Method and system for separating byproducts of tantalum powder mixed salt

By combining enhanced leaching, density gradient separation, and defluorination treatment, the high cost and wastewater discharge problems in the separation of tantalum powder mixed salt byproducts have been solved, achieving efficient resource recovery and an environmentally friendly separation process.

CN120328619BActive Publication Date: 2026-11-17NINGXIA ORIENT TANTALUM INDUSTRY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510512709.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-23
Publication Date
2026-11-17
Estimated Expiration
2045-04-23

AI Technical Summary

Technical Problem

Existing technologies for processing tantalum powder mixed salt byproducts suffer from high costs, large amounts of wastewater discharge, environmental pollution, and low recovery rates.

Method used

A combined approach of enhanced leaching, density gradient separation, and defluorinating agent treatment is adopted. Through physical separation and chemical treatment, sodium fluoride and tantalum pentoxide are separated from the mixed salt, reducing the concentration of fluoride ions in the solution, reducing the amount of defluorinating agent used, and achieving solid-liquid separation.

Benefits of technology

It effectively improves the recovery rate, reduces separation costs, reduces wastewater discharge, reduces environmental impact, and achieves efficient separation and resource recovery of tantalum powder mixed salt byproducts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120328619B_ABST
    Figure CN120328619B_ABST
Patent Text Reader

Abstract

This invention relates to the field of tantalum powder mixed salt byproduct separation technology, and particularly to a method and system for separating tantalum powder mixed salt byproducts. The method includes: leaching and separating tantalum powder mixed salt to obtain a mixed solid containing sodium fluoride and tantalum pentoxide, and a mixed salt solution whose main component is potassium chloride; physically separating the mixed solid to obtain purified sodium fluoride and tantalum slag; and defluorinating the mixed salt solution until the fluoride ion concentration in the mixed salt solution meets preset conditions. Compared with traditional methods, the tantalum powder mixed salt byproduct separation method provided in this application effectively improves the recovery rate while reducing costs; furthermore, because it uses less water and does not generate wastewater, it minimizes the environmental impact throughout the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of tantalum powder mixed salt by-product separation technology, and in particular to a method and system for separating tantalum powder mixed salt by-products. Background Technology

[0002] The sodium reduction of potassium fluorotantalate, also known as the Hunter process, is a method for preparing tantalum powder using K₂TaF₇ and sodium metal as the main raw materials, and adding a halogen salt or a mixture of halogen salts as a diluent during the reaction. Its chemical reaction equation is as follows: K2TaF7+5Na=Ta+5NaF+2KF This method has low production costs and is the most commonly used method for tantalum production. However, the process generates a mixed salt byproduct containing a large amount of KF, NaCl, NaF and KCl and a small amount of Ta2O5 (about 0.4-0.7%). If this byproduct is discarded directly, it will cause great harm to the environment.

[0003] Currently, traditional treatment methods for this tantalum-containing mixed salt byproduct can be divided into three types: The first method involves dissolving all the mixed salts and then adding a large amount of calcium chloride or other fluoride ion precipitant to the dissolved solution to remove fluoride, ensuring that the fluoride ion levels in the wastewater meet emission standards before direct discharge, as shown in CN109399669A. The second method involves dissolving all the mixed salts and recovering the fluoride ions in the solution as sodium fluoroaluminate or potassium fluoroborate before discharging the wastewater, as shown in CN212102961U. Both methods require dissolving all the mixed salts first, extracting ultrafine tantalum powder and oxides from the filter residue, and then using a wet extraction process to recover the tantalum powder. However, the solubility of sodium fluoride in the tantalum-containing mixed salt byproduct is low; only 4.02g of sodium fluoride can dissolve in 100g of water. Both methods generate large amounts of industrial wastewater, polluting the environment, and the recovery rate of valuable elements in the byproducts is low. Moreover, lime is usually used as a defluorinating agent, which requires a large amount of lime, resulting in high defluorination costs and a large amount of lime residue, increasing additional storage and transportation costs. The third method is to directly evaporate the obtained solution to obtain a composite salt for the preparation of potassium fluorotantalate or metallurgical tantalum powder, such as CN102336438A and CN102352444A. Although this method realizes the effective utilization of solid waste resources, the process differences in the preparation of different types of tantalum powder are large, resulting in large fluctuations in the mixed salt composition of the by-products, which is difficult to adjust. Summary of the Invention

[0004] In view of this, it is necessary to provide a method for separating tantalum powder mixed salt byproducts to reduce recycling costs, reduce wastewater discharge, and avoid environmental pollution.

