Uranium nitride-silicon carbide composite pellet and preparation method thereof

Through the micro-encapsulation structure of the composite core pellet of uranium nitride and silicon carbide, the existing nuclear fuel resists water oxygen corrosion and fission product leakage at high temperatures, and achieves high thermal conductivity and high safety nuclear fuel applications, suitable for a variety of reactor types.

CN120260986APending Publication Date: 2025-07-04TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510203143.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-24
Publication Date
2025-07-04

AI Technical Summary

Technical Problem

The existing nuclear fuel uranium dioxide cannot efficiently deduce fission heat when the coolant is lost, resulting in melting accidents of core pellets or cladding. When the cladding in the reactor is ruptured, the fission product is easily reacted with water and oxygen, causing the fission product to leak, which cannot meet the requirements of high power and high safety.

Method used

The composite core pellet of uranium nitride and silicon carbide is adopted, with uranium nitride as the diffuse phase and silicon carbide as the continuous phase. A micro-encapsulated structure is formed through mixing and sintering treatment. The uranium nitride particles are wrapped with silicon carbide, which improves the resistance to water oxygen corrosion and thermal conductivity.

Benefits of technology

It achieves high thermal conductivity and high uranium density, enhances the water-oxygen corrosion resistance of the composite core pellet, effectively retains fission products, improves the safety and economy of nuclear fuel, and is suitable for advanced pressurized water reactors, fast neutron reactors and space reactors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005283752010000011
    Figure HDA0005283752010000011
  • Figure HDA0005283752010000012
    Figure HDA0005283752010000012
  • Figure HDA0005283752010000021
    Figure HDA0005283752010000021
Patent Text Reader

Abstract

The invention discloses a uranium nitride-silicon carbide composite pellet and a preparation method thereof, the composite pellet comprises a dispersed phase and a continuous phase, and the dispersed phase comprises uranium nitride; the continuous phase comprises silicon carbide, and the continuous phase is dispersed in the dispersed phase. The composite pellet disclosed by the invention has relatively high density and uranium density, relatively low fission product release rate, relatively good water and oxygen corrosion resistance at high temperature and relatively high safety and economical efficiency, the preparation method is simple, and the composite pellet has a wide application prospect in the field of nuclear fuel and can be applied to various advanced pressurized water reactors, fast neutron reactors and space reactors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of nuclear fuels, and specifically, to a uranium nitride-silicon carbide composite pellet and a preparation method thereof. Background Art

[0002] In the prior art, uranium dioxide is used as nuclear fuel, and its thermal conductivity is relatively low. In the event of a possible loss of coolant, UO2 cannot efficiently conduct fission heat and decay heat due to its low thermal conductivity, resulting in a melting accident of the pellet or cladding.

[0003] Uranium nitride (UN) is widely regarded as accident tolerant fuel (ATF), fast reactor fuel, and space reactor fuel because of its high thermal conductivity, high melting point, high uranium density, good irradiation stability, and hard neutron spectrum. However, the chemical properties of UN are relatively active, and its powder is extremely easy to be oxidized and self-ignited by air at room temperature, and it is also extremely easy to react with water at higher temperatures. In the event of a cladding rupture accident that may occur in a reactor, the UN pellet reacts with water and oxygen and will crack, resulting in a large amount of fission product leakage.

[0004] Therefore, the above-mentioned fuel pellets cannot meet the requirements of reactors for higher power and higher safety. Summary of the Invention

[0005] This application aims to solve at least one of the technical problems existing in the prior art to some extent. For this purpose, this application provides a composite pellet and a preparation method thereof. The composite pellet has a high density, thermal conductivity, and uranium density, excellent resistance to water and oxygen corrosion at high temperatures, high safety and economy, a simple preparation method, and broad application prospects in the field of nuclear fuels, and can be applied to various advanced pressurized water reactors, fast neutron reactors, and space reactors. Silicon carbide (SiC) has excellent irradiation stability, chemical stability, and high-temperature stability, and its thermal conductivity is also higher than that of UN.

[0006] In the first aspect of this application, this application proposes a composite pellet. According to an embodiment of this application, the composite pellet includes: a dispersed phase, the dispersed phase includes uranium nitride; a continuous phase, the continuous phase includes silicon carbide, and the dispersed phase is dispersed in the continuous phase.

