Base material, method for manufacturing same, and wiring board using same
By adopting multiple thin film laminated structures in the substrate of the wiring substrate, low transmission loss and stable thermal expansion control in the high-frequency region are achieved, and the problem of insufficient electrical and physical characteristics of fluororesin substrates in the prior art is solved, and a substrate and wiring substrate with stable high-frequency characteristics and thermal expansion are provided.
Patent Information
- Application Number
- CN202380089706.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-28
- Filing Date
- 2023-12-25
- Publication Date
- 2025-08-05
AI Technical Summary
The prior art is difficult to maintain the excellent electrical characteristics of the fluororesin while stably providing the high physical characteristics required by the wiring substrate, especially in terms of suppression of transmission losses and thermal expansion control in high-frequency regions.
A plurality of thin film laminated structures are adopted, wherein the thin film has anisotropy of linear expansion coefficient in the extension surface of the substrate. The substrate is formed by cross-lamination to ensure the main component of the fluororesin. The linear expansion coefficient of the thin film satisfies a specific relationship in the range of 30°C to 250°C to control the thermal expansion characteristics.
It realizes low transmission loss and stable thermal expansion control in high-frequency regions, maintains excellent electrical characteristics of fluororesin, and improves the uniformity and reliability of physical characteristics of substrates and wiring substrates.
Smart Images

Figure CN120435387A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a base material and a wiring board having excellent electrical and physical properties. Background Art
[0002] In recent years, the volume of information communication has continued to increase. As a solution to increasing communication speeds, there is a demand for higher frequencies in transmission signals within communication devices. Consequently, minimizing transmission loss in the high-frequency range has become crucial in wiring boards used in these communication devices.
[0003] To minimize transmission loss, it is crucial to reduce the relative dielectric constant εr and dielectric loss tangent tanδ of the dielectric layer of a wiring board. Therefore, the use of fluororesins such as polytetrafluoroethylene (PTFE) as dielectric layer materials is being studied. These materials are not only thermally and / or chemically stable but also naturally possess excellent electrical properties.
[0004] Physical properties are also important for wiring boards and the base materials they are made of. Wiring boards are often required to withstand low temperatures of -30°C or below and heat resistance exceeding 260°C during both their manufacturing and subsequent use. In some cases, flexibility, such as flexibility, is also required in addition to a certain elastic modulus.
[0005] Furthermore, substrates must be formed with high precision on both the surface and interior of micrometer-level patterns. Warping associated with temperature fluctuations in thin substrates can sometimes cause serious issues with productivity and / or reliability. Therefore, substrates used as wiring boards are required to exhibit thermal expansion characteristics with minimal in-plane distribution over a wide temperature range.
[0006] However, in general, the linear expansion coefficient of fluororesins cannot be said to be sufficiently small to meet the above-mentioned high requirements.
[0007] In this regard, by combining fluororesin with other materials having a smaller linear expansion coefficient than fluororesin, attempts can be made to control the thermal expansion of wiring boards having fluororesin dielectric layers. Examples of thermal expansion control materials that achieve this effect of reducing thermal expansion include woven fabrics, non-woven fabrics, particles, hollow particles, fibers, and tubes made of materials such as glass and ceramics.
[0008] Patent document 1 discloses a fluororesin substrate containing hollow glass beads in a dielectric layer. In a substrate having a glass cloth impregnated with fluororesin as a dielectric layer, the high-frequency characteristics are reduced due to the large relative dielectric constant ε of the glass cloth. To address this problem, the relative dielectric constant can be suppressed by hollow glass beads. However, when the amount of beads added is too small, the occurrence of warping cannot be prevented. For example, the embodiment discloses a mixing ratio (mass ratio) of fluororesin: hollow glass beads = 100:30. In addition, even compared with a conductor pattern formed by setting the 50% particle size of the glass beads to 16μm or 30μm, the size is of the same degree. Therefore, there are problems such as deterioration of electrical properties caused by the glass added to the substrate, increase in volume, unevenness of physical properties depending on the distribution of beads, and deterioration of processability.
[0009] Patent Document 2 discloses a printed wiring board comprising a dielectric layer having a porous layer primarily composed of fluororesin on one side, and a conductive pattern laminated on at least one side of the dielectric layer. The dielectric layer of this printed wiring board includes a reinforcing layer comprising glass cloth on the other side of the porous layer, thereby reducing warping, deformation, linear expansion changes, and the like. However, this printed wiring board also suffers from problems such as deterioration of electrical properties, increased volume, and uneven physical properties caused by the reinforcing layer material, such as glass cloth.
[0010] For example, Patent Document 3 discloses a composite structure formed by at least partially filling the pores of a porous polymer membrane composed of stretched PTFE with a resin such as a metal, metalloid, ceramic, or polymer material. The composite structure exhibits extremely high resistance to breakage and damage. However, such a structure is difficult to achieve a sufficiently low linear expansion coefficient. Furthermore, the absorption or filling of the other material in the pores can lead to deterioration in thermal expansion characteristics and / or electrical properties.
[0011] Thus, in attempts to control the physical properties of a fluororesin substrate by compositeing it with a structure or organization composed of materials other than fluororesin, the composite material also has a trade-off relationship in which the physical properties are favorable on the one hand but the electrical properties are disadvantageous on the other. This makes it difficult to obtain a wiring substrate that fully balances the physical properties required of the substrate or base material with the excellent electrical properties naturally possessed by fluororesin.
[0012] In this regard, the inventors of the present application provide a fluororesin film in patent document 4, which has an endothermic peak in a melting curve at a specified position and has a specific relationship between film thickness and haze value. For this fluororesin film, the relative dielectric constant at 30 GHz is less than 2.1, and the dielectric loss tangent at 30 GHz is less than 0.001. Moreover, when the linear expansion coefficient of the film in the XY direction at 30°C to 250°C (hereinafter referred to as CTE) is less than 100 ppm / °C, the fluororesin film has both electrical and physical properties in a high dimension. However, there is still room for further improvement in obtaining a substrate or wiring substrate that stably possesses electrical and physical properties.
[0013] Prior art literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Laid-Open No. 2013-201344
[0016] Patent Document 2: Japanese Patent Application Laid-Open No. 2016-46433
[0017] Patent Document 3: Japanese Patent Application No. 2006-504848
[0018] Patent Document 4: International Publication No. WO2022 / 071237A1 Summary of the Invention
[0019] Problems to be solved by the invention
[0020] The technical solution described in the present application is made in view of such circumstances, and an object thereof is to provide a base material and a wiring board that maintain the excellent electrical properties of fluororesin and stably possess the high physical properties required of the base material.
[0021] Solutions for solving problems
[0022] A substrate according to one embodiment of the present invention is a substrate for a dielectric layer of a wiring board, wherein the substrate comprises a fluororesin content of 90% by weight or greater, the substrate comprising a first film and a second film formed on the first film, the first film and the second film each having a first direction and a second direction perpendicular to the first direction within an extended surface of the substrate, and wherein a linear expansion coefficient in the first direction within a range of 30°C to 250°C is defined as CTE. S (ppm / °C), and the linear expansion coefficient in the second direction is set as CTE L (ppm / ℃), respectively meeting CTE S <CTE LThe anisotropy of the linear expansion coefficient in this relational expression is such that the first direction of the first film and the first direction of the second film intersect with each other in a plan view of the substrate.
[0023] In addition, another embodiment of the present invention is a substrate used as a dielectric layer of a wiring board, characterized in that the substrate is formed by laminating a plurality of thin films mainly composed of fluororesin, wherein the plurality of thin films have a first direction and a second direction perpendicular to the first direction within an extension plane of the substrate, and a linear expansion coefficient in the first direction within a range of 30°C to 250°C is defined as CTE. S (ppm / °C), and the linear expansion coefficient in the second direction is set as CTE L (ppm / ℃), respectively meeting CTE S / CTE L The plurality of films include a first film and a second film, which are stacked such that the first direction of the first film and the first direction of the second film intersect each other when viewed from above the substrate.
[0024] In addition, another embodiment of the present invention is a substrate for a dielectric layer of a wiring board, characterized in that the substrate includes a first film and a second film formed on the first film, the first film and the second film both having a fluororesin as a main component and having anisotropy in the linear expansion coefficient, the first film and the second film being stacked in such a manner that the direction of the anisotropy of the linear expansion coefficient of the first film intersects the direction of the anisotropy of the linear expansion coefficient of the second film when the substrate is viewed from above, the substrate having a first direction of the substrate and a second direction of the substrate perpendicular to the first direction of the substrate within an extended plane of the substrate, and the linear expansion coefficient of the substrate in the first direction in the range of 30°C to 250°C is defined as CTE. D1 (ppm / °C), and the linear expansion coefficient of the substrate in the second direction is set as CTE D2 (ppm / ℃), satisfying 0.7<CTE D1 / CTE D2 <1.3.
[0025] In addition, another embodiment of the present invention is a substrate used as a dielectric layer of a wiring board, characterized in that the substrate includes a first film containing a fluororesin as a main component and a second film formed on the first film and containing a fluororesin as a main component, the first film and the second film having the same chemical composition, and the difference between the refractive index of the first film and the refractive index of the second film in an observation plane on any cross-section of the substrate perpendicular to the substrate surface is 0.01 or more.
[0026] Furthermore, a method for manufacturing a substrate according to one embodiment of the present invention is a method for manufacturing a substrate for a dielectric layer of a wiring board, characterized in that the method comprises: preparing a plurality of films having a fluororesin as a main component, laminating the plurality of films to form a substrate, wherein the plurality of films having the fluororesin as a main component each have a first direction and a second direction perpendicular to the first direction within an extension plane of the plurality of films, and wherein the linear expansion coefficient in the first direction in a range of 30° C. to 250° C. is set as CTE. S (ppm / °C), and the linear expansion coefficient in the second direction is set as CTE L (ppm / °C), the first film and the second film have a CTE that satisfies S / CTE L The anisotropy of the linear expansion coefficient of the relationship of <0.5, and stacking the plurality of films to form a substrate includes stacking the plurality of films so that the first direction of the first film and the first direction of the second film intersect with each other in a plan view of the substrate.
[0027] Furthermore, a wiring board according to one aspect of the present invention is characterized by including any of the above-mentioned base materials and a conductive pattern formed on the base material.
[0028] According to these base materials and wiring boards, the excellent electrical properties of the fluororesin are maintained, and the high physical properties required of the base materials are stably provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram showing a substrate according to the first embodiment of the present invention. Figure 1 (a) is a top view of the substrate observed from above, Figure 1 (b) is a cross-sectional view of the substrate viewed from the transverse direction.
[0030] Figure 2 It is a schematic diagram showing a substrate according to a second embodiment of the present invention, and is a cross-sectional view of the substrate as viewed from the transverse direction.
[0031] Figure 3 Schematic diagram showing a substrate according to a third embodiment of the present invention, and a cross-sectional view of the substrate as viewed from the transverse direction.
[0032] Figure 4 This is a schematic diagram showing one embodiment of the wiring substrate of the present invention. Figure 4 (a) is a top view of the substrate observed from above, Figure 4 (b) is a cross-sectional view of the substrate viewed from the transverse direction.
[0033] Figure 5 This is a diagram for explaining an example of the production process of the substrate of the present invention.
[0034] Figure 6 This is a graph showing the relationship between the calculated linear expansion coefficient and the measured linear expansion coefficient of various substrates composed of different films. DETAILED DESCRIPTION
[0035] The following describes embodiments of a substrate and a method for manufacturing the substrate, as well as a wiring board having the substrate as a dielectric layer, according to the technical solutions described in the claims of this application. The embodiments described below do not limit the technical solutions of the claims. Furthermore, not all combinations of features described in the embodiments are essential to the solution provided by the invention. Furthermore, various embodiments described in the various embodiments and examples may be freely combined without detracting from the technical significance of the present invention.