[0005] A method for separating tantalum powder mixed salt byproducts, comprising: The tantalum powder was leached and separated to obtain a mixed solid containing sodium fluoride and tantalum pentoxide, as well as a mixed salt solution whose main component was potassium chloride. The mixed solid was physically separated to obtain sodium fluoride solid and tantalum pentoxide solid. The mixed salt solution is treated with a defluorinating agent to remove fluoride until the fluoride ion concentration in the mixed salt solution meets the preset conditions.

[0006] Preferably, the tantalum powder is leached and separated to obtain a mixed solid containing sodium fluoride and tantalum pentoxide. The leaching and separation methods used include enhanced leaching, pressure leaching, reactor leaching, and stirred leaching.

[0007] Preferably, the mixed solids are physically separated to obtain sodium fluoride solid and tantalum pentoxide solid. The physical separation methods used include density gradient separation, bubbling separation, and air separation.

[0008] Preferably, the density gradient separation method includes using one or more of sodium sulfate solution, potassium sulfate solution, and potassium fluorosilicate solution as the heavy density liquid, and the volume ratio of the heavy density liquid to the weight ratio of the tantalum powder mixed salt is 0.1~15:1; the reaction temperature is 10~100℃; and the contact time is 0.5~10 hours.

[0009] Preferably, the volume ratio of the heavy density liquid to the weight ratio of the tantalum powder mixed salt is 0.6~7.5:1; the reaction temperature is 35~90℃; and the contact time is 0.5~8 hours.

[0010] Preferably, the method further includes: mixing the mixed solid with a liquid of a certain density and then mechanically stirring it.

[0011] Preferably, the defluorination treatment of the mixed salt solution includes selecting one or at least two of magnesium chloride, polyaluminum chloride, lanthanum nitrate, calcium chloride, and polyacrylamide as defluorinating agents.

[0012] Preferably, the process further includes: after adding a defluorinating agent, solid-liquid separation is performed by centrifugation; wherein the centrifugation speed is 1000~8000 rpm; the centrifugation time is 1~10 minutes; and the centrifugation temperature is 10~100℃.

[0013] Preferably, in the solid-liquid separation by centrifugation, the centrifugation speed is 3000~7000 rpm; the centrifugation time is 2~8 minutes; and the centrifugation temperature is 30~90℃.

[0014] A tantalum powder mixed salt byproduct separation system includes: An enhanced leaching device is used to leach and separate tantalum powder mixed salt to obtain a mixed solid containing sodium fluoride and tantalum pentoxide, and a mixed salt solution whose main component is potassium chloride; A physical separation device is used to physically separate the mixed solids to obtain sodium fluoride solid and tantalum pentoxide solid; A mixed salt solution treatment device is used to defluorinate the mixed salt solution until the fluoride ion concentration in the mixed salt solution meets a preset condition.

[0015] Compared with existing technologies, the advantages of this application are as follows: In the novel method for separating tantalum powder mixed salt byproducts, an enhanced leaching process is employed, ensuring that a large amount of sodium fluoride remains in solid form, thereby reducing the fluoride ion content in the solution. This reduces the amount of defluorinating agent used, thus lowering separation costs. Furthermore, through physical separation methods such as density gradient separation, sodium fluoride and tantalum pentoxide are directly separated, eliminating the need for adding large amounts of water to dissolve sodium fluoride and obtain tantalum pentoxide. This method has low separation costs and produces no wastewater. The solution provided in this application effectively improves the recovery rate while reducing costs, and because it uses less water and produces no wastewater, it minimizes environmental impact throughout the process. Attached Figure Description

[0016] Figure 1 This is a schematic flowchart of the method for separating tantalum powder mixed salt byproducts provided in the embodiments of this application.

[0017] Figure 2 This is a schematic diagram of the planar structure of the tapered thin-walled rotary turning fixture provided in the embodiments of this application. Detailed Implementation

[0018] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Please see Figure 1 , Figure 1 This is a schematic flowchart of the method for separating tantalum powder mixed salt byproducts provided in this application embodiment. The method for separating tantalum powder mixed salt byproducts includes the following steps: S101: The tantalum powder is leached and separated into a mixed solid containing sodium fluoride and tantalum pentoxide, and a mixed salt solution whose main component is potassium chloride.

