising the following steps: Step S1, raw material pretreatment, namely pre-burning cenospheres at 600 °C for 1 h to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, namely ball milling 60 parts of activated and impurity-removed lightweight aggregate, 8 parts of reinforcing components (4 parts of mullite fiber and 4 parts of glass fiber), 12 parts of binding components (7 parts of high-purity alumina and 5 parts of silicon solution), 7 parts of binder (aluminum dihydrogen phosphate), 3 parts of pore-forming agent (polystyrene microspheres), 2 parts of sintering aid (borax) and deionized water in proportion for 4 h, where the amount of deionized water is appropriate to meet the requirements of slip casting to obtain a uniform slurry; Step S3, vacuum extrusion molding, namely injecting the uniform slurry into a mold and pressurizing to form a preform; Step S4, gradient drying, drying at 55 °C for 4 h, drying at 75 °C for 6 h, and drying at 105 °C for 2 h to obtain a block to be sintered; Step S5, segmented sintering, holding at 400 °C for 2 h, holding at 1000 °C for 3 h, holding at 1100 °C for 2 h, and cooling with the furnace to obtain the insulation bricks.

[0045] Example 3

[0046] A preparation method of heat-resistant spalling insulation bricks includes the following steps: Step S1, raw material pretreatment, that is, pre-burning cenospheres at 800 °C for 1 h to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, that is, ball milling 65 parts of activated and impurity-removed lightweight aggregate, 6 parts of reinforcing components (3 parts of mullite fiber and 3 parts of glass fiber), 10 parts of binding components (6 parts of high-purity alumina and 4 parts of silicon solution), 6 parts of binder (aluminum dihydrogen phosphate), 3 parts of pore-forming agent (polystyrene microspheres), 2 parts of sintering aid (borax) and deionized water in proportion for 4 h, where the amount of deionized water is appropriate to meet the requirements of slip casting to obtain a uniform slurry; Step S3, vacuum extrusion molding, that is, injecting the uniform slurry into a mold and pressing to form a preform; Step S4, gradient drying, drying at 60 °C for 4 h, 80 °C for 6 h, and 110 °C for 2 h to obtain a block to be sintered; Step S5, segmented sintering, keeping warm at 450 °C for 2 h, 1100 °C for 3 h, and 1200 °C for 2 h, and cooling with the furnace to obtain the insulation bricks.

[0047] Example 4

[0048] A preparation method of heat-resistant spalling insulation bricks includes the following steps: Step S1, raw material pretreatment, that is, pre-burning cenospheres at 600 °C for 1 h to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, that is, ball milling 55 parts of activated and impurity-removed lightweight aggregate, 9 parts of reinforcing components (6 parts of mullite fiber and 3 parts of glass fiber), 15 parts of binding components (10 parts of high-purity alumina and 5 parts of silicon solution), 8 parts of binder (aluminum dihydrogen phosphate), 4 parts of pore-forming agent (polystyrene microspheres), 2 parts of sintering aid (borax) and deionized water in proportion for 4 h, where the amount of deionized water is appropriate to meet the requirements of slip casting to obtain a uniform slurry; Step S3, vacuum extrusion molding, that is, injecting the uniform slurry into a mold and pressing to form a preform; Step S4, gradient drying, drying at 50 °C for 4 h, 70 °C for 6 h, and 100 °C for 2 h to obtain a block to be sintered; Step S5, segmented sintering, keeping warm at 400 °C for 2 h, 1000 °C for 3 h, and 1100 °C for 2 h, and cooling with the furnace to obtain the insulation bricks.

[0049] Example 5

[0050] A preparation method of a heat-resistant spalling insulation brick, comprising the following steps: Step S1, raw material pretreatment, that is, pre-burning cenospheres at 600 °C for 1 h to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling and mixing, that is, ball milling 55 parts of activated and impurity-removed lightweight aggregate, 9 parts of reinforcing components (5 parts of mullite fiber and 4 parts of glass fiber), 15 parts of binding components (9 parts of high-purity alumina and 6 parts of silicon solution), 8 parts of binder (aluminum dihydrogen phosphate), 4 parts of pore-forming agent (polystyrene microspheres), 2 parts of sintering aid (borax) and deionized water in proportion for 4 h, where the amount of deionized water is appropriate to meet the requirements of slip casting to obtain a uniform slurry; Step S3, vacuum extrusion molding, that is, injecting the uniform slurry into a mold and pressing to form a preform; Step S4, gradient drying, drying at 50 °C for 4 h, drying at 70 °C for 6 h, and drying at 100 °C for 2 h to obtain a block to be sintered; Step S5, segmented sintering, heat preservation at 400 °C for 2 h, heat preservation at 1100 °C for 5 h, and cooling with the furnace to obtain the insulation brick.

[0051] Rapid heat treatment: During the heating process, the test temperature should be 5 °C lower than the actual maximum service temperature of the test brick. Raise the temperature in the heating device to the test temperature at the fastest heating rate and keep it for 10 min. Then quickly transfer the test brick sample into the heating device and keep it at this temperature for 10 min.

