Expandable rubber cable tube occluder and method of making same
By using graphene modification and microcapsule self-healing technology, an expandable rubber cable conduit plug with dual water-thermal response was developed, solving multiple challenges of sealing materials in existing technologies and achieving a long-term sealing effect with high efficiency and strong weather resistance.
Patent Information
- Application Number
- CN202511034456.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-25
- Publication Date
- 2026-01-27
- Estimated Expiration
- 2045-07-25
AI Technical Summary
Existing cable duct sealing materials suffer from problems such as a single response mechanism, low sealing efficiency, poor weather resistance, and lack of self-healing ability, making it difficult to effectively seal and use them for a long time in complex environments.
The graphene-modified dual-response expandable rubber cable conduit plug achieves efficient sealing and self-repair through water-heat dual-response expansion function and microcapsule self-healing system, combined with multiple anti-aging components.
It can quickly form an effective seal under various environmental conditions, has excellent weather resistance and self-healing ability, and has a service life of more than 20 years with stable sealing performance.
Smart Images

Figure CN120623658B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable and duct sealing technology, specifically to an expandable rubber cable and duct plug and its preparation method, applicable to cable and duct sealing and protection in the fields of power, communication, rail transportation, marine engineering and petrochemicals. Background Technology
[0002] Cable conduits are an indispensable component of various infrastructures, and their sealing and protection are crucial to ensuring the safe operation of these facilities. Currently, cable conduit sealing faces multiple challenges, including waterproofing and moisture prevention, fire resistance, flame retardancy, aging resistance, and adaptability to complex environments.
[0003] In existing technologies, commonly used cable conduit sealing methods mainly include: polyurethane foam sealing, mechanical compression sealing, water-swellable rubber sealing, and thermally expanding flame-retardant material sealing. However, these methods all have significant shortcomings:
[0004] 1. Although polyurethane foam has good filling properties, as pointed out in the research report of AC Cable Solutions (Why Using Expanding Polyurethane Foamin Cable Ducts is a Bad Idea, 2023), it has serious defects such as long-term shrinkage, poor aging resistance and difficulty in removal. Moreover, the foaming process is difficult to control and can easily cause pressure damage to the cable.
[0005] 2. Mechanical gland-type plugs, such as the product series from MISUMI in the United States, have reliable sealing performance, but the installation process is complicated, requires professional tools, has poor adaptability to irregular pipelines, and is relatively expensive.
[0006] 3. Water-swellable rubber sealing materials, such as those described in Geoforming's products and related patents US20130269787A1 and US9540501B2, respond well to moisture, but are prone to shrinkage and failure in dry environments, and are sensitive to temperature changes, with their expansion performance significantly reduced under high-temperature conditions.
[0007] 4. Thermal expansion flame retardant materials, such as FireFoam FM from Firewise in the UK, are mainly designed for fire scenarios. They have limited sealing performance in daily use and are expensive, making them unsuitable for large-scale applications.
[0008] In addition, existing sealing materials generally suffer from the following common problems:
[0009] 1. Single response mechanism: It responds either to moisture or temperature, making it difficult to cope with complex and ever-changing environmental challenges;
[0010] 2. Low sealing efficiency: It is difficult to form an effective seal during initial installation, and it often needs to expand before it can function.
[0011] 3. Poor weather resistance: Long-term exposure to harsh environments can easily lead to material aging and cracking, resulting in sealing failure;
[0012] 4. No self-healing ability: Once the sealing material is damaged, it cannot recover on its own and requires manual intervention to replace it.
[0013] Therefore, there is an urgent need to develop a new type of cable conduit sealing material and its preparation method that combines multiple response mechanisms, high sealing efficiency, excellent weather resistance and self-healing function. Summary of the Invention
[0014] The purpose of this invention is to overcome the shortcomings of the prior art and provide a graphene-modified dual-response expandable rubber cable conduit plug and its preparation method. The plug has water-heat dual-response expansion function, self-healing ability, excellent sealing efficiency and long-term weather resistance.