[0020] A rotating liquid film reactor can be used for enhanced leaching of tantalum powder mixed salts, which significantly shortens the leaching time compared to traditional leaching methods. This allows for the complete exchange of fluoride, chloride, sodium, and potassium ions in the tantalum powder mixed salts, converting them into high-value-added KCl and NaF. Furthermore, sodium fluoride is poorly soluble in water and easily separated from the salt solution. Since a large amount of sodium fluoride remains in solid form after enhanced leaching, the fluoride ion content in the solution is low, greatly reducing the amount of defluorinating agent used and thus lowering separation costs. The reaction equation is: KF + NaCl = NaF + KCl.

[0021] In addition to enhanced leaching, other methods such as pressure leaching, reactor leaching, and stirred leaching can also be selected.

[0022] S102: The mixed solids are physically separated to obtain sodium fluoride solid and tantalum pentoxide solid.

[0023] Physical separation methods include density gradient separation, bubbling, and air separation. Furthermore, this application preferably employs density gradient separation, using one or more mixtures selected from sodium sulfate solution, potassium sulfate solution, potassium fluorosilicate solution, carbon tribromide, xylyl ether, and carbon tetrabromide as the heavy density liquid, wherein the volume ratio of the heavy density liquid to the weight ratio of the tantalum powder mixed salt is 0.1~15:1; the reaction temperature is 10~100℃; and the contact time is 0.5~10 hours. To promote thorough mixing, the mixed solid and the heavy density liquid are mechanically stirred after mixing, and multiple stirring speeds can be set for differential stirring.

[0024] Furthermore, as a preferred embodiment of this application, the volume ratio of the heavy density liquid to the weight ratio of the tantalum powder mixed salt is 0.6~7.5:1; the reaction temperature is 35~90℃; and the contact time is 0.5~8 hours.

[0025] Sodium fluoride and tantalum pentoxide can be directly separated using density gradient separation without further treatment. Compared to directly dissolving sodium fluoride in a large amount of water to obtain tantalum pentoxide, gravity separation has lower operating costs and produces no wastewater. After separating tantalum pentoxide and sodium fluoride, the density gradient liquid can still be used for the next density gradient separation, which can greatly reduce the amount of density gradient liquid used and further reduce separation costs.

[0026] S103: The mixed salt solution is defluorinated using a defluorinating agent until the concentration of fluoride ions in the mixed salt solution meets the preset conditions.

[0027] Fluoride ion removal: The first step is to address the small amount of fluoride ions present in the solution. According to the present invention, various defluorinating agents can be used to reduce the concentration of fluoride ions in the solution. These defluorinating agents include, but are not limited to, magnesium chloride, polyaluminum chloride, lanthanum nitrate, calcium chloride, and polyacrylamide. Preferably, calcium chloride is used as the defluorinating agent because it reacts with fluoride ions to form a water-insoluble calcium fluoride precipitate, thereby effectively removing fluoride ions.

[0028] After adding a defluorinating agent, solid-liquid separation is performed by centrifugation. The centrifugation speed is 1000~8000 rpm; the centrifugation time is 1~10 minutes; and the centrifugation temperature is 10~100℃. Preferably, the centrifugation speed is 3000~7000 rpm; the centrifugation time is 2~8 minutes; and the centrifugation temperature is 30~90℃.

[0029] The reaction equation is:

[0030] It is important to note that when using composite defluorinating agents, the ratio of calcium ions to fluoride ions in the salt solution should be maintained at 1:2 to avoid introducing other unwanted ions. During fluoride ion removal, the reaction temperature is set within a specific range, typically 10-100°C, preferably 35-90°C. Appropriate temperature helps improve the efficiency of the chemical reaction, allowing for more complete removal of fluoride ions.

[0031] The fluoride ion concentration in the mixed salt solution after the above treatment must meet the relevant environmental or industrial reuse standards. For example, the maximum allowable discharge concentration of fluoride ions in industrial wastewater in China is typically 1 mg / L (i.e., 1 ppm), but this value may be lower in some more stringent regions or for certain specific industries. If the treated solution is planned for use in further industrial production processes, such as the preparation of other chemicals or as process water, it is necessary to ensure that the fluoride ion concentration is below a level that would affect the performance of subsequent processes (depending on the specific application and process requirements). When the goal of the treatment is to convert the solution into a marketable product, such as high-purity potassium chloride (KCl), the fluoride ion concentration must meet the quality specifications of the corresponding product. Once these standards are met, the solution can be sold directly or further processed through cooling precipitation, evaporation, etc., to obtain potassium chloride (KCl) products with higher purity.