[0007] According to the composite pellet of the above embodiments of the present application, its dispersion phase includes uranium nitride, which has the characteristics of high thermal conductivity, high melting point, and high uranium density and can be used as the fuel of a nuclear reactor. Thus, uranium nitride can meet the application requirements of nuclear fuel elements in many aspects; in addition, the continuous phase includes silicon carbide, which can wrap the uranium nitride particles to isolate them from water and oxygen in the outside world. Thus, to a certain extent, the water and oxygen corrosion resistance of UN particles and the entire composite pellet at high temperatures can be improved, and the thermal conductivity of the composite pellet can be increased. Thus, in the composite pellet of the present application, silicon carbide can form a "micro-encapsulation" for the uranium nitride particles wrapped therein, and each uranium nitride particle and the silicon carbide between the particles constitute a small "fuel element", and fission products can be effectively retained in the UN particles wrapped by SiC and are not likely to leak.

[0008] In addition, the composite pellet according to the above embodiments of the present application may further have the following additional technical features:

[0009] According to an embodiment of the present application, the uranium nitride content in the composite pellet is 10 wt% to 90 wt%.

[0010] According to an embodiment of the present application, the silicon carbide content in the composite pellet is 10 wt% to 90 wt%.

[0011] According to an embodiment of the present application, the uranium nitride is distributed in the composite pellet in a dispersed granular and discontinuous manner.

[0012] According to an embodiment of the present application, the silicon carbide is continuously distributed in the composite pellet in a three-dimensional network form.

[0013] In the second aspect of the present application, the present application proposes a method for preparing the above composite pellet. According to an embodiment of the present application, the method includes: mixing uranium nitride powder and silicon carbide powder to obtain a mixed powder; sintering the mixed powder to obtain the composite pellet.

[0014] According to the method for preparing the above composite pellets according to the embodiments of the present application, by mixing uranium nitride powder and silicon carbide powder, uranium nitride has the characteristics of high thermal conductivity, high melting point, and high uranium density and can be used as the fuel of a nuclear reactor. Thus, uranium nitride can meet the application requirements of nuclear fuel elements in multiple aspects. In addition, the continuous phase includes silicon carbide, which can wrap the uranium nitride particles to isolate them from water and oxygen in the outside world. Thus, to a certain extent, the water and oxygen corrosion resistance of UN particles and the entire composite pellets at high temperatures can be improved, and the thermal conductivity of the composite pellets can be further increased. Sintering the mixture of uranium nitride powder and silicon carbide powder can obtain formed composite pellets, and the content ratio of uranium nitride to silicon carbide in the composite pellets and the size of the pellets can be flexibly adjusted. Thus, in the composite pellets prepared by this method, silicon carbide can form "micro-encapsulation" for the uranium nitride particles wrapped therein, and each uranium nitride particle and the silicon carbide between the particles constitute a small "fuel element", and fission products can be effectively retained in the UN particles wrapped by SiC and are not easily leaked.

[0015] In addition, the composite pellets according to the above embodiments of the present application may further have the following additional technical features:

[0016] According to the embodiment of the present application, the average particle size of the uranium nitride powder is 1-30 μm.

[0017] According to the embodiment of the present application, the average particle size of the silicon carbide powder is 0.3-1.5 μm.

[0018] According to the embodiment of the present application, the mixing process is carried out in an inert atmosphere.

[0019] According to the embodiment of the present application, the sintering process includes spark plasma sintering, hot pressing sintering, and hot isostatic pressing sintering; preferably, spark plasma sintering.

[0020] According to the embodiment of the present application, the heating rate of the spark plasma sintering is 5-250 °C / min, the target temperature is 1300-2000 °C, the holding time is 3-120 min, and the pressure is 20-200 MPa.

[0021] According to the embodiment of the present application, the sintering process is carried out in an inert atmosphere or in a vacuum.

[0022] According to the embodiment of the present application, the sintering die used in the sintering process contains a graphite lining.

[0023] According to the embodiment of the present application, after the sintering process is completed, the obtained sintered product is polished.

[0024] Additional aspects and advantages of the present application will be given in part in the following description, become apparent in part from the following description, or be learned through the practice of the present application. Description of the Drawings

[0025] The above and / or additional aspects and advantages of the present application will become apparent and be readily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0026] Figure 1 is a schematic structural diagram of the composite pellet of the present application.