[0015] To achieve the above objectives, the technical solution provided by the present invention is as follows:
[0016] The expandable rubber cable conduit plug, by weight, is composed of the following components: 100 parts EPDM rubber, 0.5-1.0 parts graphene, 0.2 parts silane coupling agent KH550, 10 parts sodium carboxymethyl cellulose, 15 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 8 parts bentonite, 5 parts expandable graphite, 3 parts 4,4'-oxobisbenzenesulfonyl hydrazine foaming agent, 1 part zinc stearate, 2.5 parts peroxide DCP, 2 parts crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 5 parts modified nano-montmorillonite, 20 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, 8 parts naphthenic oil, 10 parts microcapsules, and 0.5 parts boron trifluoride diethyl ether complex catalyst.
[0017] The EPDM rubber contains 55% ethylene and 5% ENB (the third monomer); the graphene is multilayer graphene with 5-10 layers; the polyvinyl alcohol is PVA-1799; the bentonite is sodium bentonite with a particle size of 300 mesh; the expansion temperature of the expandable graphite is 180℃; the specific surface area of the fumed silica is 200 m² / g; the particle size of the light calcium carbonate is 1250 mesh; and the microcapsules are composed of an epoxy resin core and a urea-formaldehyde resin shell.
[0018] The expandable rubber cable conduit plug of this invention has a dual water- and heat-responsive expansion function. The water expansion rate reaches 200-300% after immersion at 25°C for 24 hours, and the thermal expansion rate reaches 150-200% after heating at 180°C for 10 minutes. The sealing pressure after expansion is not less than 1.0 MPa. Simultaneously, it has a self-healing function. When cracks appear on the material surface, the microcapsules rupture, releasing the epoxy resin core material, which cures and repairs the cracks under the action of a boron trifluoride diethyl ether complex catalyst, achieving a crack repair rate of not less than 85%.
[0019] The physical properties of the expandable rubber cable conduit plug are: density 1.15 ± 0.05 g / cm³. 3 The Shore A hardness is 45±5 degrees, the tensile strength is not less than 12MPa, the elongation at break is not less than 350%, the tear strength is not less than 25kN / m, and the compression set is not greater than 20% after 24 hours at 70℃.
[0020] Preferably, the weather resistance performance indicators of the expandable rubber cable conduit plug are as follows: after 168 hours of thermal aging at 150℃, the performance retention rate is not less than 80%; after 96 hours of ozone aging at 40℃ with a concentration of 50pphm, there is no cracking; after 1000 hours of UV aging at UV-B 313nm, the performance retention rate is not less than 85%; after 1000 hours of salt spray testing in 5% sodium chloride solution, there is no obvious corrosion; the operating temperature range is -40℃ to +150℃; and the service life is not less than 20 years.
[0021] The method for preparing the expandable rubber cable conduit plug includes the following steps:
[0022] A. Graphene pre-dispersion: Graphene, silane coupling agent KH550 and 10 parts naphthenic oil are mixed in a high-speed disperser at a speed of 3000 rpm and a temperature of 60℃ for 30 minutes. Then, ultrasonic treatment is performed at a power of 400W for 20 minutes.
[0023] B. Secret mixing process:
[0024] B1. First stage of mixing: At a temperature of 80℃, add EPDM rubber to a mixer and plasticize for 2 minutes, then add the pre-dispersed graphene mixture obtained in step A, then add zinc oxide and stearic acid, and mix for 5 minutes.
[0025] B2. Second stage of mixing: Raise the temperature to 100℃, add fumed silica, modified nano montmorillonite, and light calcium carbonate in batches and ensure full dispersion. Then add antioxidant TMQ, antioxidant 6PPD, hindered phenolic antioxidant 1076 and UV absorber UV-329. The mixing time is 8 minutes.
[0026] B3. Third stage of mixing: Raise the temperature to 120°C, add sodium carboxymethyl cellulose, sodium acrylate-acrylamide copolymer, polyvinyl alcohol, bentonite, expandable graphite and the remaining naphthenic oil, and mix for 5 minutes.
[0027] B4. Final mixing: Reduce the temperature to 60°C, add peroxide DCP, crosslinking agent TAIC, 4,4'-oxobisbenzenesulfonylhydrazine foaming agent, zinc stearate, microcapsules and boron trifluoride diethyl ether complex catalyst, mix lightly to avoid microcapsule breakage, and the mixing time is 3 minutes.
