Modification method and application of recycled concrete aggregate
By pretreatment, physical modification, chemical modification and surface enhancement treatment of recycled concrete aggregate, the problem of rough and poor bonding performance of recycled concrete aggregate is solved, its comprehensive performance is improved, the application scope is expanded and the cost is reduced.
Patent Information
- Application Number
- CN202510504922.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-22
- Publication Date
- 2025-07-25
AI Technical Summary
The recycled concrete aggregate has rough surface, high water absorption, and poor bonding performance with fresh cement slurry, which affects its working performance, mechanical properties and durability, limiting its large-scale application.
Pretreatment, physical modification, chemical modification and surface enhancement treatment are adopted, including crushing and screening, mechanical grinding, heat treatment, acid treatment, alkali treatment, silane coupling agent treatment and calcium dihydrogen phosphate treatment, to form a dense organic-inorganic transition layer to enhance the compatibility and bonding strength of the aggregate and cement-based materials.
It significantly improves the comprehensive performance of recycled aggregates, expands its application range in construction projects, reduces the cost of building materials, realizes efficient recycling and utilization of waste concrete, and protects natural resources.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of recycled concrete aggregates, and relates to a modification method and application of recycled concrete aggregates. Background Art
[0002] In the process of the rapid development of global urbanization and industrialization, the scale of the construction industry continues to expand, and the amount of construction waste generated therefrom is also increasing. According to statistics, the annual construction waste generated in China has exceeded 2 billion tons, and waste concrete accounts for a quite large proportion; processing waste concrete into recycled concrete aggregates for reuse has become a key measure to solve the problem of construction waste accumulation and achieve resource recycling, which can reduce the over-exploitation of natural aggregates and protect the ecological environment.
[0003] However, recycled concrete aggregates have many performance defects, which severely limit their large-scale application; the old cement mortar attached to the surface of recycled aggregates makes the surface of the aggregates rough and uneven, which not only leads to a significant increase in the water absorption of the aggregates, reduces the strength of the aggregates themselves, but also their crushing index is much higher than that of natural aggregates;
[0004] At the same time, the presence of old cement mortar makes the bonding performance between recycled aggregates and fresh cement paste poor, and the interfacial transition zone becomes a weak link in the performance of recycled concrete, greatly affecting the workability, mechanical properties and durability of recycled concrete. Therefore, how to improve the overall performance of recycled concrete is an urgent technical problem to be solved by those skilled in the art. Summary of the Invention
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A modification method for recycled concrete aggregates specifically includes the following detailed steps:
[0007] Pretreatment:
[0008] Crushing and screening: Collect waste concrete, first perform coarse crushing using a jaw crusher to crush it into larger particles; then perform medium crushing using a cone crusher to further reduce the particle size; finally, perform fine screening using a vibrating screen to screen out recycled concrete aggregates with a suitable particle size range according to different engineering requirements;
[0009] Impurity removal: Remove impurities such as wood, plastic, and metal mixed in the recycled aggregates to ensure the purity of the recycled aggregates.
[0010] Physical modification:
[0011] Mechanical grinding: Place the pre-treated recycled aggregate in a planetary ball mill. The grinding media in the ball mill are zirconia balls of different diameters. The mass ratio of large balls (diameter 10 mm), medium balls (diameter 5 mm) and small balls (diameter 3 mm) is 3:4:3. Control the rotation speed of the ball mill within the range of 300 - 400 r / min, and the grinding time is 20 - 30 min.
[0012] During the grinding process, through the synergistic effect of multi-level grinding media, efficient stripping of the old mortar on the surface of the recycled aggregate, optimization of the surface microstructure, and protective grinding of the aggregate particles are achieved. While efficiently removing the old mortar on the surface of the recycled aggregate, the surface microstructure (roughness, specific surface area) is optimized and the strength of the aggregate body is protected, providing convenience for subsequent chemical modification and surface strengthening steps.