[0027] Figure 2 is a high-magnification SEM image of the composite pellet obtained in Example 1 of the present application.

[0028] Figure 3 is a low-magnification SEM image of the composite pellet obtained in Example 1 of the present application and its corresponding EDX image.

[0029] Figure 4 is a high-magnification SEM image of the composite pellet obtained in Example 2 of the present application. Detailed Description of the Embodiments

[0030] Embodiments of the present application will be described in detail below. The embodiments described below are exemplary and are only used to explain the present application and should not be construed as a limitation of the present application.

[0031] It should be noted that the terms "first" and "second" are only used for descriptive purposes and should not be construed as indicating or implying relative importance or implicitly specifying the quantity of the indicated technical features. Thus, features defined with "first" and "second" may explicitly or implicitly include one or more of such features. Further, in the description of the present application, unless otherwise specified, the meaning of "plurality" is two or more.

[0032] In the ranges disclosed herein, the endpoints and any values are not limited to the exact ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, between the endpoint values of each range, between the endpoint values and individual point values of each range, and between individual point values, they can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed herein.

[0033] In this document, the term "comprising" or "including" is an open expression, that is, it includes the content specified in the present application, but does not exclude other aspects of the content.

[0034] In this document, the terms "optionally", "optional" or "option" generally mean that the subsequent events or conditions may or may not occur, and this description includes the cases where the events or conditions occur and the cases where the events or conditions do not occur.

[0035] This application proposes a composite pellet and its preparation method, which will be described in detail below respectively.

[0036] Composite pellet

[0037] In the first aspect of this application, this application proposes a composite pellet. According to an embodiment of this application, the composite pellet includes: a dispersed phase, the dispersed phase includes uranium nitride; a continuous phase, the continuous phase includes silicon carbide, and the dispersed phase is dispersed in the continuous phase. According to an embodiment of this application, referring to Figure 1 , this composite pellet includes: uranium nitride (UN) and silicon carbide (SiC). For the composite pellet according to the above embodiment of this application, its dispersed phase includes uranium nitride, and uranium nitride has the characteristics of high thermal conductivity, high melting point, and high uranium density, and can be used as the fuel of a nuclear reactor. Thus, uranium nitride can meet the application requirements of nuclear fuel elements in multiple aspects; in addition, the continuous phase includes silicon carbide, which can wrap the uranium nitride particles to isolate them from water and oxygen in the outside world. Thus, to a certain extent, it can improve the resistance of UN particles and the entire composite pellet to water and oxygen corrosion at high temperatures, and improve the thermal conductivity of the composite pellet. Thus, in the composite pellet of this application, silicon carbide can form a "micro-encapsulation" for the uranium nitride particles wrapped therein, and each uranium nitride particle and the silicon carbide between the particles constitute a small "fuel element", and fission products can be effectively retained in the UN particles wrapped by SiC and are not easy to leak.

[0038] In addition, the composite pellet according to the above embodiment of this application may also have the following additional technical features:

[0039] According to an embodiment of this application, the content of uranium nitride in the composite pellet is 10 wt% - 90 wt%. Thus, it can further improve the uranium density and thermal conductivity of the composite pellet, and the content ratio can be flexibly adjusted as needed.

[0040] According to an embodiment of this application, the content of silicon carbide in the composite pellet is 10 wt% - 90 wt%. Thus, it ensures that the composite pellet has a high thermal conductivity, while improving its ability to retain fission products and corrosion resistance, and the content ratio can be flexibly adjusted as needed.

[0041] According to an embodiment of this application, the uranium nitride is in the form of particles and is discontinuously distributed in the composite pellet. Thus, an efficient micro-encapsulation structure is formed to ensure the high uranium density of the composite pellet and ensure the efficiency and performance of nuclear fuel.

[0042] According to an embodiment of this application, the silicon carbide is continuously distributed in the composite pellet in a three-dimensional network form. Thus, an efficient micro-encapsulation structure is formed, which helps to improve the resistance of the composite pellet to water and oxygen corrosion at high temperatures, and also helps to limit the spillage of fission products.