[0028] C. Refining and Shaping:
[0029] C1. Open milling process: The compound obtained in step B is placed on an open mill for open milling. The front roll temperature is 50℃, the rear roll temperature is 60℃, the roll gap is 2-3mm, the number of thin passes is 6-8, and the sheet thickness is 4-5mm.
[0030] C2. Extrusion molding: The extruder is used for molding, with a die head temperature of 80℃, a die body temperature of 70℃, a screw speed of 20-30 rpm, and an extrusion pressure of 8-10 MPa. The plugs are made according to the cable conduit size to produce specific specifications.
[0031] D. Vulcanization process:
[0032] D1. First stage vulcanization: The molded body obtained in step C is subjected to compression vulcanization at a temperature of 150℃, a pressure of 10MPa, and a time of t90+2 minutes, approximately 8-10 minutes.
[0033] D2. Second-stage vulcanization: The product after the first-stage vulcanization is placed in an oven for second-stage vulcanization at a temperature of 120℃ for 4 hours. The purpose is to eliminate internal stress and stabilize the dimensions.
[0034] E. Post-processing:
[0035] E1. Surface treatment: The vulcanized product is subjected to plasma treatment to improve the surface energy. The power is 100W and the time is 30 seconds.
[0036] E2. Pre-expansion treatment: Place the product in an environment of 80℃ and 85%RH for 2 hours, controlling the expansion rate to 10-15%, to obtain the final product.
[0037] Preferably, in the graphene pre-dispersion step, a combination of high-speed dispersion and ultrasonic treatment is used to form a uniform and stable dispersion of graphene in naphthenic oil, with the graphene agglomerate size being less than 2 μm and the dispersion uniformity reaching more than 90%.
[0038] Preferably, the internal mixing process adopts a segmented heating method, gradually increasing the temperature from 80°C to 120°C and then decreasing it to 60°C. The filler is added in batches, with each batch of filler not exceeding 30% of the total filler amount, to ensure the uniformity of the mixed rubber compound. The internal mixing rotor speed is 30-50 rpm, and the temperature of the internally mixed rubber compound exiting the mixing process does not exceed 130°C.
[0039] Preferably, the vulcanization process combines single-stage and two-stage vulcanization. The single-stage vulcanization uses compression molding, with the degree of vulcanization controlled above 95%. The vulcanization time is determined based on the t90 value determined by a Mooney vulcanizer. The two-stage vulcanization uses dry heat curing to achieve dimensional stability and performance uniformity of the product. The crosslinking density of the vulcanized product is 1.5 × 10⁻⁶. -4 Up to 2.0×10 -4 mol / cm 3 .
[0040] Preferably, the pre-expansion treatment in the post-processing step, by controlling the combination of temperature and humidity, enables the product to partially pre-expand, forming a gradient expansion structure. The internal density remains the same, while an expansion layer is formed on the outside. The thickness of the expansion layer is 0.5-1.0 mm, providing the product with an initial sealing pressure of not less than 0.3 MPa in actual applications. This ensures that a preliminary seal is formed immediately after installation, and further expansion to form a complete seal after contact with moisture or temperature increase.
[0041] The present invention also provides a method for preparing the above-mentioned expandable rubber cable conduit plug, including steps such as graphene pre-dispersion, internal mixing process, open mixing and molding, vulcanization process and post-treatment. By precisely controlling each process parameter, the stability and consistency of product performance are ensured.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1. Dual Response Mechanism: The sealing device of this invention possesses both water expansion and thermal expansion response functions, enabling it to rapidly form an effective seal under various environmental conditions and exhibiting strong adaptability. When exposed to water, water-expanding components such as sodium carboxymethyl cellulose and sodium acrylate-acrylamide copolymer absorb water and expand; when the temperature rises, expandable graphite and OBSH foaming agent work together to generate a thermal expansion effect, providing dual protection against environmental changes.
[0044] 2. Graphene Reinforcement Effect: By introducing a small amount of graphene (0.5-1.0 parts) and employing an innovative pre-dispersion technology, the mechanical strength, thermal conductivity, and anti-aging properties of the material are significantly improved. Experiments have shown that adding 0.5 parts of graphene can increase tensile strength by more than 30% and improve heat aging resistance by 40%.