[0013] Heating treatment assistance: After mechanical grinding, perform heating treatment on the recycled aggregate. Place the aggregate in an electric resistance furnace and heat it to 400 - 600 °C at a heating rate of 5 °C / min. After holding for 1 - 2 h, cool it to room temperature to complete the heat treatment. During the heating process, the moisture inside the aggregate evaporates, and the water vapor pressure in the microcracks increases, promoting the expansion and healing of some microcracks. At the same time, some unstable mineral components on the surface of the aggregate decompose and recombine, further improving the physical properties of the aggregate and enhancing its strength and stability.
[0014] Chemical modification:
[0015] Acid treatment: Immerse the recycled aggregate after physical modification in a dilute hydrochloric acid solution with a mass fraction of 5% - 10%. The volume ratio of the solution to the aggregate mass is 3:1. During the immersion process, dilute hydrochloric acid reacts chemically with impurities such as calcium carbonate on the surface of the aggregate to form soluble salts and carbon dioxide gas, thereby removing surface impurities. At the same time, tiny pores and grooves are formed on the surface of the aggregate, increasing the accessible surface area. The immersion time is controlled within 1 - 2 h, and stirring is carried out every 30 min during this period to ensure uniform reaction. After acid treatment, rinse the aggregate with a large amount of water until the pH value of the rinse liquid reaches 6 - 7, making the aggregate neutral.
[0016] Alkali treatment: Immerse the aggregate after acid treatment in a sodium hydroxide solution with a mass fraction of 8% - 12%. The volume ratio of the solution to the aggregate mass is also 3:1. Sodium hydroxide reacts with components such as silica and alumina on the surface of the aggregate to form cementitious aluminosilicate products. These products fill the pores and microcracks on the surface of the aggregate, improving the density and strength of the aggregate surface. The immersion time is 1.5 - 2.5 h, and the solution temperature is maintained at 40 - 50 °C during the immersion process to promote the reaction. After alkali treatment, rinse the aggregate with water again until it is neutral and dry it in an oven at 105 °C.
[0017] Silane coupling agent treatment: Immerse the dried recycled aggregate in an ethanol solution of silane coupling agent with a mass fraction of 2%-5%. The ethanol solution of silane coupling agent needs to be hydrolyzed and activated in advance. Specifically, add a small amount of water (the mass ratio of water to silane coupling agent is 1:10) to the solution, stir evenly and then let it stand for 30 min to cause the alkoxy groups in the silane coupling agent molecules to undergo hydrolysis reaction to generate silanol groups; the soaking time is 30-60 min to allow the silane coupling agent to be fully adsorbed on the surface of the aggregate; after taking out, place the aggregate in a blast drying oven and dry it at 60-80 °C for 2-4 h to cause the silane coupling agent to undergo polycondensation reaction on the surface of the aggregate, forming a dense organic-inorganic transition layer, significantly enhancing the compatibility and bonding strength between the aggregate and the cement-based material.
[0018] Surface strengthening treatment: Immerse the chemically modified recycled aggregate in a calcium dihydrogen phosphate solution with a concentration of 0.1-0.3 mol / L, and the volume ratio of the solution to the mass of the aggregate is 4:1; during the soaking process, calcium dihydrogen phosphate reacts with calcium ions and hydroxide ions on the surface of the aggregate to generate calcium phosphate-based cementitious substances, and these substances gradually deposit and crystallize on the surface of the aggregate to form a hard surface strengthening layer. The soaking time is 4-6 h. After taking out, place the aggregate in a curing room with a relative humidity of 90%-95% and a temperature of 20±2 °C for natural curing for 3-5 days to make the surface strengthening layer fully hardened, further improving the surface strength and wear resistance of the aggregate.
[0019] As a further solution of the present invention: As a further solution of the present invention: It also includes between physical modification and chemical modification: a surface treatment step, which includes:
[0020] Surface activation: Prepare a sodium silicate (water glass) solution with a modulus of 1.5-2.5 and a concentration of 5%-10%, immerse the physically modified recycled aggregate in it, and at the same time use ultrasonic wave with a frequency of 40 kHz and a power of 300 W for auxiliary treatment for 10-30 min; the sodium silicate solution reacts with the surface of the aggregate under ultrasonic wave assistance, which can effectively remove surface impurities and weak bonding layers;
[0021] At the same time, an active layer with silanol groups is formed on the surface of the aggregate; the silanol groups have strong chemical activity and can react with the silane coupling agent used in the subsequent chemical modification process, thereby enhancing the bonding performance between the aggregate and the cement paste.
