Preparation method of SiGe epitaxial layer and SiGe source drain structure

By introducing the SiGeC main body layer and the Si cap layer into the SiGe epitaxial layer, the lattice mismatch stress is alleviated, the critical thickness and carrier mobility of the SiGe epitaxial layer are improved, and the thickness limitation problem in the prior art is solved, and the performance of semiconductor devices is improved.

CN120453158APending Publication Date: 2025-08-08GTA SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510587093.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2025-08-08

AI Technical Summary

Technical Problem

In the existing SiGe epitaxial layer growth technology, the critical thickness is low, resulting in high dislocation density and incomplete crystal structure, which cannot meet the demand for thick SiGe epitaxial layers of high-performance devices, affecting carrier mobility and device performance.

Method used

By forming a SiGeC main body layer on the SiGe seed layer and forming a Si cap layer thereon, the Ge concentration and the introduction of carbon are controlled, the lattice mismatch stress is alleviated, the critical thickness of the epitaxial layer is increased, and the alloy band structure is adjusted to enhance carrier mobility.

Benefits of technology

The growth of SiGe epitaxial layer with a larger thickness is achieved, crystal defects are reduced, carrier mobility is improved, and the driving capability of semiconductor devices is enhanced. It is suitable for high-performance devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120453158A_ABST
    Figure CN120453158A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a SiGe epitaxial layer and a SiGe source drain structure. The preparation method comprises the following steps: forming a SiGe seed crystal layer on a silicon substrate; forming a SiGeC main body layer on the SiGe seed crystal layer, wherein the Ge concentration of the SiGeC main body layer is greater than that of the SiGe seed crystal layer; and forming a Si cap layer on the SiGeC main body layer. According to the preparation method of the SiGe epitaxial layer, the Ge concentration of the SiGe seed crystal layer and the SiGeC main body layer is controlled, and the strain of the SiGe alloy can be relieved by carbon at a replacement position in the ternary alloy SiGeC main body layer, so that the problem that the critical thickness of the SiGe epitaxial layer is relatively small due to stress generated by lattice mismatch is solved, the SiGe epitaxial layer with relatively large thickness can be obtained through the preparation method, and the preparation method is suitable for large-scale production. And meanwhile, the energy band structure of the SiGe alloy is adjusted by carbon, so that the mobility of a SiGe epitaxial layer carrier is improved, and the driving capability of a semiconductor device is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field related to semiconductor materials, and in particular to a method for preparing a SiGe epitaxial layer and a SiGe source-drain structure. Background Art

[0002] With the continuous evolution of integrated circuit technology, the size of wafers has gradually become smaller. At the same time, the standards for device operating speed and reliability are also constantly rising. In existing SiGe epitaxial layer growth technology, the critical thickness is generally low. When the thickness of the epitaxial layer exceeds the critical thickness, a large number of crystal defects such as dislocations will be generated. This is because there is a difference in the lattice constants of Si and Ge. As the Ge content increases, the lattice mismatch increases. During the growth process, the stress generated by the lattice mismatch will gradually accumulate. When the stress exceeds a certain limit, the stress will be released by generating dislocations, thereby limiting the critical thickness of the epitaxial layer. The lower critical thickness cannot meet the requirements of some high-performance devices for thick SiGe epitaxial layers. For example, in high-speed transistors, thick SiGe epitaxial layers can provide greater stress, thereby improving carrier mobility.

[0003] The crystal quality of SiGe epitaxial layers produced using existing technologies often fails to meet the requirements of high-end applications. This is primarily manifested in high dislocation density and an incomplete crystal structure. On the one hand, limitations of the growth process make it easy for impurities and defects to be introduced during epitaxial layer growth. On the other hand, the simple growth structure cannot effectively alleviate the stress generated by lattice mismatch, leading to the generation and propagation of defects such as dislocations. Poor crystal quality further affects the electrical properties of the SiGe epitaxial layer, such as reduced carrier mobility and increased leakage current, thereby reducing device performance and reliability.

[0004] How to solve the many problems existing in the existing SiGe epitaxial layer growth technology in terms of critical thickness (the maximum thickness of SiGe grown on the substrate without generating misfit dislocations), crystal quality and composition control, in order to meet the demand for high-performance SiGe epitaxial layers in the continuous development of semiconductor technology has become a topic in the field of semiconductor technology.