[0043] Method for preparing composite pellet

[0044] In the second aspect of the present application, the present application provides a method for preparing the above-mentioned composite pellet. According to an embodiment of the present application, the method includes: mixing uranium nitride powder and silicon carbide powder to obtain a mixed powder; sintering the mixed powder to obtain the composite pellet.

[0045] According to the method for preparing the above-mentioned composite pellet in the embodiment of the present application, by mixing uranium nitride powder and silicon carbide powder, uranium nitride has the characteristics of high thermal conductivity, high melting point, and high uranium density, and can be used as a fuel for nuclear reactors. Therefore, uranium nitride can meet the application requirements of nuclear fuel elements in many aspects; in addition, the continuous phase includes silicon carbide, which can wrap uranium nitride particles to isolate them from external water and oxygen. Thus, the water and oxygen corrosion resistance of UN particles and the entire composite pellet at high temperatures can be significantly improved, and the thermal conductivity of the composite pellet can be further increased; sintering the mixture of uranium nitride powder and silicon carbide powder can obtain a formed nuclear fuel element, and the content ratio of uranium nitride to silicon carbide in the composite pellet and the size of the pellet can be flexibly adjusted. Therefore, in the composite pellet prepared by this method, silicon carbide can form a "micro-encapsulation" for the uranium nitride particles wrapped therein, and each uranium nitride particle and the silicon carbide between the particles form a small fuel element, and fission products can be effectively retained in the UN particles wrapped by SiC and are not easily leaked.

[0046] In addition, the composite pellet according to the above embodiment of the present application may further have the following additional technical features:

[0047] According to an embodiment of the present application, the average particle size of the uranium nitride powder is 1 to 30 μm. Thus, this particle size range helps the combination between the uranium nitride powder and the silicon carbide powder, ensuring an appropriate contact area and reaction activity during the sintering process, so that uranium nitride is distributed in the composite pellet in a dispersed granular and discontinuous manner.

[0048] According to an embodiment of the present application, the average particle size of the silicon carbide powder is 0.3 to 1.5 μm. Thus, this particle size range helps the combination between the uranium nitride powder and the silicon carbide powder, ensuring an appropriate contact area and reaction activity during the sintering process, so that silicon carbide is continuously distributed in the composite pellet in a three-dimensional network shape.

[0049] According to an embodiment of the present application, the mixing process is carried out in an inert atmosphere. Thus, the uranium nitride powder is protected from oxidation and the formation of oxides is avoided, ensuring the purity and nuclear purity requirements of the powder.

[0050] According to an embodiment of the present application, the sintering treatment includes spark plasma sintering, hot pressing sintering, and hot isostatic pressing sintering; preferably, spark plasma sintering. Thus, the rapid densification of the powder is achieved by sintering technology at a relatively low temperature and in a relatively short time.

[0051] According to an embodiment of the present application, the heating rate of the spark plasma sintering is 5 - 250 °C / min, the target temperature is 1300 - 2000 °C, the holding time is 3 - 120 min, and the pressure is 20 - 200 MPa. Thus, an appropriate heating rate can quickly reach the high temperature required for sintering, while avoiding the destruction of the material structure caused by overheating; an appropriate target temperature ensures that the material can be densified at an appropriate temperature; an appropriate holding time ensures that the material is fully sintered to form a tight inter-particle bond; an appropriate pressure promotes the close arrangement of particles and the increase in density; an appropriate DC pulse current and an appropriate voltage provide the unique thermal energy and electric field effects of spark plasma sintering, further accelerating the densification process of the material.

[0052] According to an embodiment of the present application, the sintering treatment is carried out in an inert atmosphere or in a vacuum. Thus, the uranium nitride powder is protected from oxidation, avoiding the formation of oxides, and ensuring the purity and nuclear purity requirements of the powder.

[0053] According to an embodiment of the present application, the sintering mold used in the sintering treatment contains a graphite lining. Thus, heat can be quickly and evenly transferred during the sintering process, promoting the densification of the composite pellet.

[0054] According to an embodiment of the present application, after the sintering treatment is completed, the obtained sintered product is polished. Thus, the graphite lining on the surface of the composite pellet and possible surface defects are removed, ensuring that the surface of the composite pellet is flat and smooth, meeting the appearance and dimensional requirements of the nuclear fuel element.