[0036] The substrate of the invention recited in the claims of the present application and a plurality of thin films containing a fluororesin as a main component and having anisotropic linear expansion coefficients are laminated such that the anisotropies of the linear expansion coefficients of the plurality of thin films intersect.
[0037] By having such a configuration, a substrate is provided which maintains excellent electrical properties and has high physical properties required of a substrate.
[0038] (First embodiment)
[0039] Figure 1 Schematic diagram of a substrate 100 according to the first embodiment of the present invention. Figure 1 (a) is a schematic diagram obtained by observing the substrate surface of the substrate 100 from vertically above. Figure 1 (b) is a schematic diagram showing a cross section of the substrate 100 observed from the lateral direction of the substrate. Figure 1 As shown in (b), the substrate 100 includes a layer composed of a plurality of thin films. The substrate 100 of this embodiment includes at least a thin film 110 and a thin film 120, and the substrate 100 is configured as a substrate in which these thin films are stacked.
[0040] Preferably, the film 120 is formed directly on the film 110. That is, the films are bonded in contact with each other without an adhesive layer interposed therebetween. In this case, the bonding surface becomes the interface 130 shared by the surfaces of the two films.
[0041] These films all contain fluororesin as their primary component. "Primary component" here refers to the component that accounts for the largest amount of the composition, and this applies to the following descriptions unless otherwise specified. From the perspective of electrical properties, the proportion of fluororesin in the film is preferably 90% by weight or greater, more preferably 95% by weight or greater, and particularly preferably 99.5% by weight or greater.
[0042] Fluororesin can be composed primarily of polytetrafluoroethylene (hereinafter, PTFE). PTFE can be a homopolymer of tetrafluoroethylene (hereinafter, TFE) or a modified PTFE containing a small amount of other monomers. Examples of the small amount of monomers other than TFE contained in modified PTFE include chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and perfluoroalkyl vinyl ether (PPVE). These monomers may be present alone or in combination.
[0043] From the viewpoint of controlling the linear expansion coefficient, a homopolymer of TFE is preferred. Note that in this specification, thermal expansion is used to mean at least one of linear expansion in which the length of a substance changes with temperature changes and volume expansion in which the volume of a substance changes.
[0044] These films have anisotropy of linear expansion coefficient. That is, in the extension plane of the film (the plane parallel to the XY plane in the figure), these films have a small CTE direction and a large CTE direction perpendicular to the small CTE direction. The linear expansion coefficient CTE of the film in the small CTE direction is S The linear expansion coefficient CTE of the film in the direction of the larger CTE is suppressed L Small.
[0045] In this embodiment, CTE S Divide by CTE L The obtained value (hereinafter referred to as CTE S / CTE L ) is less than 0.5.
[0046] The anisotropy of the linear expansion coefficient can also be greater, and the specific CTE of at least one of the multiple films of the substrate 100 is S / CTE L It is preferably less than 0.25, more preferably less than 0.1, and particularly preferably less than 0.
[0047] It should be noted that the linear expansion coefficient refers to the ratio of dimensional change per 1°C temperature change. In this specification, unless otherwise specified, it represents the value obtained by dividing the length change rate (ppm) when the temperature is increased from 30°C to 250°C by the change temperature of 220°C (unit: ppm / °C).
[0048] The anisotropy of the linear expansion coefficient of the film can also be specified by the difference. L Subtract the linear expansion coefficient CTE of the film in the direction of small CTE S The obtained value (hereinafter referred to as the difference CTE L -CTE S) can also be greater than 50ppm / ℃. The linear expansion coefficient can also have a greater anisotropy, and the difference CTE of at least one of the multiple films of the substrate 100 is L -CTE S It can be greater than 80ppm / ℃, greater than 120ppm / ℃, and even greater than 140ppm / ℃.
[0049] In the substrate 100 , the direction of the anisotropy of the linear expansion coefficient in the extended surface of the substrate of the film 110 and the direction of the anisotropy of the linear expansion coefficient in the extended surface of the substrate of the film 120 are arranged to intersect with each other.
[0050] exist Figure 1 In (a), for the film 110 of this embodiment, the left-right direction of the paper (i.e., the X direction of the arrow in the figure) is the small CTE direction of the film 110, and the up-down direction of the paper (i.e., the Y direction in the figure) is the large CTE direction of the film 110. In contrast, for the film 120, the up-down direction of the paper is the small CTE direction, and the left-right direction of the paper is the large CTE direction. That is, the film 120 is stacked in such a way that the small CTE direction of the film 120 intersects the small CTE direction of the film 110. When the smaller of the angles formed by two straight lines of the small CTE direction of the film 110 and the small CTE direction of the film 120 is set as the angle between the small CTE direction of the film 110 and the small CTE direction of the film 120, the angle of the angle can be greater than 45 degrees, greater than 60 degrees, or greater than 80 degrees. In this embodiment, the angle between the small CTE direction of the film 110 and the small CTE direction of the film 120 is approximately 90 degrees. It should be noted that, in this specification, "approximately 90 degrees" and "approximately perpendicular" are not limited to the mathematical 90 degrees, and may include, for example, an error of ±5 degrees caused by manufacturing inequalities. Similarly, in this specification, "approximately parallel" may also include an error of ±5 degrees relative to the geometrically absolutely parallel direction.
[0051] In addition, the paired films whose anisotropic directions intersect with each other among the plurality of films of the substrate 100 can be the films having greater anisotropy as described above. S / CTE L and / or poor CTE L -CTE S .
[0052] The substrate 100 of this embodiment maintains the excellent electrical properties of fluororesin and stably possesses the physical properties required of a substrate. The reasons why the substrate 100 possesses such advantageous properties are described below.
[0053] Typical crystalline polymers consist of nanometer-sized crystalline portions and randomly arranged amorphous portions. Applying shear forces, for example, to these constituent molecules can elongate the molecular chains in the crystalline and amorphous portions, creating a nearly linear molecular structure. It is believed that the linear expansion coefficient decreases in the direction in which these molecules are elongated. Therefore, it is believed that by controlling the shape of the polymers that make up a film, even with the same chemical composition, a film with a suppressed linear expansion coefficient can be obtained.
[0054] Methods for achieving this linear molecular state include extrusion, rolling, and / or stretching of polymers. When these methods are used to elongate the shape of the material being processed in a certain direction, the molecular crystals constituting the material also approach an arrangement stretched in the same direction. Hereinafter, the direction in which the polymer constituting the material is elongated toward a specific direction is referred to as orientation. It is believed that for such oriented materials, the higher the degree of orientation, i.e., the more molecules are stretched in a specific direction, the smaller the linear expansion coefficient in that specific direction is suppressed.
[0055] In particular, it is known that some resins, such as fluororesins, can be stretched at temperatures below their crystalline melting point to form a unique microporous structure composed of nodes and fibrils. Appropriate combinations of extrusion, rolling, and the aforementioned stretching methods are preferred for producing highly oriented fibrous or film-like resin materials. The resulting structure, characterized by a unique microstructure composed of nodes and fibrils, obtained by stretching PTFE is known as expanded PTFE, stretched PTFE, or expanded PTFE, and is widely used in applications such as clothing.
[0056] Furthermore, in the manufacture of wiring boards, fine patterns are typically formed on a panel or roll, which is an assembly of multiple unit boards. This is then cut into individual unit boards. Therefore, it is believed that controlling the thermal expansion of the substrate material used for wiring boards, rather than macroscopically controlling the thermal expansion of the substrate itself, is most effectively controlling the thermal expansion of each region within the substrate's surface to be as isotropic and uniform as possible.
[0057] However, simply elongating the molecules and imparting orientation to the material through extrusion, rolling, or stretching is not sufficient to consistently achieve the isotropic and uniform thermal expansion characteristics required of the substrate. It is important to note that even if the linear expansion coefficient of the polymer is suppressed in the direction of elongation, the linear expansion coefficient in the perpendicular direction will not be suppressed and may even increase.
[0058] By stretching molecules so that they are oriented to the same degree in multiple directions, a substrate with improved isotropy of the linear expansion coefficient can be obtained. However, this method has been difficult to obtain a substrate with consistently desired thermal expansion properties. This is presumably due to the inability to directly control the stretching direction of each molecule.
[0059] Based on this actual situation, the inventors of this application conducted careful research and found that direct control can be achieved by using multiple layers composed of very thin films whose orientation and thermal expansion characteristics are independently controlled on a layer-by-layer basis and combining them in a specified form to form a substrate.
[0060] The substrate is constructed as a stack of multiple thin films exhibiting anisotropic linear expansion coefficients within the substrate's extended plane. In this substrate, the molecular orientation and the direction and magnitude of the anisotropy of the linear expansion coefficient can be independently and directly controlled for each individual film unit. Furthermore, the thermal expansion characteristics of the substrate comprising these thin film stacks, including their isotropy and uniformity, can be directly controlled by the stacking configuration of the individual films.
[0061] As a result, a fluororesin base material having isotropic, uniform, and sufficiently low thermal expansion characteristics can be stably provided.
[0062] In a substrate having such a structure and a wiring board using the same, the fluororesin, serving as the matrix resin, inherently controls the linear expansion coefficient, eliminating the need for thermal expansion control materials such as glass and ceramics. Consequently, deterioration in electrical properties caused by the composite material is significantly suppressed or virtually eliminated, resulting in a substrate and wiring board that fully utilize the excellent electrical properties inherent to the fluororesin.
[0063] Furthermore, in this structure, the elongated fluororesin molecules have the effect of suppressing CTE. Unlike thermal expansion control materials such as glass fibers and ceramic beads, which are millimeter- or micron-sized, fluororesin molecules and the crystals they form are nanometer-sized. This significantly reduces variations in the physical properties of substrates and wiring boards within their surfaces.
[0064] Furthermore, a wiring board with improved conductor formation accuracy can be obtained. For example, when forming via holes, the thermal expansion control material suppresses laser scattering and reduces the occurrence of processability variations, thereby enabling the formation of regularly shaped via holes and vias.
[0065] In this embodiment, if Figure 1As shown in (a), the substrate 100 is a film-like member having a rectangular shape. However, the length of each side may be within a range of 2 mm to 1500 mm, or within a range of 50 mm to 700 mm. The substrate 100 is configured to include the substrate in the in-plane direction. Figure 1 In the plane of the X-Y direction indicated by the arrows, the material, thickness, and various properties are uniform.
[0066] The thickness of the substrate 100 (the size in the Z direction in the figure) is not limited thereto, and may be in the range of 0.003 mm to 2 mm, or in the range of 0.02 mm to 0.2 mm.
[0067] In the substrate 100 , the thickness (the size in the Z direction in the figure) of at least one of the film 110 and the film 120 is not limited thereto, but may be 0.005 mm or less, or 0.003 mm or less.
[0068] In this embodiment, the substrate 100 is not mechanically reinforced by a thermal expansion control material such as glass or ceramic. Mechanical reinforcement by a thermal expansion control material refers to suppressing the linear expansion coefficient of the substrate by dispersing a certain amount of fibers or particles composed of a material having a smaller linear expansion coefficient than that of the matrix resin, i.e., the fluororesin, into the multiple fluororesin films constituting the substrate 100. The proportion of the thermal expansion control material in the overall substrate 100 may be 20% by weight or less, 10% by weight or less, or even 2% by weight or less. In particular, a proportion of 0.5% by weight or less achieves exceptional electrical properties.