[0005] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present invention, and therefore may include information that does not constitute prior art known to those skilled in the art. Summary of the Invention

[0006] In response to the problems in the prior art, the purpose of the present invention is to provide a method for preparing a SiGe epitaxial layer and a SiGe source-drain structure. This preparation method can break through the traditional critical thickness limitation of the SiGe epitaxial layer by adding carbon to relieve the strain in the germanium silicon material and the influence of carbon on the alloy band structure, thereby improving the mobility of carriers in the SiGe epitaxial layer and enhancing the driving capability of the semiconductor device. The high-performance SiGe epitaxial layer can meet the requirements of higher-performance devices.

[0007] Specifically, the first aspect of the present invention provides a method for preparing a SiGe epitaxial layer, the method comprising the following steps:

[0008] forming a SiGe seed layer on a silicon substrate;

[0009] forming a SiGeC bulk layer on the SiGe seed layer, wherein the Ge concentration of the SiGeC bulk layer is greater than the Ge concentration of the SiGe seed layer;

[0010] A Si cap layer is formed on the SiGeC body layer.

[0011] According to the first aspect of the present invention, the Ge concentration of the SiGeC body layer is 20% to 50%.

[0012] According to the first aspect of the present invention, the thickness of the SiGeC main layer is 50 nm to 200 nm.

[0013] According to the first aspect of the present invention, the Ge concentration of the SiGeC body layer gradually increases along the thickness direction of the silicon substrate.

[0014] According to the first aspect of the present invention, the Ge concentration in the SiGe seed layer is 10% to 30%; and / or

[0015] The thickness of the SiGe seed layer is between 1 nm and 50 nm.

[0016] According to the first aspect of the present invention, the SiGe seed layer is formed by one of atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition, plasma enhanced chemical vapor deposition or molecular beam epitaxy; and / or

[0017] The process temperature of the SiGe seed layer is between 450°C and 1000°C.

[0018] According to the first aspect of the present invention, the SiGeC main layer is formed by a chemical vapor deposition process;

[0019] Wherein, the silicon source is dichlorosilane, silane and / or disilane;

[0020] The germanium source is germane;

[0021] The carbon source is methane, ethylene, tetramethylsilane, diborane and / or tetraborane.

[0022] According to the first aspect of the present invention, the process temperature of the SiGeC main layer is between 500°C and 1200°C.

[0023] A second aspect of the present invention provides a SiGe source-drain structure obtained by using the method for preparing a SiGe epitaxial layer described in the first aspect.

[0024] According to a second aspect of the present invention, the SiGe source-drain structure is formed in a trench in a silicon substrate, and the cross section of the sidewall of the trench is Σ-shaped, comprising:

[0025] a SiGe seed layer formed on an inner surface of the trench;

[0026] a SiGeC bulk layer formed on the SiGe seed layer;

[0027] a Si cap layer formed on the SiGeC body layer;

[0028] Wherein, the thickness of the SiGeC main layer is between 80nm and 200nm.

[0029] Compared with the prior art, the preparation method of the SiGe epitaxial layer of the present invention can relieve the strain of the SiGe alloy by controlling the Ge concentration of the SiGe seed layer and the SiGeC main layer, and the carbon in the substitution position in the ternary alloy SiGeC main layer, thereby solving the problem of the small critical thickness of the SiGe epitaxial layer due to the stress generated by the lattice mismatch. The preparation method can obtain a SiGe epitaxial layer with a larger thickness. At the same time, the carbon adjusts the band structure of the SiGe alloy, improves the mobility of the carriers in the SiGe epitaxial layer, and enhances the driving capability of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The drawings herein are incorporated into and constitute a part of the specification, illustrating embodiments consistent with the present application, and together with the specification, are used to explain the principles of the present application. By reading the detailed description of the non-limiting embodiments with reference to the following drawings, other features, purposes and advantages of the present invention will become more apparent. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work. In addition, the drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same figure numbers in the figures represent the same or similar parts, and their repeated descriptions will be omitted. Some of the block diagrams shown in the drawings are functional entities and do not necessarily correspond to physically or logically independent entities.