[0032] The following describes a method for separating tantalum powder mixed salt byproducts with specific examples: Using a certain tantalum byproduct as experimental material, the weight percentage of its main components was analyzed to be: 26.53% Na, 19.71% F, 27.38% Cl, 25.72% K and 0.66% Ta2O5.

[0033] The separation process of this tantalum powder mixed salt is as follows: 500g of tantalum powder mixed with salt was stirred, leached and separated to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed evenly with a saturated sodium sulfate solution at a solid-liquid ratio of 1:2, and then subjected to density gradient separation at 80°C with mechanical stirring at 500 rpm, 200 rpm and 100 rpm for one hour each. The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard. Example 2:

[0034] 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed evenly with a saturated sodium sulfate solution at a solid-liquid ratio of 1:2, and then subjected to density gradient separation at 80°C with mechanical stirring at 500 rpm, 200 rpm and 100 rpm for one hour each.

[0035] The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard. Example 3:

[0036] 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed evenly with a saturated sodium sulfate solution at a solid-liquid ratio of 1:2, and then subjected to density gradient separation at 80°C with mechanical stirring at 500 rpm, 200 rpm and 100 rpm for one hour each. Add calcium chloride to the obtained mixed salt solution A to remove fluoride until the fluoride ion concentration in the solution meets the standard. Example 4:

[0037] 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed with deionized water at a solid-liquid ratio of 1:2 and then subjected to density gradient separation at 80°C. The mechanical stirring was carried out at 500 rpm, 200 rpm and 100 rpm for one hour each. The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard. Example 5:

[0038] 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed evenly with a saturated sodium sulfate solution at a solid-liquid ratio of 1:1, and then subjected to density gradient separation at 80°C with mechanical stirring at 500 rpm, 200 rpm and 100 rpm for one hour each. The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard. Example 6:

[0039] 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed evenly with a saturated sodium sulfate solution at a solid-liquid ratio of 1:2, and then subjected to density gradient separation at 20°C with mechanical stirring at 500 rpm, 200 rpm and 100 rpm for one hour each. The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard. Example 7:

[0040] 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The obtained solid mixture A was mixed with a saturated sodium sulfate solution at a solid-liquid ratio of 1:2, and then subjected to density gradient separation at 80°C with mechanical stirring at 500 rpm for one hour. The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard.

[0041] Comparative Example 500g of tantalum powder mixed salt was subjected to enhanced leaching and separation to obtain a mixed solid A containing sodium fluoride and tantalum pentoxide, and a mixed salt solution A; The resulting solid mixture A was subjected to air separation. The obtained mixed salt solution A is added to a composite defluorinating agent composed of calcium chloride and polyaluminum chloride to remove fluoride until the fluoride ion concentration in the solution meets the standard.

[0042] Please refer to Table 1, which shows the yields of fluorine, chlorine, sodium, potassium, and tantalum pentoxide in Examples 1-7 and the comparative examples, as well as examples of fluoride ion concentrations in the mixed salt solution after fluoride removal: Table 1

[0043] As can be seen from Table 1: In the embodiments of this application, the fluorine recovery rate is relatively high, ranging from approximately 92.17% to 95.91%, indicating that the method of this application has a significant effect on the effective recovery of fluorine.

[0044] In addition to fluorine, sodium, potassium, and chlorine also showed high recovery rates, especially potassium and chlorine, which approached or exceeded 98% in some embodiments, demonstrating the effective separation and recovery capabilities of the present invention for multiple elements.

[0045] The recovery rate of tantalum pentoxide varied considerably among the examples, ranging from a minimum of 11.24% (comparative example) to a maximum of 46.98% (Example 2). This indicates that the choice of physical separation steps has a significant impact on the recovery efficiency of tantalum pentoxide, and the density gradient separation method used in this application can significantly improve the recovery efficiency of tantalum pentoxide compared to air separation.