[0069] As a result of minimizing the need for composites with other materials, a wiring board using substrate 100 can have a relative dielectric constant εr of 2.3 or less, preferably 2.1 or less, at 30 GHz and 22°C. Similarly, a dielectric loss tangent tanδ can be set to 0.001 or less, more preferably 0.0003 or less, and particularly preferably 0.0001 or less. Furthermore, at 50 GHz and 110 GHz, a relative dielectric constant εr of 2.3 or less, preferably 2.1 or less, at 22°C, and a dielectric loss tangent tanδ can be set to 0.001 or less, more preferably 0.0003 or less, and particularly preferably 0.0001 or less. Moreover, the relative dielectric constant εr of the wiring substrate using the substrate 100 at 250 GHz and 300 GHz and 22°C can be set to less than 2.3, preferably less than 2.1, and the dielectric loss tangent tanδ can also be set to less than 0.001, more preferably less than 0.0003, and particularly preferably less than 0.0001, thereby providing a wiring substrate with extremely excellent dielectric properties that are difficult to achieve through other structures.
[0070] The relative dielectric constant εr and dielectric loss tangent tanδ can be measured using standard measuring instruments. However, for measurements in the high-frequency range of 250 GHz and 300 GHz, the Fabry-Perot method, a type of open resonator method, can be used. When measuring electrical properties using the Fabry-Perot method, the ideal measurement environment is a temperature of 25°C ± 3°C and a relative humidity of 60% or less.
[0071] The relative dielectric constant εr and dielectric loss tangent tanδ of the substrate described in the claims of the present application were measured by the Fabry-Perot method. The relative dielectric constant εr at 250 GHz and 22°C was 2.3 or less, and the dielectric loss tangent tanδ was 0.001 or less. Similarly, the relative dielectric constant εr at 300 GHz and 22°C was 2.3 or less, and the dielectric loss tangent tanδ was 0.001 or less. Moreover, at any frequency in the range of 250 GHz to 300 GHz at 22°C, the relative dielectric constant εr of the substrate described in the claims of the present application was 2.3 or less, and the dielectric loss tangent tanδ was 0.001 or less.
[0072] It should be noted that, in this embodiment, Figure 1 As shown in (a), the small CTE direction of the film 110 is parallel to one side of the rectangular substrate 100. However, the small CTE direction or large CTE direction of the film may not necessarily be parallel to the extending direction of the side of the substrate 100. Alternatively, based on observations of dimensional changes in the film 110 during temperature changes, the direction of minimum thermal expansion within the extended plane of the film 110 may be defined as the small CTE direction of the film 110, and the direction perpendicular to the small CTE direction may be defined as the large CTE direction of the film 110.
[0073] In practice, films, substrates, or wiring boards often have a roughly rectangular shape or a combination of roughly rectangular shapes for reasons such as production efficiency. The linear expansion coefficient can also be measured along the direction extending from a specific side of these rectangles and in a direction perpendicular to that direction. The minimum and maximum CTE directions of the film can be determined based on whether or not the linear expansion coefficient of the film satisfies this anisotropy.
[0074] In other films in the substrate including the film 120 , the small CTE direction and the large CTE direction can also be determined by the same method.
[0075] The linear expansion coefficient CTE of the film 110 and / or the film 120 in the small CTE direction SIt can be less than 30 ppm / °C. More preferably, it is less than 20 ppm / °C, further preferably less than 0 ppm / °C, and particularly preferably less than -20 ppm / °C. S It may be -60 ppm / ° C. or higher, and preferably -50 ppm / ° C. or higher. When the film has a predetermined linear expansion coefficient, its thermal behavior tends to be stabilized.
[0076] Linear expansion coefficient CTE of each film in the large CTE direction L It can be 30ppm / ℃ or more. It can also be 40ppm / ℃ or more. It can also be 80ppm / ℃ or more. It can also be 120ppm / ℃ or more. Even in the case of large CTE direction, the extremely large linear expansion coefficient CTE L Since the thermal behavior may become unstable, it is preferably 200 ppm / °C or less.
[0077] As described later, in the substrate described in the present application, the linear expansion coefficient CTE in the direction of the small CTE of the film can be made S CTE L plays a leading role, therefore, in terms of the anisotropy of the linear expansion coefficient in each film, the linear expansion coefficient CTE in the direction of small CTE S The linear expansion coefficient in the large CTE direction is less than 30ppm / ℃ and is greater than 30ppm / ℃. More preferably, the linear expansion coefficient in the small CTE direction is S Less than 20ppm / ℃ and the linear expansion coefficient in the large CTE direction is 40ppm / ℃ or more. More preferably, the linear expansion coefficient CTE in the small CTE direction is S The linear expansion coefficient in the direction of large CTE is preferably less than 0ppm / ℃ and is preferably 40ppm / ℃ or more. It is particularly preferred that the linear expansion coefficient in the direction of small CTE is S Less than -20ppm / ℃ and the linear expansion coefficient in the large CTE direction is 40ppm / ℃ or more.
[0078] Alternatively, regarding the anisotropy of the linear expansion coefficient in each film, the linear expansion coefficient CTE in the direction of small CTE may be set to S The linear expansion coefficient in the large CTE direction is less than 20 ppm / °C and is greater than 20 ppm / °C.
[0079] By providing a thin film having a suppressed linear expansion coefficient in the small CTE direction, it is easy to stably obtain a substrate having a linear expansion coefficient of 60 ppm / °C or less.
[0080] It is preferred that at least two or more thin films among the plurality of thin films included in the substrate 100 have the above-mentioned linear expansion coefficient, and it is particularly preferred that all the thin films have the above-mentioned linear expansion coefficient.
[0081] The film constituting the substrate 100 has the above-mentioned anisotropy of the linear expansion coefficient, but it is preferable that the linear expansion coefficient of the substrate 100 has a predetermined isotropy. For example, there is an arbitrary direction D1 and a direction D2 perpendicular to the D1 on the substrate surface. When the linear expansion coefficient of the substrate 100 in the D1 direction is set as CTE D1 , and the linear expansion coefficient of the substrate 100 in the D2 direction is set as CTE D2 When CTE D1 Divide by CTE D2 The obtained value (hereinafter referred to as CTE D1 / CTE D2 ) is 0.5 or less and 2 or less. D1 / CTE D2 It is preferably 0.7 or more and 1.3 or less, and particularly preferably 0.8 or more and 1.2 or less.
[0082] Here, the D1 direction of the substrate 100 can also be set to be parallel to the small CTE direction (or large CTE direction) of the film 110, and the D2 direction of the substrate 100 can be set to be parallel to the large CTE direction (or small CTE direction) of the film 110.
[0083] When the D1 direction of the substrate 100 is set to be parallel to the small CTE direction of the film 110, that is, Figure 1 In the X direction, the linear expansion coefficient CTE of the substrate 100 in the X direction is D1 and the linear expansion coefficient CTE in the Y direction D2 The linear expansion coefficient CTE in the small CTE direction of the film 110 can also be greater than S Furthermore, the linear expansion coefficient CTE of the substrate 100 in the D1 direction is D1 and the linear expansion coefficient CTE in the D2 direction D2 They can also be smaller than the linear expansion coefficient CTE in the large CTE direction of the film 110. L .
[0084] In addition, the linear expansion coefficient CTE of the substrate 100 D1 and linear expansion coefficient CTE D2 The average value is less than the linear expansion coefficient CTE of the film 110 S and linear expansion coefficient CTE LThe average value of is good. This substrate 100 is obtained by forming the substrate 100 in a state where the orientation and crystal structure of the film 110 are maintained as much as possible. For example, in the process of laminating multiple films, the fluororesin constituting the film is controlled so as not to undergo crystallization and melting. In this way, the controlled linear expansion coefficient CTE of the film can be reflected in a form dominated by the linear expansion coefficient of the substrate. S In addition, the anisotropy of the linear expansion coefficient of the film 110 is increased, that is, the specific CTE is increased. S / CTE L It is also effective.
[0085] Similarly, the linear expansion coefficient CTE of the substrate 100 in the D1 direction is D1 and the linear expansion coefficient CTE in the D2 direction D2 are all greater than the linear expansion coefficient CTE in the small CTE direction of the film 120 S In addition, the linear expansion coefficient CTE of the substrate 100 in the D1 direction is D1 and the linear expansion coefficient CTE in the D2 direction D2 are all smaller than the linear expansion coefficient CTE in the large CTE direction of the film 120 L In addition, the linear expansion coefficient CTE of the substrate 100 is D1 and linear expansion coefficient CTE D2 The average value is less than the linear expansion coefficient CTE of the film 120 S and linear expansion coefficient CTE L The average value is good.
[0086] The linear expansion coefficient CTE of the substrate 100 in the D1 direction D1 The linear expansion coefficient CTE in the D2 direction D2 The concentration is preferably 60 ppm / °C or less, more preferably 50 ppm / °C or less, further preferably 45 ppm / °C or less, and particularly preferably 40 ppm / °C or less.
[0087] In addition, when the thickness direction of the substrate 100 is Figure 1 When the linear expansion coefficient in the direction indicated by the arrow Z is set to CTED3, CTED3 may be greater than the linear expansion coefficient CTE in the D1 direction of the substrate 100. D1 and the linear expansion coefficient CTE in the D2 direction D2 Alternatively, CTED3 may be greater than 60 ppm / °C, greater than 80 ppm / °C, or even greater than 100 ppm / °C. Prioritizing low thermal expansion in the substrate surface direction over the substrate thickness direction is beneficial for improving fine pattern formation, thermal warpage in thin substrates, and electrical properties.
[0088] Substrate 100 is flexible. It is particularly advantageous if it can be stored wound on a roll, and preferably has the flexibility to enable the use of roll-to-roll continuous processing equipment in the wiring board manufacturing process. For example, even after being stored at room temperature for four weeks wound on a 200 mm diameter roll, it can easily return to a flat shape. Furthermore, it is preferred that, even after such storage, it maintains the stability required for a substrate used in the dielectric layer of a wiring board.
[0089] The substrate 100 may be in the form of a flexible strip. The width of the strip is preferably 60 mm or more, more preferably 150 mm or more, and the length of the strip is preferably 1 m or more, more preferably 10 m or more.
[0090] Alternatively, the substrate 100 may be wound around a winding frame called a reel or bobbin to form a roll. The substrate can be formed in such a manner, thereby improving the continuous productivity of the wiring board.
[0091] The tensile modulus of substrate 100 at room temperature is preferably 200 MPa or greater. Furthermore, the tensile modulus of substrate 100 at 200°C is preferably 100 MPa or greater. Having a predetermined tensile strength, the substrate suppresses deformation even under applied external stress. This substrate enables excellent wiring board properties and high production yields, even in wiring boards requiring micron-level patterning accuracy.
[0092] The substrate 100 and the film constituting the substrate 100 are preferably not subjected to post-stretching calcination. Even when PTFE is the main component, such a substrate can be confirmed by the absence of an endothermic peak derived from PTFE at temperatures lower than 339°C in the crystal melting curve obtained by differential scanning calorimetry (DSC).
[0093] Preferably, when the main component of the film 110 constituting the substrate 100 is PTFE, the density of the film 110 is higher than that of the porous stretched PTFE. The density of the film 110 is, for example, 1.8 g / cm 3 Above and 2.4g / cm 3 Below, preferably 1.9 g / cm 3 Above and 2.4g / cm 3 The following. Moreover, the film 120 may also have the same density. In addition, the substrate 100 may also have the same density.