[0022] Microcrack repair: Prepare a repair fluid, which contains 1%-3% of nano-silica (particle size 10-30 nm), 0.5%-2% of silane coupling agent (KH-550 or KH-570), 0.1%-0.3% of dispersant (polycarboxylate), and the balance is water; Place the surface-activated aggregate in a vacuum reactor, first evacuate to -0.1 MPa and maintain for 10 min, then inject the repair fluid, and pressurize to 0.1-0.5 MPa and maintain for 1-2 h. This step repairs the microcracks that may occur during the physical modification process and the internal defects existing in the aggregate itself.
[0023] Nano-silica has an extremely small particle size and a large specific surface area, which can fill into microcracks and play a role in physical filling and strengthening; The silane coupling agent can form a chemical bond between nano-silica and the aggregate matrix, further enhancing the repair effect.
[0024] As a further scheme of the present invention: In the surface activation step, the modulus of the sodium silicate solution is 1.8-2.2, the concentration is 6%-8%, and the ultrasonic treatment time is 15-25 min; Increasing the active sites on the aggregate surface, improving the bonding strength with the cement paste, can more effectively improve the treatment effect and enhance the product performance.
[0025] As a further scheme of the present invention: In the microcrack repair step, the nano-silica content is 1.5%-2.5%, the silane coupling agent content is 1%-1.5%, the dispersant content is 0.15%-0.25%, and the vacuum reactor is pressurized to 0.2-0.4 MPa and maintained for 1.2-1.8 h; It can effectively improve the compactness and strength of the aggregate, and reduce the porosity and water absorption of the aggregate.
[0026] The present invention also provides the application of the modified recycled concrete aggregate prepared by the above modification method in the preparation of recycled concrete, the production of concrete products, and the laying of road base materials.
[0027] When preparing recycled concrete, the replacement rate of the modified recycled aggregate can be reasonably adjusted according to different engineering requirements;
[0028] In non-load-bearing structures, the replacement rate of the modified recycled aggregate can reach 100%. Such as the infill walls of buildings, partitions inside buildings, etc. Using the recycled concrete prepared with the modified recycled aggregate can significantly reduce costs while meeting the structural requirements, realizing the high-value utilization of waste concrete.
[0029] Load-bearing structure application: In load-bearing structures, the replacement rate of modified recycled aggregates can be controlled between 30% and 70%. Through reasonable mix design, it can be used in structures such as beams, slabs, and columns of high-rise buildings, with good workability. Its 28-day compressive strength is increased by 25% - 40% compared to recycled concrete prepared with unmodified aggregates. The impermeability grade can reach P8 - P10, and the frost resistance grade reaches F200 - F300, fully meeting the mechanical properties and durability requirements of load-bearing structures.
[0030] Production of concrete products: When used to prepare concrete products, modified recycled aggregates can improve the dimensional stability, crack resistance, and durability of the products. For example, for concrete blocks, after using modified recycled aggregates, their compressive strength is significantly improved, reaching 15 MPa or even higher, the water absorption rate is reduced, and the frost resistance is good, meeting the usage requirements of building wall materials, while reducing production costs and improving production efficiency.
[0031] Laying of road base materials: When applied in road base materials, modified recycled aggregates can replace natural aggregates 100% and be used in combination with cementitious materials (such as cement: fly ash = 7:3). This significantly improves the bearing capacity of the road base, enhances the anti-deformation ability, effectively extends the service life of the road, while reducing the road construction cost, reducing the dependence on natural stone materials, and having good economic and environmental benefits.