[0031] Figure 1 Schematic diagram of a method for preparing a SiGe epitaxial layer according to an embodiment of the present invention;

[0032] Figures 2 to 5 Schematic diagram of the structure of a silicon substrate corresponding to each step when a SiGe source-drain structure is prepared using a method for preparing a SiGe epitaxial layer according to an embodiment of the present invention;

[0033] Figure 6 FIG. 1 is a transmission electron microscope (TEM) image of a SiGe source-drain structure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0034] The following describes the embodiments of the present invention through specific examples. Those skilled in the art will readily understand the other advantages and benefits of the present invention from the disclosure herein. The present invention may also be implemented or applied in various other specific embodiments, and the various details of the present invention may be modified or altered based on different viewpoints and application systems without departing from the spirit of the present invention. It should be noted that the embodiments and features of the embodiments of the present invention may be combined with each other unless they conflict.

[0035] The following is a detailed description of the embodiments of the present invention with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention. The present invention can be embodied in many different forms and is not limited to the embodiments described herein.

[0036] In the description of the present invention, reference to the terms "one embodiment," "some embodiments," "examples," "specific examples," or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with that embodiment or example are included in at least one embodiment or example of the present invention. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples. Furthermore, those skilled in the art may combine and integrate different embodiments or examples described in the present invention, as well as features of different embodiments or examples, unless otherwise inconsistent.

[0037] In order to clearly describe the present invention, components not related to the description are omitted, and the same or similar components are denoted by the same reference numerals throughout the specification.

[0038] Throughout this specification, when a device is said to be "connected" to another device, this includes not only "direct connection" but also "indirect connection" with other elements interposed therebetween. Furthermore, when a device is said to "include" a certain component, unless otherwise stated, this does not exclude the inclusion of other components but rather implies that the device may include other components.

[0039] When a device is said to be "on" another device, it may be directly on the other device, but there may also be other devices between it. In contrast, when a device is said to be "directly on" another device, there are no other devices between it.

[0040] Although the terms first, second, etc. are used in some instances herein to represent various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another. For example, the first interface and the second interface, etc. are represented. Furthermore, as used in this article, the singular forms "one," "an," and "the" are intended to also include the plural forms, unless there is a contrary indication in the context. It should be further understood that the terms "comprise," "include," and "include" indicate the presence of features, steps, operations, elements, components, items, types, and / or groups, but do not exclude the presence, occurrence, or addition of one or more other features, steps, operations, elements, components, items, types, and / or groups. The terms "or" and "and / or" used herein are interpreted as inclusive, or mean any one or any combination. Therefore, "A, B, or C" or "A, B, and / or C" means "any of the following: A; B; C; A and B; A and C; B and C; A, B, and C." Exceptions to this definition only occur when the combination of elements, functions, steps, or operations is inherently mutually exclusive in some way.

[0041] The technical terms used herein are intended only to refer to specific embodiments and are not intended to limit the present invention. The singular as used herein also includes the plural unless expressly stated to the contrary. The term "comprising" as used in this specification specifies specific features, regions, integers, steps, operations, elements, and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.

[0042] Although not defined differently, all terms used herein, including technical and scientific terms, have the same meanings as those generally understood by those skilled in the art to which this invention belongs. Terms defined in commonly used dictionaries are to be interpreted as having meanings consistent with the relevant technical literature and current knowledge, and unless otherwise defined, they should not be overly interpreted as ideal or highly formalized meanings.

[0043] The following further illustrates the method for preparing the SiGe epitaxial layer and the SiGe source-drain structure of the present invention in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments are not intended to limit the scope of protection of the present invention.

[0044] Figure 1Schematic diagram of a method for preparing a SiGe epitaxial layer according to an embodiment of the present invention. Specifically, the method for preparing a SiGe epitaxial layer includes the following steps:

[0045] Step S100: forming a SiGe seed layer on a silicon substrate. In this step, the SiGe seed layer is formed on the exposed surface of the silicon substrate. When the preparation method is applied to the preparation of a SiGe source-drain structure, the surface in the trench in this step.

[0046] Step S200: forming a SiGeC bulk layer on the SiGe seed layer, wherein the Ge concentration of the SiGeC bulk layer is greater than the Ge concentration of the SiGe seed layer;

[0047] Step S300: forming a Si cap layer on the SiGeC body layer).

[0048] The present invention also provides a SiGe source-drain structure obtained using the above-mentioned method for preparing a SiGe epitaxial layer. The SiGe source-drain structure can be used to form the source and drain regions of a semiconductor field-effect transistor (FET), such as the source and drain regions of a P-type metal oxide semiconductor field-effect transistor (PMOS). The SiGe source-drain structure includes a SiGe seed layer formed on the inner surface of a trench, a SiGeC bulk layer formed on the SiGe seed layer, and a Si cap layer formed on the SiGeC bulk layer.