[0094] From the perspective of electrical properties, the main component of substrate 100 is preferably a fluororesin. The proportion of fluororesin in substrate 100 may be 75% by weight or greater, but is preferably 90% by weight or greater. Furthermore, the proportion of fluororesin in substrate 100 is particularly preferably 95% by weight or greater. By setting it to 99.5% by weight or greater, the excellent electrical properties inherent in fluororesin can be fully utilized.
[0095] As with the film, the fluororesin may contain PTFE as a main component.
[0096] Multiple films can also have a high degree of orientation in the fluororesin polymer that is their main component. The linear chains of the fluororesin molecules in the film preferentially align along the direction of low CTE over the direction of high CTE of the film, and this is believed to result in anisotropy in the linear expansion coefficient.
[0097] In particular, significant anisotropy of the linear expansion coefficient can be found in stretched fluororesin films. As a result of the compression and other treatments described later, this anisotropy is maintained or strengthened even in a state where identification of the fibrils by electron microscopy becomes difficult. Therefore, it is believed that this is not a characteristic of the so-called porous structure composed of nodes and fibrils itself, but rather a physical characteristic caused by the film having a crystalline structure derived from the fibrils generated by stretching. The reason for this is that within the fibrils with a fiber shape having a high aspect ratio, the straight chains of the fluororesin molecules are more effectively stretched in a straight line along the direction of fibril extension.
[0098] (Second embodiment)
[0099] Figure 2 Schematic diagram showing a cross section of a substrate 100 according to a second embodiment of the present invention observed from the horizontal direction. In this embodiment, the number of layers and the stacking state of the multiple thin films constituting the substrate 100 are different from those of the first embodiment, but the other structures can be the same as those of the first embodiment. The substrate 100 includes at least one of a plurality of thin films 110 and a thin film 120, and these thin films are stacked alternately. Figure 2 In the figure, an example of a substrate including three layers consisting of film 110 and three layers consisting of film 120 is shown, but as long as one or both of film 110 and film 120 are multiple, film 110 and film 120 can also have more than four layers or more layers.
[0100] exist Figure 2In the figure, multiple films 110 are arranged with the X direction in the figure as the direction of low CTE and the Y direction in the figure as the direction of high CTE. Conversely, multiple films 120 are arranged with the Y direction in the figure as the direction of low CTE and the X direction in the figure as the direction of high CTE. In other words, multiple films 110 and multiple films 120 are stacked so that their respective low CTE directions intersect at approximately right angles.
[0101] In this embodiment, thin film 120 is formed directly on thin film 110, and another thin film 110 is formed directly on thin film 120. That is, substrate 100 includes a three-layer thin film stack structure, with thin film 120 formed between two thin films 110. Alternatively, another thin film 120 may be formed directly on the other thin film 110. In other words, substrate 100 may also include a four-layer thin film stack structure: thin film 110, thin film 120, thin film 110, and thin film 120.
[0102] Thus, in this embodiment, substrate 100 includes a plurality of at least one of thin films 110 and 120, and preferably a plurality of both. By forming substrate 100 of uniform thickness using layers composed of more thin films, the in-plane uniformity of thickness and linear expansion coefficient can be further improved.
[0103] Furthermore, by alternately stacking the plurality of thin films 110 and the plurality of thin films 120 in the thickness direction, the uniformity of the physical properties within the substrate surface can be improved.
[0104] It should be noted that in this embodiment, a configuration in which multiple films 110 and multiple films 120 are alternately stacked in layers is illustrated, but the present invention is not limited thereto. For example, the substrate may include a region in which multiple films 110 and / or one of films 120 are continuously arranged in the thickness direction. A bonding interface between two films whose linear expansion coefficient anisotropies are approximately parallel can provide higher bonding reliability than a bonding interface between two films whose linear expansion coefficient anisotropies are orthogonal.
[0105] (Third embodiment)
[0106] Figure 3 This is a schematic diagram showing a cross-section of a substrate 100 according to a third embodiment of the present invention. This embodiment differs from the other embodiments in that the substrate 100 has a thin film stack structure that is symmetrical in the thickness direction, but the other structures can be the same as those of the other embodiments.
[0107] In this embodiment, for the multiple films 110, the horizontal direction (X direction in the figure) is the direction of minimum CTE, and the direction perpendicular to the paper (Y direction in the figure) is the direction of maximum CTE. In contrast, for the film 120, the direction perpendicular to the paper is the direction of minimum CTE, and the horizontal direction is the direction of maximum CTE. In other words, the films 120 are stacked such that the direction of minimum CTE of the film 120 intersects the direction of minimum CTE of the multiple films 110 at a substantially right angle.
[0108] In this embodiment, substrate 100 has a structure in which three thin film layers, namely film 110, film 120, and film 110, are sequentially stacked. By having substrate 100 with such a symmetrical thin film stack structure in the thickness direction, warping of the substrate or wiring board can be suppressed.
[0109] "Symmetrical in the thickness direction" means that, with the intersection points of an imaginary straight line perpendicular to the substrate surface (the dotted line indicated by A in the figure) and the substrate surface at arbitrary positions on the substrate surface being P1 and P2, respectively, and the midpoint between P1 and P2 being P3, the types and stacking order of the multiple thin films constituting P1 to P3 are equal to the types and stacking order of the multiple thin films constituting P2 to P3. For example, in this embodiment, the types and stacking order of the thin films constituting either P1 to P3 or P2 to P3 are film 110 - film 120.
[0110] The thin film stack structure that is symmetrical in the thickness direction is not limited to the above. Although not shown in the figure, for example, the thin film stack structures of P1 to P3 and P2 to P3 can both be thin film 110 - thin film 120 - thin film 110, or can both be thin film 110 - another thin film - thin film 120. Examples of the other thin film include a film that differs from both film 110 and film 120 in at least one of composition, thickness, anisotropy, and low CTE direction.
[0111] The substrate may be symmetrical in the thickness direction across substantially the entire surface of the substrate. Furthermore, preferably, in addition to the types of thin films and the stacking order of thin films constituting the thin film stack structures P1 to P3 and P2 to P3 being substantially equal, the thickness of each thin film is also substantially equal. Alternatively, the substrate 100 may be linearly symmetrical about an imaginary line (not shown) parallel to the substrate surface passing through the midpoint P3 when viewed in cross-section, or may be plane-symmetrical about a plane including the midpoint P3.
[0112] In this embodiment, the thickness of the film 120 is greater than the thickness of each film 110, and the total thickness of the plurality of films 110 is formed to be substantially equal to that of the film 120. The total thickness of the films 110 may be greater than 70% and less than 130% of the thickness of the film 120, or may be greater than 90% and less than 110%. In addition, in this embodiment, the films 110 and 120 have the same anisotropy of the linear expansion coefficient. For example, the specific CTE of the plurality of films 110 is greater than 10%. S / CTE L The specific CTE of the film 120 may be S / CTE L 70% or more and 130% or less, or 90% or more and 110% or less. L -CTE S It can be the difference in CTE of the film 120 L -CTE S The range may be 70% to 130% inclusive, or 90% to 110% inclusive.
[0113] In this way, the thickness of the thin film including the intersection point P1 and / or the intersection point P2 on the surface of the substrate 100 may be configured to be smaller than the thickness of the thin film including the midpoint P3.
[0114] Although not shown in the figure, when the multiple films constituting the substrate include a first film group composed of multiple films having a common small CTE direction and another film group composed of multiple films having another small CTE direction that intersects with the small CTE direction of the first film group, the total film thickness of the former film group can also be approximately equal to the total film thickness of the latter film group.
[0115] It should be noted that it is also possible to combine films 110 and 120 having different anisotropy of linear expansion coefficient. For example, when the CTE of the plurality of films 110 is different from the anisotropy of linear expansion coefficient, the film 110 and the film 120 may be different from each other. S / CTE L Greater than the specific CTE of the film 120 S / CTE L In this case, the total thickness of the film 110 can also be made smaller than the thickness of the film 120. In addition, the thickness of the substrate can be adjusted by adjusting the number of multiple films constituting the substrate, and the thickness of the substrate can be adjusted by adjusting the thickness of the multiple films constituting the substrate.
[0116] The thickness of the film 110 including the intersection point P1 can be set to, for example, 0.005 mm or less, and the thickness of the film 120 including the midpoint P3 can be set to greater than 0.005 mm and 0.04 mm or less. By arranging a film having a thickness greater than that of the film including the substrate surface at the center of the substrate thickness in this manner, the thickness and CTE of the substrate can be easily controlled.
[0117] By appropriately combining the anisotropy of the linear expansion coefficient in the substrate surface direction and the thickness of the thin films constituting the substrate in this manner, the anisotropy of the linear expansion coefficient of the substrate can be suppressed even when different thin films are combined.
[0118] (Fourth embodiment)
[0119] The substrate 100 of this embodiment includes a thin film 110 and a thin film 120 formed on the thin film 110. Both thin films 110 and 120 contain fluororesin as their main component and have the same chemical composition. Furthermore, in any cross-section of the substrate 100 perpendicular to the substrate surface, the difference between the refractive index of the thin film 110 and the refractive index of the thin film 120 is 0.01 or greater. Other configurations may be the same as those of the other embodiments described above.
[0120] The difference in refractive index between two layers having the same chemical composition is caused by the difference in angle of the orientation direction of the molecules of each thin film with respect to the arbitrary cross section, that is, the surface for measuring the refractive index.
[0121] The difference in refractive index between films 110 and 120 is preferably 0.02 or greater, and particularly preferably 0.03 or greater.
[0122] The linear expansion coefficient and anisotropy of the substrate 100 having such a structure are suppressed. As a result, a substrate having the physical properties required of a substrate while maintaining excellent electrical properties can be provided.
[0123] Furthermore, thin films 110 and 120 have nearly identical properties other than orientation-induced anisotropy, providing a substrate with extremely high microscopic uniformity. This feature offers various advantages for the manufacturability of wiring boards and the electrical properties of dielectric layers.
[0124] The reason why the refractive index differs due to orientation will be described below.
[0125] Each polymer molecule is shaped like a nanometer-sized rope. The irregular amorphous portions of the polymer are randomly bent and have no directionality. The regularly folded crystalline portions are also irregularly arranged within the polymer structure, lacking directionality. Therefore, the medium becomes a completely uniform medium for light. However, when polymer molecules are oriented, the refractive index for light polarized in the orientation direction differs from the refractive index for light polarized in a direction perpendicular to the orientation direction. Generally speaking, the refractive index in the orientation direction is higher, while the refractive index in the perpendicular direction is lower.
[0126] As a result, a difference in refractive index is observed between the film 110 and the film 120 in which the orientation directions intersect with each other.
[0127] The refractive index can be measured in accordance with Japanese Industrial Standard JIS K 0062. A sample for measurement including a cross-section perpendicular to the extended surface of the substrate is cut out from a substrate or a wiring substrate including the substrate using a cutter or the like, and the cross-section is set as the observation surface. Light with a wavelength of 589 nm is incident on the observation surface, and the critical refraction angle is observed to measure the refractive index of the film. In this case, by using a polarizing lens in the eyepiece, the refractive index of the film in a certain direction can be measured. The measuring instrument can be an Abbe refractometer manufactured by Atago.
[0128] Having the same chemical composition means that the ratios of the elements, compounds, and other chemical components that make up each film are equal, but differences in terminal functional groups and impurities may exist. Alternatively, the difference in the ratio of the elements or compounds that make up film 110 and film 120 may be less than 2% by weight.