[0032] Advantages of the present invention: It realizes the efficient recycling of waste concrete, reduces the environmental pollution caused by construction waste, reduces the extraction amount of natural aggregates, and protects natural resources. At the same time, by using a synergistic modification method of physical, chemical, and surface strengthening treatments, each modification step cooperates and promotes each other. Physical modification creates good surface conditions for chemical modification, chemical modification further optimizes the surface composition and structure of the aggregates, and surface strengthening treatment ultimately improves the surface properties of the aggregates, effectively solving various problems existing in recycled aggregates and comprehensively improving the comprehensive performance of recycled aggregates. It expands the application range in construction projects, reduces the cost of building materials, and has significant economic and environmental benefits. Specific implementation manners
[0033] The technical solutions in the embodiments of the present application will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. It should be understood that the present application is not limited by the exemplary embodiments disclosed herein. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative efforts shall fall within the protection scope of the present application.
[0034] Example 1, A method for modifying recycled concrete aggregates in this example includes the following steps:
[0035] Pretreatment: Collect waste concrete, first crush it with a jaw crusher to a particle size less than 50 mm, then crush it with a cone crusher to a particle size less than 20 mm, and finally use a vibrating screen to screen out recycled concrete aggregates with a particle size of 5 - 20 mm; remove impurities in the aggregates to obtain pure recycled aggregates.
[0036] Physical modification: Put the pretreated recycled aggregates into a planetary ball mill, add zirconia grinding media, set the rotation speed of the ball mill to 300 r / min, and grind for 20 min. After grinding, put the aggregates into an electric resistance furnace, heat them to 400 °C at a heating rate of 5 °C / min, keep them at this temperature for 1 h, and then cool them down with the furnace.
[0037] Chemical modification:
[0038] Acid-base treatment: Immerse the physically modified aggregates in a 5% dilute hydrochloric acid solution, with the volume ratio of the solution to the aggregate mass being 3:1, soak for 1 h and stir every 30 min; after acid treatment, rinse with clean water until neutral, then immerse the aggregates in an 8% sodium hydroxide solution, keep the solution temperature at 40 °C, and soak for 1.5 h; after alkali treatment, rinse again until neutral, and dry in an oven at 105 °C to constant weight.
[0039] Silane coupling agent treatment: Hydrolyze and activate a 2% silane coupling agent ethanol solution, add a small amount of water (the mass ratio of water to silane coupling agent is 1:10), stir evenly and let it stand for 30 min; immerse the dried aggregates in this solution for 30 min, take them out and dry in a forced-air drying oven at 60 °C for 2 h.
[0040] Surface strengthening treatment: Immerse the chemically modified aggregates in a 0.1 mol / L calcium dihydrogen phosphate solution, with the volume ratio of the solution to the aggregate mass being 4:1, soak for 4 h; take them out and place them in a curing room with a relative humidity of 90% and a temperature of 20 °C, and cure naturally for 3 days to obtain modified recycled concrete aggregates.
[0041] Mix the above modified recycled aggregates with P·O42.5 cement, medium sand, water and water reducer (water reduction rate 20%) at a ratio of 50% natural aggregate replacement rate to prepare recycled concrete, and the mix ratio is cement:sand:modified recycled aggregates:water:water reducer = 350:650:800:180:7.
[0042] After testing, the slump of this recycled concrete is 180 mm, and the slump loss in 1 h is 15 mm; the 28-day compressive strength reaches 35 MPa, the impermeability grade is P8, and the frost resistance grade is F200. Compared with the recycled concrete prepared with unmodified aggregates, the compressive strength is increased by 30%, and the impermeability and frost resistance are also significantly improved.
[0043] Example 2
[0044] Pretreatment: Similar to Example 1, recycled concrete aggregates with a particle size of 5 - 20 mm were obtained and impurities were removed. Physical modification: The recycled aggregates were placed in a planetary ball mill, the rotation speed was adjusted to 350 r / min, and grinding was carried out for 25 min; after grinding, they were heated to 500 °C at a heating rate of 5 °C / min, held for 1.5 h, and then cooled in the furnace.
[0045] Chemical modification:
[0046] Acid - base treatment: The physically modified aggregates were immersed in a 8% by mass dilute hydrochloric acid solution for 1.5 h, rinsed with clean water until neutral, and then immersed in a 10% by mass sodium hydroxide solution with the solution temperature maintained at 45 °C for 2 h; after alkali treatment, they were rinsed to neutral and dried.