[0049] The following further illustrates the method for preparing the SiGe epitaxial layer by forming a SiGe source-drain structure in a P-type metal oxide semiconductor field effect transistor (PMOS), wherein the doping concentration of the silicon substrate 10 can be determined according to the structure of the target semiconductor device. Of course, a PMOS gate structure 20 is also formed on the silicon substrate 10, and trenches H are formed in the silicon substrate 10 on both sides of the gate structure 20, and the SiGe source-drain structure is formed in the trench H.

[0050] Figures 2 to 5 Schematic diagram of the structure of the silicon substrate corresponding to each step when preparing a SiGe source-drain structure using a method for preparing a SiGe epitaxial layer according to an embodiment of the present invention. Figure 2 As shown, the sidewall cross-section of the trench H in the silicon substrate 10 is Σ-shaped, i.e., the sidewall of the trench H is stepped and recessed, with a depth of 10 nm to 30 nm. The trench H with Σ-shaped sidewalls can be obtained by forming a mask layer on the surface of the silicon substrate 10, patterning the mask layer to form a plurality of openings exposing the surface of the silicon substrate 10, and finally performing a dry etching process superimposed on a wet etching process by adjusting the parameters of each etching stage, such as the selected etching gas / etching liquid. The specific parameters are not further described here.

[0051] exist Figure 2The silicon substrate 10 with the groove H performs step S100 to form a SiGe seed layer 51 on the silicon substrate (groove H). The SiGe seed layer 51 is formed on the bottom wall of the groove H and the Σ-shaped side wall. It should be noted that the lattice constants of the III-V material layer and the silicon substrate are quite different. The epitaxial formation of the III-V material layer on the surface of the silicon substrate as the channel layer will form more defects in the channel layer, thereby affecting the performance of the effect transistor finally formed. As the starting layer for the growth of the entire SiGe epitaxial layer, the SiGe seed layer 51 needs to provide a good crystal nucleus and lattice matching foundation for subsequent growth. Appropriate Ge concentration and thickness can reduce the lattice mismatch between the substrate and the subsequent growth layer, reduce the generation of defects such as dislocations, and thus improve the crystal quality of the epitaxial layer. On the other hand, the lattice mismatch between the SiGe epitaxial layer and Si depends on the concentration of germanium (Ge) in SiGe (i.e., Si 1-x Ge x (x value in [ 0 ]), that is, the higher the concentration of germanium in the SiGe seed layer, the higher the lattice mismatch between it and the substrate. Preferably, the Ge concentration (the atomic percentage of Ge atoms in SiGe) in the SiGe seed layer 51 covering the trench H (bottom and sidewalls) is 10% to 30%. More preferably, the Ge concentration in the SiGe seed layer 51 is 10% to 20%. The lattice mismatch between the SiGe seed layer 51 with the above Ge concentration and the silicon substrate 10 can be less than 1% to 1%.

[0052] For a SiGe seed layer 51 with a lattice mismatch of less than 1% or less, the thickness of the SiGe seed layer 51 as a buffer layer can be between 1 nm and 100 nm. The SiGe seed layer 51 as an initial transition layer can better alleviate the lattice mismatch between the silicon substrate and the subsequent growth layer, reducing the generation of dislocations and defects. Preferably, the thickness of the SiGe seed layer 51 is between 1 nm and 50 nm, such as 10 nm or 20 nm.

[0053] For example, the SiGe seed layer 51 can be formed using atmospheric pressure chemical vapor deposition (APCVD), low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), or molecular beam epitaxy (MBE). The growth process of the SiGe seed layer can be selected according to the situation. For example, atmospheric pressure chemical vapor deposition (APCVD) has a faster growth rate and is suitable for large-scale production; low pressure chemical vapor deposition (LPCVD) can obtain a SiGe seed layer with better uniformity; plasma enhanced chemical vapor deposition (PECVD) can grow at a lower temperature, reducing the impact on the silicon substrate 10; and molecular beam epitaxy (MBE) can achieve precise control at the atomic level. The growth process temperature of the SiGe seed layer 51 is between 450°C and 1000°C. The process for growing the SiGe seed layer 51 can be optimized according to specific production requirements and equipment conditions.