[0129] The fact that films 110 and 120 have the same chemical composition can also be considered to have the same thermal properties. For example, when DSC analysis of these films is performed under the conditions described in Patent Document 4, films 110 and 120 preferably have peaks with the largest areas at substantially the same position (temperature), or they may have peaks with the largest areas at substantially the same position (temperature).
[0130] Figure 4 Schematic diagram of a wiring board 200 including a base material 100 according to an embodiment of the present invention as a dielectric layer. Figure 4 (a) is a schematic diagram obtained by observing the wiring substrate 200 from a direction perpendicular to the substrate surface. Figure 4 (b) is a schematic diagram of the wiring substrate 200 as viewed from a cross-sectional direction of the wiring substrate.
[0131] Wiring substrate 200 includes multiple conductor patterns. These multiple conductor patterns include one or more of pads 210, wiring 220, vias 230, antenna pads 240, or ground plane 250. Other electronic components are electrically connected to pads 210. Vias 230 form electrical connections along the thickness direction of the wiring substrate (the Z direction in the figure). In particular, they form electrical connections between the conductor pattern formed on the upper surface of the dielectric layer and the conductor pattern formed on the lower surface of the dielectric layer.
[0132] In this embodiment, wiring substrate 200 includes wiring 220 , and electrical signals having a frequency of, for example, 50 GHz or higher are transmitted along wiring 220 as a path.
[0133] The width of the wiring may be 1 μm to 100 μm, or 10 μm to 30 μm. The thickness of the wiring may be 1 μm to 40 μm, or 7 μm to 25 μm.
[0134] The wiring substrate 200 includes a base material 100, and the plurality of conductor patterns described above are formed on the upper surface and / or lower surface of the base material 100. In this embodiment, the wiring substrate 200 includes a base material 100, and the plurality of conductor patterns described above are formed on the upper surface and / or lower surface of the base material 100. Figure 3 The substrate 100 shown is a wiring substrate 200 having a dielectric layer, but for example, a Figure 1 、 Figure 2 The substrate 100 according to another embodiment of the present invention is shown as a dielectric layer.
[0135] The wiring substrate 200 may further include a protective layer (not shown) made of an insulating material formed on the plurality of conductor patterns.
[0136] Wiring substrate 200 includes a dielectric layer formed of base material 100. The dielectric layer functions as a base for forming a conductor layer on its upper surface and / or lower surface, and functions as a support member for supporting the conductor layer and the plurality of conductor patterns within each conductor layer so that they are electrically independent.
[0137] In this embodiment, the dielectric layer significantly reduces the deterioration of electrical properties caused by the addition of other composite materials. Therefore, wiring substrate 200 can fully utilize the excellent electrical properties of fluororesin. In particular, even very high-frequency signals exceeding 50 GHz can be transmitted with extremely low loss.
[0138] Furthermore, due to the suppressed linear expansion coefficient of the base material 100 , it is possible to provide the wiring board 200 having excellent physical properties in which deformation and warpage associated with temperature changes are significantly reduced.
[0139] Preferably, the dielectric layer of wiring substrate 200 contains no thermal expansion control material or contains only a very small amount of thermal expansion control material. For example, when a microstrip line (not shown) is formed between a wiring that transmits a high-frequency signal of 50 GHz and a conductor plane with a fixed potential formed below the wiring, the dielectric layer between the wiring and the conductor plane may not contain a thermal expansion control material. It is particularly preferred that the dielectric layer between the wiring and the conductor plane be composed solely of a film primarily composed of a fluororesin.
[0140] Alternatively, in cross-sectional view at any position of the wiring substrate 200 , the area ratio of the thermal expansion control material in the dielectric layer between the high-frequency signal transmission wiring and the conductor plane may be set to 10% or less, or 1% or less.
[0141] Furthermore, wiring substrate 200 may not include a reinforcing layer containing 30% by weight or more of a thermal expansion control material.
[0142] On the substrate surface of the wiring substrate 200, there are an arbitrary direction D1 and a direction D2 perpendicular to the direction D1. When the linear expansion coefficient of the wiring substrate 200 in the direction D1 is defined as CTE D1 , the linear expansion coefficient of the wiring substrate 200 in the D2 direction is set as the CTE of the wiring substrate D2 When CTE D1 Divide by CTE D2 The obtained value (hereinafter referred to as CTE D1 / CTE D2 ) is 0.5 or more and 2 or less. D1 / CTE D2 It is preferably 0.7 or more and 1.3 or less, and particularly preferably 0.8 or more and 1.2 or less.
[0143] Here, the D1 direction of the wiring substrate 200 can also be set to a direction parallel to the small CTE direction (or large CTE direction) of the film 110, and the D2 direction of the wiring substrate 200 can be set to a direction parallel to the large CTE direction (or small CTE direction) of the film 110.
[0144] Wiring substrate 200 may further include a second dielectric layer (not shown) and a third conductor layer (not shown) formed on the second dielectric layer. In this case, preferably, base material 100 according to any embodiment of the present invention is also used for the second dielectric layer.
[0145] (Method for producing substrate)
[0146] Hereinafter, an example of a method for producing a substrate according to an embodiment of the present invention will be described. Figure 5The schematic diagram of the substrate manufacturing process is shown in FIG. The substrate manufacturing process can be roughly divided into a process group for preparing a sheet (S1 to S5 in the figure), a process for preparing a film having predetermined thermal expansion characteristics (S6), and a process group for forming a substrate by stacking these films in a cross-layered manner (S7 and S8 in the figure).
[0147] The number of times and implementation methods of each step are not limited to the following, and each step may be performed multiple times or combined with other preceding / following steps without losing the technical significance of the step.
[0148] First, a sheet containing fluororesin as a main component is formed by the following steps. The fluororesin sheet can also be formed by a known method.
[0149] (mix)
[0150] Unfired PTFE fine powder is mixed with an additive to prepare a paste composed of resin particles. Commercially available PTFE fine powder can be used, but it is preferred to select a PTFE fine powder with a small average particle size, so that the film has the desired thermal expansion characteristics. A preferred average particle size is 250 μm or greater and 900 μm or less. The apparent density of the PTFE fine powder is exemplified as 0.3 g / ml or greater and 0.8 g / m or less.
[0151] Commercially available additives can be used as the additive, and examples thereof include petroleum-based solvents having an initial boiling point (IBP) of 150° C. to 250° C.
[0152] (Preform)
[0153] The prepared paste is compression molded to form a preform. The subsequent extrusion process is performed at a temperature lower than the initial boiling point of the additive, such as room temperature, to suppress volatilization of the additive.
[0154] (Extrusion)
[0155] The preform is passed through an extrusion die while being pressurized, thereby forming a film-like sheet having a longitudinal dimension. The width and thickness of the sheet are controlled by the extrusion conditions, especially the shape of the die.
[0156] The process after extrusion can also be applied continuously while the sheet is flowing in the long direction of the sheet. Hereinafter, the direction in which the sheet or film flows is indicated as MD (machine direction; longitudinal direction), and the width direction of the film perpendicular to the MD is indicated as TD (transverse direction; transverse direction).
[0157] (Rolling)
[0158] As needed, the outer shape is adjusted so that the thickness of the sheet becomes the desired thickness by clamping the formed sheet from above and below with metal rollers or the like and applying pressure. Here, the dimensional change is not limited to the thickness but may also be accompanied by changes in the overall length (MD size) and width (TD size) of the sheet.
[0159] (dry)
[0160] By heating the sheet, the additive remaining in the sheet is volatilized and removed. Of course, increasing the drying temperature can improve the efficiency of removing the additive, but for reasons described below, it is preferably controlled so as not to exceed the crystalline melting point of the molecules constituting the sheet.
[0161] By doing this, a long sheet mainly composed of fluororesin can be prepared.
[0162] Next, the above-mentioned sheet is used to form a thin film having predetermined thermal expansion characteristics.
[0163] (extend)
[0164] Tensile stress is applied to the dried sheet at a temperature below the crystalline melting point of the fluororesin constituting the sheet, thereby stretching the sheet along its surface. The direction of stress application, i.e., the stretching direction, can be the MD, TD, or other directions, and can be a single direction or multiple directions. When stretching in multiple directions, stretching in each direction can be performed independently and combined, or it can be performed simultaneously in a form that includes different stretching directions. The stretching ratio in a particular direction can be, for example, greater than 1 and less than 50 times, or it can be stretched at a ratio greater than this.
[0165] In particular, during the stretching of PTFE, a film having a porous structure consisting of nodes and fibrils can be obtained. The thickness of the film at this time point can be between 0.005 mm and 3 mm, preferably between 0.01 mm and 1 mm. The density of the film at this time point can be, for example, 0.1 g / cm 3 Above and 0.7g / cm 3 Below, preferably 0.2g / cm 3 Above and 0.5g / cm 3 the following.
[0166] The film laminated in the subsequent process has the above-mentioned predetermined thermal expansion characteristics. The predetermined thermal expansion characteristics of the film include, for example, the above-mentioned specific CTE. S / CTE L and / or poor CTE L -CTE STherefore, stretching conditions should be determined so that the film exhibits the specified thermal expansion characteristics. Such thermal expansion characteristics can be imparted to the film, for example, by adjusting the stretching ratio and direction. However, as a result of the multiple pre-stretching steps, it is important to note that the sheet already has molecular orientation before stretching. For example, during extrusion and rolling, molecular orientation in the MD and / or TD occurs according to the specific implementation conditions. Furthermore, sometimes, high process temperatures cause at least a portion of the molecules to become amorphous again, reducing the degree of orientation.
[0167] Therefore, it is advisable to understand and / or manage the molecular orientation and / or linear expansion coefficient of the sheet before stretching. Thus, by stretching the sheet with the managed orientation and / or linear expansion coefficient under conditions adjusted so that the film has the desired thermal expansion characteristics, a film suitable for the substrate of the present invention can be obtained.
[0168] In the extension of PTFE, fibril formation contributes to the above-mentioned orientation and imparts thermal expansion characteristics to the film. It is believed that fibril is composed of a linear molecular chain drawn from a node. As a result, it is believed that the linear expansion coefficient of the direction in which the extension of the fibril is more strongly suppressed.
[0169] The stretching conditions for imparting predetermined thermal expansion characteristics to the film can be determined by actually stretching a sheet prepared under the managed conditions under various stretching conditions, measuring the linear expansion coefficient of the resulting film, and selecting appropriate stretching conditions.
[0170] When achieving a specific anisotropy of linear expansion coefficient, forming a substrate using a roll-to-roll process, or obtaining a substrate with specific external dimensions, it is sometimes difficult to achieve the desired thermal expansion characteristics simply by using stretching conditions. In such cases, stretching conditions can be determined based on a preliminary study of various conditions in the sheet forming process and optimization as needed.
[0171] In this manner, a film having a controlled and / or managed linear expansion coefficient can be prepared.
[0172] (Thin Film Lamination)
[0173] Next, the film having the above-mentioned thermal expansion characteristics is laminated.
[0174] Multiple films having the specified thermal expansion characteristics prepared as described above are stacked. During stacking, the films are stacked so that the small CTE directions of one film and the other films intersect when viewed from above (through the thickness of the films). For example, multiple small film sheets can be cut from a large film having both small and large CTE directions, and the sheets are stacked so that the small CTE directions of the film sheets are approximately orthogonal to each other.