[0047] Silane coupling agent treatment: A 3% by mass silane coupling agent ethanol solution was hydrolyzed and activated, and after standing for 30 min, the dried aggregates were immersed in it for 45 min, taken out and dried at 70 °C for 3 h.
[0048] Surface strengthening treatment: The chemically modified aggregates were immersed in a 0.2 mol / L calcium dihydrogen phosphate solution for 5 h, taken out and naturally cured in a curing room with a relative humidity of 92% and a temperature of 20 °C for 4 days to obtain modified recycled concrete aggregates.
[0049] Using the modified recycled aggregates, recycled concrete was prepared with a natural aggregate replacement rate of 70%, and the mix ratio was cement:sand:modified recycled aggregates:water:water - reducing agent = 380:620:980:175:7.6.
[0050] After testing, the slump of the recycled concrete was 175 mm, and the slump loss after 1 h was 12 mm; the 28 - day compressive strength reached 38 MPa, the impermeability grade was P9, and the frost - resistance grade was F250, which was superior to the concrete prepared with unmodified aggregates in terms of workability, mechanical properties and durability.
[0051] Example 3
[0052] Pretreatment: The same as in Example 1, qualified recycled concrete aggregates were prepared.
[0053] Physical modification: The rotation speed of the ball mill was set to 400 r / min, and the recycled aggregates were ground for 30 min; after grinding, they were heated to 600 °C, held for 2 h, and then cooled in the furnace.
[0054] Chemical modification:
[0055] Acid-base treatment: Immerse the physically modified aggregate in a 10% by mass dilute hydrochloric acid solution for 2 h. After rinsing until neutral, immerse it in a 12% by mass sodium hydroxide solution. Keep the solution temperature at 50 °C and immerse for 2.5 h, then rinse and dry.
[0056] Silane coupling agent treatment: After hydrolyzing and activating a 5% by mass ethanol solution of silane coupling agent, immerse the dry aggregate in it for 60 min. After taking it out, dry it at 80 °C for 4 h.
[0057] Surface strengthening treatment: Immerse the chemically modified aggregate in a 0.3 mol / L calcium dihydrogen phosphate solution for 6 h. After taking it out, cure it naturally in a curing room with a relative humidity of 95% and a temperature of 20 °C for 5 days to obtain the modified recycled concrete aggregate.
[0058] Use this modified recycled aggregate to completely replace natural aggregate to prepare recycled concrete. The mix ratio is cement:sand:modified recycled aggregate:water:water reducing agent = 400:600:1200:170:8.
[0059] After testing, the slump of the concrete is 170 mm, and the slump loss in 1 h is 10 mm; the 28-day compressive strength reaches 40 MPa, the impermeability grade is P10, and the frost resistance grade is F300. All performance indicators meet the requirements of building engineering and can be widely used in general building structures.
[0060] Performance comparison of recycled aggregates before and after modification in each example:
[0061]
[0062]
[0063] It can be seen from the comparison of multiple examples that the performance of the modified recycled aggregate is significantly better than that of the unmodified recycled aggregate. In Examples 1-3, the recycled aggregates prepared from waste concrete have all undergone the pretreatment, physical modification, chemical modification and surface strengthening treatment of the present invention.
[0064] When preparing recycled concrete, the workability of the concrete prepared with unmodified recycled aggregate is poor, the slump loss is large, the 28-day compressive strength is low, and the impermeability and frost resistance grades are also low.
[0065] However, the performance of the concrete prepared with the modified recycled aggregate has been greatly improved; taking Example 1 as an example, the slump of the concrete prepared with the modified recycled aggregate is 180 mm, and the slump loss in 1 h is 15 mm; the 28-day compressive strength reaches 35 MPa, which is 30% higher than that of the unmodified one, the impermeability grade is P8, and the frost resistance grade is F200.