[0054] After obtaining the SiGe seed layer 51 of the SiGe source-drain structure, step S200 is performed to form a SiGeC main layer 52 on the SiGe seed layer 51. Figure 3 Among Group IVA elements, the atomic radius increases gradually from carbon (C), silicon (Si), to germanium (Ge). The Si-Ge bond is longer than the Si-Si bond, while the Si-C bond is shorter than the Si-Si bond. Therefore, when a SiGe epitaxial layer is grown on a silicon substrate, a certain degree of compressive strain is generated within the epitaxial layer; conversely, when SiC is grown on a silicon substrate, tensile strain is generated. SiGeC ternary alloys have sparked widespread research interest, and the substitutional carbon element plays two primary roles: Since the atomic radius of carbon is much smaller than that of silicon and germanium, its introduction can alleviate the compressive strain caused by the difference in atomic radius between germanium and silicon, increasing the critical thickness of the epitaxial layer and creating favorable conditions for epitaxial layer growth. Carbon also has the ability to regulate the band structure of the germanium-silicon alloy. The lattice constant of diamond is 52% smaller than that of silicon crystals, and the atomic radius of carbon is also smaller. Therefore, when carbon is incorporated into a SiGe epitaxial layer and replaces some Ge atoms, it increases the critical thickness of the epitaxial layer, thereby achieving a balance between defect control and the functional requirements of semiconductor devices.

[0055] The Ge concentration of the SiGeC main layer 52 in step S200 is greater than the Ge concentration of the SiGe seed layer 51. Figure 4 In step S200, a chemical vapor deposition process such as atmospheric pressure chemical vapor deposition (APCVD), low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition, etc. can be used to form a SiGeC main layer, wherein the silicon source can be dichlorosilane (SiH2Cl2), silane (SiH4) and / or disilane (Si2H6), the germanium source can be germane (GeH4); the carbon source can be methane (CH4), ethylene (C2H4), tetramethylsilane (Si(CH3)4), diborane (B2H6) and / or tetraborane (B4H 10 The growth process temperature of the SiGeC bulk layer 52 is between 500° C. and 1200° C. The composition and properties of the SiGeC bulk layer 52 can be precisely controlled by using the above-mentioned combination of gases.

[0056] The Ge concentration of the SiGeC main layer 52 can be 20% to 50%. For example, when the Ge concentration of the SiGe seed layer 51 is 10%, the Ge concentration of the SiGeC main layer 52 can be 20%; when the Ge concentration of the SiGe seed layer 51 is 20%, the Ge concentration of the SiGeC main layer 52 can be 30% or 40%. It is sufficient that the Ge concentration of the SiGeC main layer 52 is greater than the Ge concentration of the SiGe seed layer 51. No limitation is made here.

[0057] In order to reduce the lattice mismatch, in some embodiments, the Ge concentration of the SiGeC main layer 52 is gradually increased along the thickness direction of the silicon substrate 10. For example, when the Ge concentration of the SiGe seed layer 51 is 10%, the thickness of the SiGeC main layer 52 is 100nm, and the Ge concentration can be gradually increased from 20% to 50% along the thickness direction of the SiGeC main layer 52. The control of the Ge concentration of the SiGeC main layer 52 can be achieved by controlling (gradually changing) the flow rate of the silicon source and the germanium source or the ratio between the two. The gradual Ge concentration design allows the SiGe main layer to gradually release the lattice mismatch stress during the growth process, avoiding stress concentration and the generation of a large number of dislocations. At the same time, suitable growth gas and temperature conditions help to control the growth direction and quality of the crystal, so that the SiGe main layer can maintain a good crystal structure even when it is thicker, thereby increasing the critical thickness of the SiGe main layer and reducing the lattice defects in the SiGe main layer.