[0175] The lamination method is not limited to the above; for example, continuous lamination in a roll-to-roll configuration is also possible. First, prepare one or more long strips of MD stretched film and TD stretched film. MD stretched film is a film formed by orienting the molecules in the MD, such as by setting the MD as the primary stretching direction, with the MD as the direction of minimum CTE. TD stretched film is a film formed by orienting the molecules in the TD, such as by setting the TD as the primary stretching direction, with the TD as the direction of minimum CTE. MD stretched film can be formed, for example, by making the take-up speed of the receiving roll greater than the delivery speed of the supply roll. TD stretched film can be formed, for example, by applying tensile stress in the TD to the sheet during transport from the supply roll to the receiving roll, thereby widening the sheet.
[0176] Next, by laminating these films while flowing together in the MD, a long laminate can be obtained in which the MD stretched film and the TD stretched film are laminated with the directions of the anisotropy of their linear expansion coefficients intersecting with each other.
[0177] In the case of lamination in this manner, the anisotropy of the linear expansion coefficient of the MD stretched film can also be made smaller than the anisotropy of the linear expansion coefficient of the TD stretched film. S / CTE L Specific CTE of TD stretched film S / CTE L The closer it is to 1, the better. A wide, long film laminate can be obtained, which is advantageous in production efficiency when cutting a plurality of wiring boards.
[0178] In addition, the TD stretch ratio of the TD stretched film can be made greater than the MD stretch ratio of the MD stretched film. Here, the stretch ratio refers to the rate of change in the dimension of the sheet in the stretching direction before and after stretching. Even if the molecular orientation in TD during the sheet preparation process is not sufficiently ensured, it is possible to obtain a film with an anisotropic linear expansion coefficient close to that of the MD stretched film (for example, a CTE of 0.05). S / CTE L and / or poor CTE L -CTE S ) is combined and laminated with anisotropic TD stretched films, thereby obtaining a substrate with excellent uniformity and stability.
[0179] Alternatively, the MD stretched film and the TD stretched film can be laminated with the MD stretched film positioned on the substrate surface. For example, the MD stretched film can be laminated with the TD stretched film on the outside, such as in the following pattern: MD stretched film - TD stretched film - MD stretched film. MD stretched film can have high physical properties such as MD tensile strength, enabling stable continuous production even under conditions where tension is likely to be applied to the MD, such as conveyor speeds that prioritize productivity.
[0180] Alternatively, the thickness of the TD stretched film can be greater than that of the MD stretched film. While the TD stretched film ensures thickness, it is possible to use an MD stretched film that is thinner than the TD stretched film and has higher physical properties such as tensile strength in the MD direction, allowing the substrate thickness and properties to be adjusted within the desired range. Conversely, the thickness of the MD stretched film can be made greater than that of the TD stretched film by adjusting the thickness and stretching ratio. While TD stretched film tends to have lower physical properties such as tensile strength than MD stretched film, it is particularly advantageous in terms of using a thinner film because it achieves higher stretch ratios in the TD direction. To adjust the substrate thickness, the TD stretched film can be placed on the substrate surface and laminated with the MD stretched film. For example, a laminated structure such as TD stretched film - MD stretched film - TD stretched film can be used, with the TD stretched film on the outside.
[0181] Alternatively, at least one of the MD stretched film and the TD stretched film can be laminated continuously. For example, the TD stretched film can be laminated continuously in the following order: MD stretched film - TD stretched film - TD stretched film - MD stretched film, or in the following order: TD stretched film - MD stretched film - MD stretched film - TD stretched film. It is believed that films with roughly parallel anisotropy of linear expansion coefficients have more sites for bonding between molecules, thus improving the bonding strength between the films. In this way, a substrate having a bonding interface formed by adjacent films having parallel orientation directions within the laminate can provide improved bonding strength in the thickness direction.
[0182] As multiple films, films having different weights per unit area (hereinafter referred to as area density) may also be used. For example, a film stack may be formed in a manner including a high-area-density film having a certain area density and a low-area-density film having an area density less than 0.7 times the area density of the high-area-density film. Furthermore, it may be stacked in a manner that the small CTE direction of the low-area-density film crosses the small CTE direction of the high-area-density film. At this time, the distance between the thickness center of the substrate and the thickness center of the low-area-density film may also be configured to be greater than the distance between the thickness center of the substrate and the thickness center of the high-area-density film. In the case where each film has a small uneven thermal expansion characteristic within the plane, warping of the substrate or substrate may occur, but by arranging the high-area-density film, which is more susceptible to unevenness, at a position close to the thickness center of the substrate, warping, etc. can be reduced. Particularly preferred is, as Figure 3 As shown in the laminated structure, the substrate is arranged so that the center of the thickness is located in the thin film with high area density in cross-sectional view.
[0183] Furthermore, when stacking thin films with low area density and high area density, the number of thin films with low area density or the number of layers composed of thin films can be greater than the number of thin films with high area density. This provides a substrate that not only allows fine-tuning of the thermal expansion characteristics of the substrate by increasing or decreasing the number of thin films with low area density, but also improves reliability by reducing the number of film-to-film interfaces through the use of high area density films.
[0184] (compression)
[0185] The film stack obtained as described above may also be further compressed. A film stack in which multiple films are simply stacked may not have sufficient bonding strength between the films. In the compression step, by compressing the stack in the thickness direction, the bonding between the films can be strengthened.
[0186] Compression can be performed by, for example, applying pressure by clamping the film laminate with a press, or by continuously applying pressure by passing the film laminate through a pair or more pairs of rollers while clamping the film laminate. The temperature during compression can be, for example, 40° C. to 340° C.
[0187] The pressure during compression is appropriately adjusted based on the thickness and density of the desired substrate. When compression is performed using a press, the pressure is exemplified by a range of 5 MPa to 400 MPa.
[0188] The thickness of the compressed substrate can be, for example, 5 μm or more and 250 μm or less, preferably 10 μm or more and 200 μm or less, more preferably 20 μm or more and 200 μm or less. Preferably, by compression, the pore size and distribution in the porous PTFE film change and become high-density. If it is a PTFE substrate, its density can also be compressed to 1.9 g / cm 3 Above and 2.4g / cm 3 the following.
[0189] In stretched PTFE, the high density achieved by compression makes the characteristic porous structure composed of nodes and fibrils invisible even under an electron microscope. However, as a result of the process not exceeding the crystalline melting temperature, the thermal expansion characteristics brought about by the linear molecular chains contained in the fibrils are maintained or further improved.
[0190] The high density achieved through compression can be seen as the matrix resin itself filling the pores of the porous expanded PTFE. This not only improves electrical properties but also brings many advantages, such as uniform properties and excellent reliability.
[0191] Figure 6 This graph shows the relationship between the calculated linear expansion coefficient of the substrate calculated based on the linear expansion coefficient of the thin film and the actually measured linear expansion coefficient of the substrate, for various substrates composed of multiple sample levels produced by varying the fluororesin used as the material, stretching conditions, film lamination conditions, and / or compression conditions.
[0192] The calculated linear expansion coefficient is the CTE of the film constituting the substrate S With CTE L When the substrate is composed of multiple films, the average value of the film with the smallest value is used. The measured linear expansion coefficient is the CTE of the substrate. D1 With CTE D2 The average value of the measured values of the respective linear expansion coefficients is obtained. Based on the linear expansion coefficients of each substrate obtained in this way, the x-axis of the graph is the calculated linear expansion coefficient and the y-axis is the measured linear expansion coefficient, and the resulting graph is as follows: Figure 6 .
[0193] Figure 6 The solid line L1 in the figure indicates y = x. The majority of samples were horizontally plotted in the region y < x. This confirms that the substrate described in the present application is not only improved in isotropy by cross-laminating only constituent films having anisotropic linear expansion coefficients, but also exhibits a measured linear expansion coefficient that is further suppressed by the calculated linear expansion coefficient calculated from the constituent films.
[0194] It should be noted that some samples are located at a position close to the solid line L1 y = x. The existence of measurement unevenness is not denied. In addition, the CTE of each of the multiple films constituting the substrate is taken into account in the calculation of the linear expansion coefficient. S With CTE L Using the minimum value among the average values as the representative value may cause deviations, etc.
[0195] and, Figure 6 The solid line L2 in shows y = 0.93x. It was confirmed that even including the above-mentioned variations and calculation deviations, the relationship y < 0.93x was satisfied at most sample levels.
[0196] (Conductor Layer Formation)
[0197] As described above, it is possible to produce a substrate that maintains excellent electrical properties and has high physical properties required of a substrate.
[0198] Furthermore, as needed, a conductor layer composed of a metal film or the like can be formed on one or both surfaces of the obtained substrate to form a conductor layer-forming substrate. A conductor layer-forming substrate using a copper film having excellent electrical properties as the conductor layer is preferably used as a member for manufacturing wiring boards.
[0199] The metal film can be formed, for example, by applying pressure to a metal film such as copper foil while overlapping the substrate, thereby pressing the metal film and the substrate together. Pressing can be achieved by applying pressure as a surface by clamping the substrate with a press, or by continuously applying pressure as a line by passing the substrate between one or more pairs of rollers while being clamped. Alternatively, a substrate with a metal layer formed on its surface can be obtained by growing a metal film on the substrate using other methods such as plating.
[0200] Furthermore, it is preferable to control the temperature of the resin material used, preferably during all steps from mixing to conductor layer formation, or at least during the steps from extrusion to film lamination, so that the temperature does not exceed the crystalline melting temperature. This is because melting may reduce the molecular orientation, resulting in a film with the desired thermal expansion characteristics not being obtained or being lost. For example, in the case of PTFE, it is preferable to control the temperature to not exceed 340°C, and more preferably not exceed 330°C, throughout all these steps.
[0201] Next, an example of a method for manufacturing a wiring board using the above-mentioned substrate will be described. A substrate is prepared, and a conductor pattern is formed on the substrate surface using a known method. The conductor pattern is formed using a subtractive method, whereby a copper film previously formed on the substrate surface is etched away except for the areas remaining as the conductor pattern. An additive method, whereby a conductor layer is deposited only in the areas designated as the conductor pattern through plating or other methods, can also be used. Photolithography techniques using a resist containing a photosensitive resin can also be used to define the etching and plating areas.
[0202] In the case of a double-sided substrate, after forming a via hole through the substrate, a via conductor can be formed within the via hole. This via conductor electrically connects the conductive pattern on the upper side of the substrate to the conductive pattern on the lower side of the substrate. Examples of methods for forming a via conductor include plating and filling with a conductive paste.
[0203] If necessary, a protective insulating layer may be formed on the conductive pattern to protect the conductive pattern.
[0204] Example
[0205] A paste is prepared by adding an auxiliary agent to commercially available PTFE fine powder and stirring. The paste is preformed by compacting it in a die and then continuously extruded through an extrusion die to form a long sheet with MD longer than TD.
[0206] The resulting sheet is rolled to a specified thickness using roller pressure. Furthermore, stretching in the MD and / or TD is performed while adjusting the stretching ratio in each direction to produce an anisotropic film with a specified linear expansion coefficient. During stretching, heating is applied as appropriate depending on the desired stretching ratio. The temperature of the sheet and film, including rolling, stretching, and removal of additives through heating, is controlled to be below 340°C.
[0207] Since the density of the film changes between the porous state before compression and the solid state after compression, the weight per unit area (area density) is used as a method to determine the amount of resin. The test piece is cut out by pressing a punch with a specified inner diameter at room temperature without applying tensile stress to the film, film laminate or substrate to be measured. Then, the weight (g) of the cut test piece is measured and divided by the area calculated based on the specified inner diameter to calculate the weight per unit area (g / m 2 ).
[0208] The volume of the test piece can be calculated by measuring the thickness of the test piece with a micrometer, etc. The density of the film can be calculated from the measured weight and the calculated volume.