[0046] The fluoride ion concentration in the treated mixed salt solution is very low, typically around 10. -5 The concentration is on the order of mol / L, meeting stringent environmental emission standards or industrial reuse requirements. For example, Example 3 achieved a minimum value of 0.01*10. -5 mol / L, while other examples remained in a similarly low range.

[0047] Based on the same inventive concept, this application also provides a tantalum powder mixed salt byproduct separation system 200. Please refer to... Figure 2 , Figure 2 This is a structural schematic diagram of the tantalum powder mixed salt byproduct separation system provided in this application embodiment; the tantalum powder mixed salt byproduct separation system 200 includes: Leaching apparatus 201 is used to leach and separate tantalum powder mixed salt to obtain a mixed solid containing sodium fluoride and tantalum pentoxide, and a mixed salt solution whose main component is potassium chloride; Physical separation device 202 is used to physically separate the mixed solids to obtain sodium fluoride solid and tantalum pentoxide solid; The mixed salt solution treatment device 203 is used to defluorinate the mixed salt solution until the fluoride ion concentration in the mixed salt solution meets the preset conditions.

[0048] For the implementation process of the above-mentioned tantalum powder mixed salt by-product separation system 200 and its various devices, please refer to steps S101 to S103 and their optional embodiments, which will not be repeated in this application.

[0049] In summary, this application not only achieves the effective recovery of valuable tantalum pentoxide, but also reduces the environmental impact of waste by effectively recovering elements such as fluorine, sodium, potassium, and chlorine. Furthermore, by optimizing conditions such as temperature and stirring speed, the recovery efficiency of various components can be further improved.

Claims

1. A process for separating a mixed salt by-product from tantalum powder, characterized by, include: The tantalum powder was leached and separated to obtain a mixed solid containing sodium fluoride and tantalum pentoxide, as well as a mixed salt solution whose main component was potassium chloride. The mixed solids are physically separated using a density gradient separation method. This method involves using one or more of the following: sodium sulfate solution, potassium sulfate solution, and potassium fluorosilicate solution as the heavy density liquid. The volume ratio of the heavy density liquid to the weight ratio of the tantalum powder mixed salt is 0.1–15:

1. The reaction temperature is 10–100°C, and the contact time is 0.5–10 hours. The mixed solids are then mechanically stirred after mixing with the heavy density liquid to obtain sodium fluoride solid and tantalum pentoxide solid. The mixed salt solution is treated with a defluorinating agent to remove fluoride until the fluoride ion concentration in the mixed salt solution meets the preset conditions.

2. The process of claim 1 wherein, The leaching and separation of tantalum powder mixed salts yields a mixed solid containing sodium fluoride and tantalum pentoxide. The leaching and separation methods used include enhanced leaching, pressure leaching, reactor leaching, and stirred leaching.

3. The method of claim 1, wherein the tantalum powder mixed salt byproduct is separated by, The volume ratio of the heavy-density liquid to the weight ratio of the tantalum powder mixed salt is 0.6~7.5:1; the reaction temperature is 35~90℃; and the contact time is 0.5~8 hours.

4. The process of claim 1 wherein, The defluorination treatment of the mixed salt solution includes selecting one or at least two of magnesium chloride, polyaluminum chloride, lanthanum nitrate, calcium chloride, and polyacrylamide as defluorinating agents.

5. The method of claim 4, wherein the mixture of the tantalum powder and the salt byproduct is separated by, Also includes: After adding a defluorinating agent, solid-liquid separation is carried out by centrifugation. The centrifugation speed is 1000~8000 rpm, the centrifugation time is 1~10 minutes, and the centrifugation temperature is 10~100℃.

6. The process of claim 5 wherein the process is characterized by, In solid-liquid separation by centrifugation, the centrifugation speed is 3000~7000 rpm; the centrifugation time is 2~8 minutes; and the centrifugation temperature is 30~90℃.

Citation Information

Patent Citations

  • Method for preparing potassium fluotantalate with byproduct produced during reduction preparation of tantalum powder with recovered sodium

    CN102336438A

  • Method for producing compound salts by tantalum metallurgy byproducts

    CN102352444A

  • Method for treating waste compound salt by-products and waste washing water of tantalum powder production by sodium reduction method

    CN109399669A

  • Recovery system for fluorine in tantalum powder by-products

    CN212102961U

  • Method for recovering by-product fluorine-chlorine-sodium-potassium-containing mixed salt in tantalum powder production

    CN120229743A