[0058] In one embodiment, plasma enhanced chemical vapor deposition (PECVD) of the SiGeC main layer 52 is used. The silicon source may be dichlorosilane, the carbon source may be methane, the flow rate of dichlorosilane is 20 sccm to 120 sccm, the flow rate of germane is 7 sccm to 100 sccm, the flow rate of methane is 7 sccm to 50 sccm, the growth temperature is 500-1100°C, the growth time is 200S to 1500S, and the SiGe seed layer 51 before the SiGeC main layer 52 and the SiGeC main layer are formed. The carbon in the substitutional position in layer 52 can relieve the strain of SiGe, resulting in a SiGeC bulk layer with a thickness of up to 200 nm. Compared to existing SiGe epitaxial layers with a critical thickness of 30 nm to 70 nm, the preparation method of the present invention can increase the critical thickness of the SiGe epitaxial layer by 30% to 50%, resulting in a SiGeC bulk layer with a thickness of 50 nm to 200 nm. When used in the preparation of SiGe source-drain structures, the thickness of SiGeC bulk layer 52 can be between 80 nm and 200 nm. The thickness of SiGeC bulk layer 52 is adapted to the depth of trench H in silicon substrate 10.

[0059] In order to prevent the surface of the SiGeC main layer 52 in the trench from being oxidized or contaminated, step S300 is performed to form a Si cap layer 53 on the SiGeC main layer. Figure 5The Si cap layer 53 can be formed by chemical vapor deposition. A gaseous precursor (e.g., silane SiH4 or dichlorosilane SiH2Cl2) decomposes on the surface of the silicon substrate 10 after step S200, depositing silicon atoms to form the Si cap layer 53. The top surface of the Si cap layer 53 protrudes above the top of the trench H in the silicon substrate 10. The Si cap layer 53 can also improve the interface performance between the SiGeC epitaxial layer and subsequent structures in the semiconductor device, thereby enhancing the stability and reliability of the device.

[0060] Figure 6 This transmission electron microscope (TEM) image of a SiGe source-drain structure in accordance with an embodiment of the present invention shows that the SiGe epitaxial layer fabrication method of the present invention can overcome the traditional critical thickness limitation, resulting in a 90nm thick SiGe source-drain structure with minimal lattice defects in the SiGe bulk layer. Test results show that the carrier mobility in this SiGe source-drain structure can be increased by 20-50%. Furthermore, the thicker SiGe source-drain provides a larger contact area, reducing contact resistance (Rc) by 15-25% and increasing drive current (Ion) by 10-20%, making it suitable for high-frequency, low-power logic device applications.

[0061] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

[0062] The above is a further detailed description of the present invention in conjunction with specific preferred embodiments, and the specific implementation of the present invention should not be considered to be limited to these descriptions. For those skilled in the art of the present invention, without departing from the concept of the present invention, several simple deductions or substitutions can be made, which should be considered to fall within the scope of protection of the present invention.

Claims

1. A method for preparing a SiGe epitaxial layer, characterized in that: The preparation method comprises the following steps: forming a SiGe seed layer on a silicon substrate; forming a SiGeC bulk layer on the SiGe seed layer, wherein the Ge concentration of the SiGeC bulk layer is greater than the Ge concentration of the SiGe seed layer; A Si cap layer is formed on the SiGeC body layer.

2. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: The Ge concentration of the SiGeC main layer is 20% to 50%.

3. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: The thickness of the SiGeC main layer is 50nm-200nm.

4. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: The Ge concentration of the SiGeC main layer gradually increases along the thickness direction of the silicon substrate.

5. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: The Ge concentration in the SiGe seed layer is 10% to 30%; and / or The thickness of the SiGe seed layer is between 1 nm and 50 nm.

6. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: Forming the SiGe seed layer by one of atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition, plasma enhanced chemical vapor deposition or molecular beam epitaxy; and / or The process temperature of the SiGe seed layer is between 450°C and 1000°C.

7. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: forming the SiGeC main layer by a chemical vapor deposition process; Wherein, the silicon source is dichlorosilane, silane and / or disilane; The germanium source is germane; The carbon source is methane, ethylene, tetramethylsilane, diborane and / or tetraborane.

8. The method for preparing a SiGe epitaxial layer according to claim 1, wherein: The process temperature of the SiGeC main layer is between 500°C and 1200°C.

9. A SiGe source-drain structure, characterized in that: The method for preparing a SiGe epitaxial layer is used to obtain the epitaxial layer.

10. The SiGe source-drain structure according to claim 9, wherein: The SiGe source-drain structure is formed in a trench in a silicon substrate, and the cross section of the sidewall of the trench is Σ-shaped, comprising: a SiGe seed layer formed on an inner surface of the trench; a SiGeC bulk layer formed on the SiGe seed layer; a Si cap layer formed on the SiGeC body layer; Wherein, the thickness of the SiGeC main layer is between 80nm and 200nm.