[0209] (Linear Expansion Coefficient Measurement Method)
[0210] The coefficient of linear expansion (CTE) represents the ratio of the change in length to the thermal expansion coefficient. CTE is measured using mechanical thermal analysis (TMA) according to ISO 11359-2. The TMA method involves stretching a test sample and placing it on a probe. The CTE is determined by measuring the change in length caused by the expansion of the test sample while the sample is held under a constant load and heated. CTE is calculated using the following formula (1).
[0211] CTE=(ΔL / L0)×(1 / ΔT)×10 6 Formula (1)
[0212] Here, ΔL represents the change in length of the measurement sample when the temperature changes from temperature T1 to temperature T2, L0 represents the length of the measurement sample before measurement, and ΔT represents the temperature change (T2-T1)° C. A TMA4000SE manufactured by NETZSCH JAPAN was used as the measuring apparatus, and the measurement was performed under the following conditions.
[0213] Measurement temperature range: room temperature to 250°C
[0214] Heating rate: 10℃ / min
[0215] Tensile load: 0.5gf
[0216] Measurement sample shape: Rectangular 15mm long x 5mm wide (sample size for the chuck: 20mm long x 5mm wide)
[0217] The CTE in the temperature range of 30° C. to 250° C. in the longitudinal direction of the measurement sample was calculated.
[0218] (Example 1)
[0219] Polyflon F-106 (product name) manufactured by Daikin Industries, Ltd. was used as PTFE fine powder, and a sheet made of PTFE was prepared by a known method. The elongation ratio of the sheet was adjusted to form a sheet with a specific CTE. S / CTE L About -0.3, poor CTE L -CTE S The film is about 35 μm thick and has an anisotropy of about 180 ppm / °C. For measurement, a test piece was cut out of the film, and the linear expansion coefficient of the laminated body formed by stacking a predetermined number of layers so that the small CTE directions were in the same direction was measured. The result confirmed that the linear expansion coefficient CTE in the small CTE direction was 180 ppm / °C. S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -37ppm / ℃. LThe film density is approximately 140 ppm / °C.
[0220] Film sheets measuring 220 mm x 220 mm were cut from each of the anisotropic films, and ten of these sheets were stacked together to form a film laminate. Half of the ten sheets were oriented with the substrate D1 direction as the film's low CTE direction, while the remaining half were stacked with the substrate D2 direction, perpendicular to the substrate D1 direction, as the film's low CTE direction. This alternating orientation was achieved by stacking the sheets in alternate directions. The sheets were compressed using a press at 340°C and 10 MPa for 20 minutes, then cooled to room temperature to form a substrate.
[0221] The sample for CTE measurement was cut out from the substrate and the linear expansion coefficient was measured by TMA (Thermomechanical Analysis). D1 The linear expansion coefficient CTE of the substrate in the D2 direction is 47ppm / ℃. D2 The thermal expansion coefficient was 39 ppm / °C. Although no thermal expansion control material such as glass cloth was contained, a fluororesin base material was obtained in which thermal expansion in both the D1 direction and the perpendicular direction (D2 direction) thereof was suppressed.
[0222] (Example 2)
[0223] A film was prepared in the same manner as in Example 1 except that Polyflon F-121 (product name) manufactured by Daikin Industries, Ltd. was used as PTFE fine powder. The obtained film had a linear expansion coefficient CTE of 0.0447 W / m in the direction of small CTE. S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -36ppm / ℃. L is 139ppm / ℃, that is, the CTE S / CTE L -0.26, poor CTE L -CTE S The anisotropic film had an anisotropic property of 175 ppm / ° C. A substrate was prepared using the film under the same conditions as in Example 1.
[0224] The linear expansion coefficient CTE of the obtained substrate in the substrate D1 direction is D1 The linear expansion coefficient CTE of the substrate in the direction D2 perpendicular to the direction D1 is 38ppm / ℃. D2 The thermal expansion was 46 ppm / °C. Even when a different fluororesin was used, a fluororesin base material with suppressed thermal expansion in both the D1 direction and the perpendicular direction (D2 direction) thereof could be obtained as in Example 1.
[0225] (Example 3)
[0226] A sheet was prepared in the same manner as in Example 1. Three films were prepared using this sheet, consisting of film 3-1, film 3-2, and film 3-3 having different thicknesses and linear expansion coefficients. Furthermore, the compression step employed a roller clamping method rather than a press.
[0227] The measured values of the prepared films showed that the area density of film 3-1 was 8 g / m 2 , linear expansion coefficient CTE in the direction of small CTE S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -8ppm / ℃. L is 89ppm / ℃. That is, the film 3-1 has a specific CTE S / CTE L -0.09, poor CTE L -CTE S The anisotropy is 97. Similarly, the area density of film 3-2 is 16 g / m 2 , linear expansion coefficient CTE in the direction of small CTE S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -31ppm / ℃. L is 130ppm / ℃. That is, the film 3-2 has a specific CTE S / CTE L -0.24, poor CTE L -CTE S The anisotropy is 161ppm / ℃. The area density of film 3-3 is 54g / m 2 , linear expansion coefficient CTE in the direction of small CTE S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -28ppm / ℃. L is 128ppm / ℃. That is, the film 3-3 has a specific CTE S / CTE L -0.22, poor CTE L -CTE S The anisotropy is 156ppm / °C.
[0228] The thin film stack is symmetrically arranged in the order of film 3-1, film 3-1, film 3-2, film 3-3, film 3-2, film 3-1, and film 3-1 in the thickness direction from one substrate surface to the other substrate surface. The arrangement direction based on the anisotropy of the linear expansion coefficient of each film is such that the small CTE directions of all films 3-1 and 3-2 are parallel to each other, and these small CTE directions are stacked in a manner that is approximately orthogonal to the small CTE direction of film 3-3. The linear expansion coefficient CTE of the compressed substrate in the D1 direction is D1The linear expansion coefficient CTE of the substrate in the direction D2 perpendicular to the direction D1 is 52ppm / ℃. D2 It is 58ppm / ℃.
[0229] Even when films having very different compositions are combined to form a laminate, or when a compression method different from that of Example 1 is applied, a fluororesin substrate having suppressed thermal expansion in both the D1 direction and the perpendicular direction (D2 direction) can be obtained, similarly to Examples 1 and 2.
[0230] (Example 4)
[0231] A film 4 - 1 adjusted so that the direction of sheet or film flow, that is, MD, becomes the direction of small CTE and a film 4 - 2 adjusted so that TD becomes the direction of small CTE are prepared.
[0232] The area density of film 4-1 is 10g / m 2 , linear expansion coefficient CTE in the direction of small CTE S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -30ppm / ℃. L is 133ppm / ℃. That is, the film 4-1 has a specific CTE S / CTE L -0.23, poor CTE L -CTE S The anisotropy is 163ppm / °C.
[0233] The area density of film 4-2 is 26g / m 2 , linear expansion coefficient CTE in the direction of small CTE S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -30ppm / ℃. L is 134ppm / ℃. That is, the film 4-2 has a specific CTE S / CTE L -0.22, poor CTE L -CTE S The anisotropy is 164ppm / °C.
[0234] The films are stacked symmetrically in the thickness direction of the substrate, with three-layer film 4-1, three-layer film 4-2, and three-layer film 4-1 being stacked in this order from one surface of the substrate to the other. Based on the anisotropy of the linear expansion coefficient of each film, the arrangement directions are such that the small CTE directions of all six layers of film 4-1 are approximately parallel to each other, and the small CTE directions of all three layers of film 4-2 are approximately orthogonal to the small CTE direction of film 4-1.
[0235] The linear expansion coefficient CTE of the substrate in the D1 direction obtained by compression by a roller device D1 The linear expansion coefficient CTE in the D2 direction perpendicular to the D1 direction is 39ppm / ℃. D2 20ppm / ℃.
[0236] It was confirmed that even when a roll-to-roll method from extrusion to compression was employed, a fluororesin base material with suppressed thermal expansion in both the D1 direction and the perpendicular direction (D2 direction) could be stably obtained, similar to other examples.
[0237] (Example 5)
[0238] A film was formed by the same method as in Example 1. Test pieces were cut out from the film and stacked so that the small CTE directions were in the same direction. The linear expansion coefficient was measured. As a result, the linear expansion coefficient CTE in the small CTE direction was obtained. S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is 15.8ppm / ℃. L The film has a CTE of 73.1ppm / ℃. S / CTE L 0.22, poor CTE L -CTE S The anisotropy was 57.3 ppm / °C. That is, a film having a smaller degree of anisotropy than that of Example 1 was prepared.
[0239] A thin film laminate was formed from this film by the same method as in Example 1. The film was compressed using a press at a temperature of 330° C. and a pressure of 10 MPa for 20 minutes, and then cooled to room temperature to prepare a substrate.
[0240] A sample for CTE measurement was cut out from the substrate and the linear expansion coefficient was measured by TMA method. D1 The linear expansion coefficient CTE of the substrate in the D2 direction is 46.2ppm / ℃. D2 It is 44.8ppm / ℃.
[0241] (Example 6)
[0242] A film was formed by the same method as in Examples 1 and 5. Test pieces were cut out from the film and stacked so that the small CTE directions were in the same direction. The linear expansion coefficient was measured and the linear expansion coefficient CTE in the small CTE direction was obtained. S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -37.9ppm / ℃. L The film has a CTE of 129.0ppm / ℃. S / CTE L-0.29, poor CTE L -CTE S The anisotropy was 166.9 ppm / °C. That is, a film having a greater degree of anisotropy than that of Example 1 was prepared.
[0243] A thin film laminate was formed from this film by the same method as in Example 1. The film was compressed using a press at a temperature of 330° C. and a pressure of 10 MPa for 20 minutes, and then cooled to room temperature to prepare a substrate.
[0244] A sample for CTE measurement was cut out from the substrate and the linear expansion coefficient was measured by TMA method. D1 The linear expansion coefficient CTE of the substrate in the D2 direction is 37.0ppm / ℃. D2 It is 38.0ppm / ℃.
[0245] (Example 7)
[0246] A film was formed by the same method as in Example 2. Test pieces were cut out from the film and laminated so that the small CTE directions were in the same direction. The linear expansion coefficient was measured. As a result, the linear expansion coefficient CTE in the small CTE direction was obtained. S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is -43.3ppm / ℃. L The film has a CTE of 127.4ppm / ℃. S / CTE L -0.34, poor CTE L -CTE S The anisotropy was 170.7 ppm / °C. This means that the film was prepared to have a smaller ratio than that in Example 2, i.e., a film with significant anisotropy. This film was formed into a thin film laminate using the same method as in Example 1. This laminate was compressed using a press at a temperature of 330°C and a pressure of 10 MPa for 20 minutes, then cooled to room temperature to form a substrate.
[0247] A sample for CTE measurement was cut out from the substrate and the linear expansion coefficient was measured by TMA method. D1 The linear expansion coefficient CTE of the substrate in the D2 direction is 39.0ppm / ℃. D2 It is 38.9ppm / ℃.
[0248] (Example 8)
[0249] A film was formed by the same method as in Example 1 except that 650J (product name) manufactured by MCF was used as the PTFE fine powder. Test pieces were cut out from the film and stacked so that the small CTE directions were in the same direction. The linear expansion coefficient was measured. As a result, the linear expansion coefficient CTE in the small CTE direction was S The linear expansion coefficient CTE in the direction perpendicular to the large CTE is 10.7ppm / ℃. L The film has a CTE of 75.8ppm / ℃. S / CTE L 0.14, poor CTE L -CTE S The anisotropy was 65.1 ppm / ° C. A thin film laminate was formed from this film in the same manner as in Example 1. The laminate was compressed using a press at a temperature of 330° C. and a pressure of 10 MPa for 20 minutes and then cooled to room temperature to prepare a substrate.