[0055] The solution of the present application will be explained below in conjunction with embodiments. Those skilled in the art will understand that the following embodiments are only used to illustrate the present application and should not be regarded as limiting the scope of the present application. For those not specified in the embodiments regarding specific technologies or conditions, they shall be carried out according to the technologies or conditions described in the literature in this field or according to the product specifications. For reagents or instruments not specified by the manufacturer, they are all conventional products that can be obtained through commercial purchase.

[0056] Example 1:

[0057] (1) In a glove box filled with high-purity argon (99.999%) atmosphere, 1 g of high-purity UN powder with an average particle size of 2 μm was weighed, and 0.2 g of high-purity SiC powder with an average particle size of 0.5 μm was weighed. After mixing, they were thoroughly ground for 1 hour.

[0058] (2) Cut the high-purity graphite paper with a thickness of 0.2 mm into two discs with a diameter of 1 cm and one circular paper tube with a diameter of 1 cm and a height of 4 cm. Select a set of high-strength, high-purity isostatic graphite molds. The inner diameter of the cylindrical sleeve of the mold is 1.04 cm, the outer diameter is 4 cm, and the height is 4 cm. The upper and lower heads of the mold are graphite cylinders with a diameter of 1 cm and a height of 3 cm. Insert the graphite paper cylinder into the mold sleeve and ensure it is flat. Place a graphite paper disc on the top of the lower head and insert it about 1.9 cm from the lower end of the mold sleeve. In an argon atmosphere glove box, pour the mixed powder of UN and SiC prepared in the previous step into the mold from the upper end of the mold sleeve and vibrate it. Place a graphite paper disc on the top of the upper head and insert it from the upper end of the mold sleeve and press it. After connecting the upper and lower heads to the upper and lower bases, the sample and mold are assembled.

[0059] (3) Move the sample and mold assembled in the previous step out of the glove box, load them into the SPS equipment furnace chamber and seal them. Turn on the vacuum pump to evacuate to below 5Pa, fill high-purity argon gas at a gas flow rate of 15L / min to atmospheric pressure, then open the outlet valve and maintain the gas flow at 15L / min. Set the sintering process as follows: heating rate of 200℃ / min, target temperature of 1700℃, holding time of 15min, and pressure of 55MPa. After the furnace cools to room temperature, stop filling with argon gas.

[0060] (4) Take out the sample and mold after sintering in the previous step. Remove the upper and lower bases and the top of the mold, and take out the composite core block wrapped with graphite paper. Use 800 mesh and 2000 mesh diamond sandpaper to grind the composite core block successively until the carbon paper wrapped on its surface is completely removed and the composite core block with silver and metallic luster is exposed. The obtained composite core block is the composite core block.

[0061] Embodiment 2:

[0062] (1) In a glove box filled with high-purity argon gas, weigh 1 g of high-purity UN powder with an average particle size of 3 μm and weigh 0.1 g of high-purity SiC powder with an average particle size of 0.5 μm, mix them, and grind them thoroughly for 1 hour.

[0063] (2) Cut two circular wafers with a diameter of 1 cm and one circular paper tube with a diameter of 1 cm and a height of 4 cm from high-purity graphite paper with a thickness of 0.1 mm. Select a set of isostatic pressing graphite molds with high strength and high purity. The inner diameter of the cylindrical sleeve of the mold is 1.02 cm, the outer diameter is 4 cm, and the height is 4 cm. The upper and lower plugs of the mold are graphite cylinders with a diameter of 1 cm and a height of 3 cm. Insert the graphite paper cylinder into the mold sleeve and ensure it is flat. Place a graphite paper wafer on the top of the lower plug and insert it about 1.9 cm from the lower port of the mold sleeve. In a glove box with an argon atmosphere, pour the mixed powder of UN and SiC prepared in the previous step into the mold from the upper end of the mold sleeve and compact it. Place a graphite paper wafer on the top of the upper plug and insert and press it from the upper port of the mold sleeve. After connecting the upper and lower plugs to the upper and lower bases, the sample and the mold are assembled.

[0064] (3) The same as (3) of Example 1, where the sintering process is as follows: the heating rate is 200 °C / min, the target temperature is 1700 °C, the holding time is 10 min, and the pressure is 55 MPa.

[0065] (4) The same as (4) of Example 1.