[0052] Rapid cooling treatment: After keeping the test brick sample at the test temperature for 10 min, quickly transfer it in front of the cooling device and blow it with a wind speed of (10 ± 0.5) m / s for rapid cooling for 10 min.

[0053] Test of heat-resistant spalling performance: Repeat the rapid heat treatment - rapid cooling treatment on the test brick sample until 10 cycles are reached, and calculate the average mass loss rate.

[0054] Specifically, when the average mass loss rate is lower than 5%, it means that the heat-resistant spalling effect of the insulation brick meets the standard.

[0055] Specifically, the insulation bricks obtained in Examples 1 - 3 were tested, and the results are shown in Table 1 below.

[0056] Table 1

[0057]

[0058] Specifically, because the contents of mullite fiber and glass fiber in the reinforcing components in Example 4 are not close to 1:1, the formation of internal pores will be affected to a certain extent during the sintering process. And when the content of high-purity alumina in the binding components is relatively high, a higher sintering temperature is required. Although the heat-resistant spalling effect is improved, the thermal conductivity is affected by the generation of internal and external pores.

[0059] Specifically, since segmented sintering was not carried out in Example 5, premature hardening of the outer layer affected the generation of internal macropores, and a dense layer could not be formed on the outer layer either. Only the pores generated by the conventional process were present, and the anti-thermal spalling effect was far inferior to that of other examples.

[0060] In summary, the heat-insulating brick with anti-thermal spalling and its preparation method ensure the full formation of the mullite phase by setting an enhanced component with composite fiber toughening and cooperating with gradient heating. Gradient heating can remove organic impurities at low temperatures, form stable crystal phases at medium and high temperatures, and form a dense layer on the surface layer at high temperatures. By utilizing the cooperation of macropores and micropores, the anti-thermal spalling effect is taken into account while achieving lightweight heat insulation.

[0061] Inspired by the ideal embodiments of the present invention described above, through the above description, relevant staff can completely make various changes and modifications without departing from the technical idea of the present invention. The technical scope of the present invention is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing thermal insulation bricks resistant to thermal spalling, characterized in that: The steps include: Step S1, raw material pretreatment, that is, pre-burning the lightweight aggregate at 600-800°C for a certain period of time to obtain activated and impurity-removed lightweight aggregate; Step S2, wet ball milling, that is, mixing the activated and impurity-removed lightweight aggregate, the reinforcing component, the bonding component, the binder, the pore former, the sintering aid and the deionized water in proportion by ball milling until a uniform slurry is obtained; Step S3, vacuum extrusion molding, that is, injecting the uniform slurry into a mold and then pressurizing it to obtain a prefabricated block; Step S4, gradient drying, gradually heating the prefabricated block from 50° C. to 110° C. to obtain a block to be sintered; Step S5, staged sintering, preheating the block to be sintered at a low temperature of 400°C and then gradually heating it at 1000-1200°C to obtain a thermal insulation brick.

2. The preparation method according to claim 1, characterized in that: The lightweight aggregate includes any one or more combinations of floating beads, expanded perlite, and aluminum silicate fiber.

3. The preparation method according to claim 1, characterized in that: The reinforcing component comprises 3-8 parts of mullite fiber and 2-5 parts of glass fiber by weight; Wherein, the mullite fiber and the glass fiber are surface-modified by a silane coupling agent.

4. The preparation method according to claim 1, characterized in that: The bonding components include 6-9 parts of high-purity alumina and 4-6 parts of silica sol by mass.

5. The preparation method according to claim 1, characterized in that: The step S2 includes the following components in parts by mass: 50-65 parts of activated and impurity-removed lightweight aggregate, 5-10 parts of reinforcing components, 10-15 parts of bonding components, 5-8 parts of binder, 3-5 parts of pore formers, and 1-2 parts of sintering aids.

6. The preparation method according to claim 1, characterized in that: The uniform slurry in step S3 is injected into a vacuum-degassed mold, and then pressurized at 20-30 MPa for molding, and the pressure is maintained for 5-10 minutes.

7. The preparation method according to claim 1, characterized in that: The gradient drying in step S4 specifically includes: drying at 50-60° C. for 4-6 hours, drying at 70-80° C. for 6-8 hours, and drying at 100-110° C. for 2-4 hours.

8. The preparation method according to claim 1, characterized in that: The staged sintering in step S5 specifically includes: keeping the to-be-sintered block at 400-450° C. for 2-3 hours, keeping it at 1000-1100° C. for 3-4 hours, and keeping it at 1100-1200° C. for 2-3 hours, and cooling it with the furnace.

9. A thermal insulation brick resistant to thermal spalling prepared by the method according to any one of claims 1 to 8, characterized in that: include: Lightweight porous inner layer and high-aluminum dense outer layer; The lightweight porous inner layer includes internal macropores with pore sizes ranging from 100 to 300 μm; The high-alumina dense outer layer includes surface micropores with a pore size range of 10-50 μm.

10. The heat-insulating brick resistant to thermal spalling according to claim 9, characterized in that: The thermal conductivity of the insulation brick is not higher than 0.15 W / (m·K).