[0250] A sample for CTE measurement was cut out from the substrate and the linear expansion coefficient was measured by TMA method. D1 The linear expansion coefficient CTE of the substrate in the D2 direction is 24.8ppm / ℃. D2 It is 34.2ppm / ℃.
[0251] Furthermore, through previous research, we have discovered that even when a film has different linear expansion coefficients in the small and large CTE directions, the linear expansion coefficient of the resulting substrate is dominated by the linear expansion coefficient of the film in the small CTE direction. This suggests that reducing the linear expansion coefficient of the film in the small CTE direction, while also increasing the linear expansion coefficient in the large CTE direction, is beneficial for reducing the thermal expansion of the substrate.
[0252] Similarly, it was discovered that by making a film having greater anisotropy such that the crossing angle of the small CTE directions (the angle formed by two small CTE directions) is close to 90 degrees, the thermal expansion of the substrate can be efficiently reduced.
[0253] As described above, according to the present invention, there are provided a substrate which maintains the excellent electrical properties of a fluororesin and stably possesses the high physical properties required of a substrate, and a wiring board using the substrate.
[0254] The present invention has been described above based on the embodiments, but the present invention is not limited to the above embodiments. Various modifications can be made to the above embodiments within the scope of the same or equivalent aspects of the present invention.
[0255] Furthermore, this application specification includes the following inventions.
[0256] A method for producing a substrate includes setting the linear expansion coefficient of a film to a predetermined anisotropy during stretching, and the method includes the following steps.
[0257] The method for manufacturing a substrate comprises preparing a fluororesin sheet, rolling the sheet, stretching the rolled sheet to form a film, and laminating the film to form a substrate. In the method,
[0258] The forming of the thin film includes stretching the thin film so that the thin film has a predetermined anisotropy of linear expansion coefficient, and the stacking of the plurality of thin films includes laminating the thin films so that directions of the anisotropy of the predetermined linear expansion coefficients of the thin films intersect.
[0259] Furthermore, the invention may be characterized in that the anisotropy of the predetermined linear expansion coefficient is determined so as to have a linear expansion coefficient required for a substrate formed by laminating the thin films.
[0260] A method for producing a substrate includes setting the anisotropy of the linear expansion coefficient of a film to a predetermined range during stretching, and the method includes the following steps.
[0261] A method for manufacturing a substrate includes preparing a fluororesin sheet, stretching the fluororesin sheet to form a film, and stacking the films to form a substrate. In the method, the step of preparing the fluororesin sheet includes managing the sheet so that its orientation is within a specified range, forming the film includes stretching the film in a direction and at a magnification having a specified anisotropic linear expansion coefficient, and stacking the multiple films includes stacking the films so that the directions of the anisotropy of the specified linear expansion coefficients of the films intersect.
[0262] Description of Reference Numerals
[0263] 100: substrate; 110 and 120: films; 200: wiring substrate; 220: wiring; 230: via.
Claims
1. A substrate used as a dielectric layer of a wiring substrate, wherein: The ratio of the fluororesin in the substrate is 90% by weight or more. The substrate includes a first film and a second film formed on the first film, The first film and the second film respectively have a first direction and a second direction perpendicular to the first direction in the extension plane of the substrate, and the linear expansion coefficient in the first direction within the range of 30°C to 250°C is set as CTE S , and the linear expansion coefficient in the second direction is set as CTE L When , the linear expansion coefficient has anisotropy that satisfies the following relationship: CTE S <CTE L Among them, CTE S and CTE L The unit is ppm / ℃, The first thin film and the second thin film are stacked such that the first direction of the first thin film and the first direction of the second thin film intersect with each other in a plan view of the substrate.
2. The substrate according to claim 1, wherein The linear expansion coefficient CTE of the first film in the first direction S The linear expansion coefficient CTE of the first film in the second direction is less than 30ppm / ℃ L It is above 30ppm / ℃.
3. The substrate according to claim 1, characterized in that The first thin film and the second thin film are stacked such that the first direction of the first thin film and the first direction of the second thin film are substantially perpendicular to each other in a plan view of the substrate.
4. The substrate according to claim 1, characterized in that The substrate has a first direction of the substrate and a second direction of the substrate perpendicular to the first direction of the substrate within the extension plane of the substrate, and the linear expansion coefficient of the substrate in the first direction within the range of 30°C to 250°C is set as CTE D1 , and the linear expansion coefficient of the substrate in the second direction is set as CTE D2 hour, The linear expansion coefficient CTE of the substrate in the first direction D1 and the linear expansion coefficient CTE of the substrate in the second direction D2 All are below 60ppm / ℃, among which, CTE D1 and CTE D2 The unit is ppm / ℃.
5. The substrate according to claim 1, characterized in that At 250 GHz and 22° C., the substrate has a relative dielectric constant of 2.3 or less and a dielectric loss tangent of 0.001 or less.
6. The substrate according to claim 1, characterized in that At 250 GHz and 22° C., the substrate has a relative dielectric constant of 2.3 or less and a dielectric loss tangent of 0.0003 or less.
7. The substrate according to claim 1, characterized in that The linear expansion coefficients CTE of the first film and the second film are S and linear expansion coefficient CTE L The minimum value of the average value is set to calculate the linear expansion coefficient, where CTE S and CTE L The unit is ppm / ℃, The substrate has a first direction of the substrate and a second direction of the substrate perpendicular to the first direction of the substrate within the extension plane of the substrate, and the linear expansion coefficient of the substrate in the first direction within the range of 30°C to 250°C is set as CTE D1 , and the linear expansion coefficient of the substrate in the second direction is set as CTE D2 When the linear expansion coefficient CTE D1 and linear expansion coefficient CTE D2 When the average value of is set as the measured linear expansion coefficient, The measured linear expansion coefficient is less than the calculated linear expansion coefficient, wherein CTE D1 and CTE D2 The unit is ppm / ℃.
8. The substrate according to claim 8, characterized in that The measured linear expansion coefficient is less than 0.93 times the calculated linear expansion coefficient.
9. A substrate used as a dielectric layer of a wiring substrate, wherein: The substrate is formed by laminating a plurality of thin films with fluororesin as the main component. The plurality of thin films each have a first direction and a second direction perpendicular to the first direction within the extension plane of the substrate, and the linear expansion coefficient in the first direction within the range of 30°C to 250°C is set as CTE S , and the linear expansion coefficient in the second direction is set as CTE L When , the linear expansion coefficient has anisotropy that satisfies the following relationship: CTE S / CTE L 0.5 Among them, CTE S and CTE L The unit is ppm / ℃, The plurality of thin films include a first thin film and a second thin film, The first thin film and the second thin film are stacked such that the first direction of the first thin film and the first direction of the second thin film intersect with each other in a plan view of the substrate.
10. The substrate according to claim 9, wherein When the linear expansion coefficient of the first film in the first direction is set as CTE S , and the linear expansion coefficient of the first film in the second direction is set to CTE L When , the following relationship is satisfied: CTE L -CTE S >50ppm / ℃ Among them, CTE S and CTE L The unit is ppm / ℃.
11. The substrate according to claim 9, characterized in that The first thin film and the second thin film are stacked such that the first direction of the first thin film and the first direction of the second thin film are substantially perpendicular to each other in a plan view of the substrate.
12. A substrate used as a dielectric layer of a wiring substrate, wherein: The substrate includes a first film and a second film formed on the first film, The first film and the second film both have fluororesin as a main component and have anisotropic linear expansion coefficients. In a plan view of the substrate, the first film and the second film are stacked so that the direction of the anisotropy of the linear expansion coefficient of the first film intersect with the direction of the anisotropy of the linear expansion coefficient of the second film. The substrate has a first direction of the substrate and a second direction of the substrate perpendicular to the first direction of the substrate within the extension plane of the substrate, and the linear expansion coefficient of the substrate in the first direction within the range of 30°C to 250°C is set as CTE D1 , and the linear expansion coefficient of the substrate in the second direction is set as CTE D2 When , the following relationship is satisfied: 0.7<CTE D1 / CTE D2 1.3 Among them, CTE D1 and CTE D2 The unit is ppm / ℃.
13. The substrate according to claim 12, characterized in that The linear expansion coefficient CTE of the first film in the first direction S The linear expansion coefficient CTE of the first film in the second direction is less than 30ppm / ℃ L It is above 30ppm / ℃.
14. The substrate according to claim 12, characterized in that The linear expansion coefficient CTE of the substrate in the first direction D1 and the linear expansion coefficient CTE of the substrate in the second direction D2 All are below 60ppm / ℃, among which, CTE D1 and CTE D2 The unit is ppm / ℃.
15. A substrate used as a dielectric layer of a wiring substrate, wherein: The substrate includes a first film containing a fluororesin as a main component and a second film formed on the first film and containing a fluororesin as a main component, The first film and the second film have the same chemical composition, In an observation plane of any cross section of the substrate perpendicular to the substrate surface, a difference between the refractive index of the first thin film and the refractive index of the second thin film is 0.01 or more.
16. The substrate according to claim 15, characterized in that The substrate has a first direction of the substrate and a second direction of the substrate perpendicular to the first direction of the substrate within the extension plane of the substrate, and the linear expansion coefficient of the substrate in the first direction within the range of 30°C to 250°C is set as CTE D1 , and the linear expansion coefficient of the substrate in the second direction is set as CTE D2 hour, The linear expansion coefficient CTE of the substrate in the first direction D1 and the linear expansion coefficient CTE of the substrate in the second direction D2 All are below 60ppm / ℃, among which, CTE D1 and CTE D2 The unit is ppm / ℃.
17. The substrate according to claim 15, characterized in that At 250 GHz and 22° C., the substrate has a relative dielectric constant of 2.3 or less and a dielectric loss tangent of 0.001 or less.
18. The substrate according to claim 15, characterized in that At 250 GHz and 22° C., the substrate has a relative dielectric constant of 2.3 or less and a dielectric loss tangent of 0.0003 or less.
19. A method for manufacturing a base material used as a dielectric layer of a wiring board, wherein: The method for manufacturing the substrate comprises: Prepare multiple films with fluororesin as the main component, The plurality of thin films are stacked to form a substrate, The plurality of films having the fluororesin as a main component respectively have a first direction and a second direction perpendicular to the first direction within the extension plane of the plurality of films, and include a first film and a second film, wherein the linear expansion coefficient in the first direction within the range of 30°C to 250°C is set as CTE S , and the linear expansion coefficient in the second direction is set as CTE L When the first film and the second film have anisotropy of linear expansion coefficient satisfying the following relationship: CTE S / CTE L 0.5 Among them, CTE S and CTE L The unit is ppm / ℃, Stacking the plurality of thin films to form a substrate includes stacking the plurality of thin films such that the first direction of the first thin film and the first direction of the second thin film intersect with each other in a plan view of the substrate.
20. The method for producing a substrate according to claim 19, wherein: The fluororesin is polytetrafluoroethylene, and the method includes setting the density of the substrate to 1.9 g / cm 3 Above and 2.4g / cm 3 The substrate was formed in the following manner.
21. A wiring board comprising: a base material according to any one of the group consisting of claim 1, claim 9, claim 12, and claim 15; and a conductor pattern formed on the base material.
Citation Information
Patent Citations
Porous polymer membrane reinforced composite
JP2006504848A
Fluororesin substrate
JP2013201344A
Printed wiring board and substrate for printed wiring board
JP2016046433A
Fluororesin film
WO2022071237A1