[0066] Example 3:

[0067] (1) In a glove box with a high-purity argon atmosphere, weigh 3 g of high-purity UN powder with an average particle size of 10 μm and weigh 0.2 g of high-purity SiC powder with an average particle size of 0.4 μm. After mixing, grind them thoroughly for 1 hour.

[0068] (2) The same as (2) of Example 1.

[0069] (3) Remove the sample and the mold assembled in the previous step from the glove box, place them in the furnace cavity of the SPS equipment and seal. Turn on the vacuum pump to pump the vacuum to below 5 Pa and keep the vacuum pump in a continuous pumping state. Set the sintering process as follows: the sintering process is: the heating rate is 200 °C / min, the target temperature is 1650 °C, the holding time is 15 min, the pressure is 145 MPa, the DC pulse current is 0 - 500 A, and the voltage is 0 - 380 V. Cool the furnace to room temperature and then break the vacuum.

[0070] (4) The same as (4) of Example 1.

[0071] Test Example

[0072] Perform SEM inspection on the composite pellets obtained in Example 1. The high-magnification image is as Figure 2 shown, and the low-magnification SEM image and the corresponding EDX image are as Figure 3 shown. Figure 2 It shows that the pellets have high density and no obvious holes. Figure 3The element distribution map shows that the light-colored area is the UN phase, which is the main component in the pellet and is diffusely and discontinuously distributed; the dark-colored area is the SiC phase, which is a minor component in the pellet, is continuously distributed, and encloses the UN particles within it. The two substances are tightly combined.

[0073] The SEM image of the composite pellet obtained in Example 2 is as Figure 4 shown, indicating that the composite pellet has a high density and no obvious pores. The light-colored area is the UN phase, which is the main component in the pellet and is diffusely and discontinuously distributed. The dark-colored area is the SiC phase, which is a minor component in the pellet, is continuously distributed, and encloses the UN particles within it. The two substances are tightly combined.

[0074] The measured densities of the composite pellets obtained in Examples 1 to 3 are 95.4% TD, 95.3% TD, and 92.0% TD, respectively.

[0075] In the description of this specification, the description referring to terms such as "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in connection with that embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in a suitable manner in any one or more embodiments or examples. In addition, without contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples.

[0076] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and should not be construed as limiting the present application. Those of ordinary skill in the art can make changes, modifications, substitutions, and variations to the above embodiments within the scope of the present application.

Claims

1. A composite pellet, characterized in that, Comprising: A dispersion phase, the dispersion phase comprising uranium nitride; A continuous phase, the continuous phase comprising silicon carbide, the continuous phase being dispersed in the dispersion phase.

2. The composite pellet according to claim 1, characterized in that, The content of uranium nitride in the composite pellet is 10 wt% to 90 wt%; Optionally, the content of silicon carbide in the composite pellet is 10 wt% to 90 wt%.

3. The composite pellet according to claim 1, characterized in that, The uranium nitride is in particulate form and is discontinuously distributed within the composite pellet; Optionally, the silicon carbide is continuously distributed in a three-dimensional network within the composite pellet.

4. A method for preparing the composite pellet according to any one of claims 1 to 3, characterized in that, Comprising: Mixing uranium nitride powder and silicon carbide powder to obtain a mixed powder; Sintering the mixed powder to obtain the composite pellet.

5. The method according to claim 4, characterized in that The average particle size of the uranium nitride powder is 1 to 30 μm; Optionally, the average particle size of the silicon carbide powder is 0.3 to 1.5 μm; Optionally, the mixing treatment is carried out in an inert atmosphere.

6. The method according to claim 4, characterized in that, The sintering treatment includes spark plasma sintering, hot pressing sintering, hot isostatic pressing sintering; preferably spark plasma sintering; Optionally, the heating rate of the spark plasma sintering is 5 to 250 °C / min, the target temperature is 1300 to 2000 °C, the holding time is 3 to 120 min, and the pressure is 20 to 200 MPa.

7. The method according to claim 4, wherein The sintering treatment is carried out in an inert atmosphere or in a vacuum.

8. The method according to claim 4, characterized in that, The sintering die used in the sintering treatment contains a graphite paper lining; Optionally, after the sintering treatment is completed, the obtained sintered product is polished.