[0066] The foregoing description of the disclosed embodiments enables those skilled in the art to practice or use the present application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Thus, the present application is not intended to be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for modifying recycled concrete aggregates, characterized in that, It includes the following steps: Pretreatment: Crushing and screening waste concrete to obtain recycled concrete aggregates with appropriate particle sizes, and removing the waste impurities mixed therein; Physical modification: Mechanically grinding the pretreated recycled aggregates, and placing them in a ball mill for grinding; controlling the rotation speed of the ball mill at 300 - 400 r / min and the grinding time at 20 - 30 min; then putting the aggregates into an electric resistance furnace, heating them to 400 - 600 °C at a heating rate of 5 °C / min, keeping them warm for 1 - 2 h, and then cooling them to room temperature with the furnace; Chemical modification: Sequentially subjecting the recycled aggregates after physical modification to acid-base treatment and silane coupling agent treatment; Among them, the acid-base treatment is to soak the aggregates in a dilute hydrochloric acid solution with a mass fraction of 5% - 10% for 1 - 2 h, rinse them with clear water until neutral, then soak them in a sodium hydroxide solution with a mass fraction of 8% - 12% for 1.5 - 2.5 h, and rinse them again until neutral and dry; The silane coupling agent treatment is to soak the dried aggregates in a hydrolyzed and activated ethanol solution of silane coupling agent with a mass fraction of 2% - 5% for 30 - 60 min, take them out and dry them in an environment of 60 - 80 °C for 2 - 4 h; Surface strengthening treatment: Immersing the recycled aggregates after chemical modification into a calcium dihydrogen phosphate solution with a concentration of 0.1 - 0.3 mol / L for 4 - 6 h, taking them out and naturally curing them in a curing room with a relative humidity of 90% - 95% and a temperature of 20 ± 2 °C for 3 - 5 days to obtain granular modified recycled aggregates.
2. The modified method of recycled concrete aggregate according to claim 1, characterized in that In the physical modification treatment, the grinding media in the ball mill are zirconia balls with different diameters. The diameters of the large balls, medium balls and small balls are 10 mm, 5 mm and 3 mm respectively, and the mass ratio of the large balls, medium balls and small balls is 3:4:
3.
3. A method for modifying recycled concrete aggregate according to claim 1, characterized in that, The hydrolysis activation treatment of the silane coupling agent ethanol solution is to add a small amount of water to the solution. The mass ratio of water to the silane coupling agent is 1:10, stir evenly and then let it stand for 30 min.
4. A method for modifying recycled concrete aggregates according to claim 1, characterized in that, Between the physical modification and the chemical modification, it also includes: a surface treatment step, which includes: Surface activation: Preparing a sodium silicate (water glass) solution with a modulus of 1.5 - 2.5 and a concentration of 5% - 10%, soaking the recycled aggregates after physical modification therein, and simultaneously using ultrasonic assistance with a frequency of 40 kHz and a power of 300 W for 10 - 30 min. Microcrack repair: Preparing a repair solution, which contains 1% - 3% of nano-silica (particle size 10 - 30 nm), 0.5% - 2% of silane coupling agent (KH-550 or KH-570), 0.1% - 0.3% of dispersant (polycarboxylate), and the balance is water; placing the aggregates after surface activation in a vacuum reactor, first evacuating to -0.1 MPa and maintaining for 10 min, then injecting the repair solution, pressurizing to 0.1 - 0.5 MPa, and maintaining for 1 - 2 h.
5. A method for modifying recycled concrete aggregates according to claim 4, characterized in that, In the surface activation step, the modulus of the sodium silicate solution is 1.8 - 2.2, the concentration is 6% - 8%, and the ultrasonic treatment time is 15 - 25 min.
6. The modified method of recycled concrete aggregate according to claim 4, wherein In the microcrack repair step, the content of nano-silica is 1.5%-2.5%, the content of silane coupling agent is 1%-1.5%, the content of dispersant is 0.15%-0.25%, the pressure in the vacuum reactor is increased to 0.2-0.4 MPa and maintained for 1.2-1.8 h.
7. An application of recycled concrete aggregate, characterized in that, The application work of the recycled aggregate for the modification method of a recycled concrete aggregate according to any one of claims 1-6 above. The modified recycled aggregate can be used in the preparation of recycled concrete, the production of concrete products, and the laying of road base materials.
Citation Information
Cited By
High-performance green cement-based grouting material and construction method
CN121872733A
High-performance green cement-based grouting material and construction method
CN121872733B