[0045] 3. Self-healing function: An innovative microcapsule self-healing system is introduced. When the material is mechanically damaged, the microcapsules rupture, releasing epoxy resin, which cures and repairs cracks under the action of a catalyst, significantly extending the product's service life. Tests show that this system can achieve a crack repair rate of over 85%.
[0046] 4. Excellent weather resistance: Through the synergistic effect of multiple anti-aging components, the plugging device of the present invention retains more than 80% of its performance after 168 hours in a high-temperature environment of 150°C, and its performance retention rate is not less than 85% after 1000 hours of UV aging, with a service life of more than 20 years.
[0047] 5. High-efficiency sealing performance: The plug of this invention can provide a sealing pressure of not less than 0.3MPa upon initial installation, and the sealing pressure can reach more than 1.0MPa after expansion. The water tightness is leak-free under 2bar water pressure, and the air tightness is no more than 5% pressure drop in 24 hours under 0.5bar air pressure.
[0048] 6. Innovative manufacturing process: Through innovative processes such as multi-stage temperature-controlled mixing, graphene pre-dispersion, two-stage sulfidation, and pre-expansion treatment, the uniform dispersion and functional performance of each functional component in the matrix are ensured, significantly improving product performance and production efficiency. Attached Figure Description
[0049] Figure 1 This is a schematic diagram of the expandable rubber cable conduit plug of the present invention;
[0050] Figure 2 This is a process flow diagram of the preparation method of the present invention;
[0051] Figure 3 This is a water expansion performance curve of the expandable rubber cable conduit plug of the present invention;
[0052] Figure 4 This is a thermal expansion performance curve of the expandable rubber cable conduit plug of the present invention. Detailed Implementation
[0053] The following examples and... Figures 1-4 The present invention will be further described below, but the scope of protection of the present invention is not limited thereto.
[0054] The core of this invention lies in the innovative combination of graphene modification, a water-thermal dual-response system, and microcapsule self-healing function to develop a new generation of high-performance expandable rubber cable conduit plugs. The components of this invention and their functions are described in detail below:
[0055] 1. EPDM Rubber: As a matrix material, it provides basic elasticity and weather resistance. EPDM rubber with a preferred content of 55% ethylene and 5% ENB (the third monomer), such as JSR Corporation's EP57 or Dow Chemical's Nordel IP4770P, is preferred. This type of EPDM exhibits excellent ozone resistance, UV resistance, and high-temperature resistance, making it suitable for long-term outdoor use.
[0056] 2. Graphene: As a nano-reinforcing phase, it significantly improves the mechanical properties, thermal conductivity, and anti-aging properties of materials. This invention uses 5-10 layers of multilayer graphene, such as MX-G05 from Ningbo Moxi Technology Co., Ltd. in China or xGnP-M5 from XGSciences in the United States. Graphene forms a three-dimensional conductive network through π-π interactions and van der Waals forces with rubber molecular chains, while also serving as physical crosslinking points to enhance the strength of the material.
[0057] 3. Water-swelling system: Composed of sodium carboxymethyl cellulose, sodium acrylate-acrylamide copolymer, polyvinyl alcohol, and bentonite. Sodium carboxymethyl cellulose (e.g., CMC-Na from Shandong Futian Pharmaceutical Co., Ltd.) exhibits excellent water absorption and swelling properties; the sodium acrylate-acrylamide copolymer (e.g., Sokalan PA110S from BASF, Germany) rapidly swells in water to form a hydrogel; polyvinyl alcohol PVA-1799 (e.g., a product from Sinopec Jinling Petrochemical Co., Ltd.) acts as a water-retaining agent; and sodium bentonite (300 mesh Na-MMT) possesses interlayer water absorption and swelling properties. These components work synergistically to ensure rapid water absorption and swelling in humid environments, forming a reliable seal.
[0058] 4. Thermal Expansion System: Composed of expandable graphite and OBSH blowing agent. Expandable graphite (HT-180EG) can expand to 150-200 times its original volume at 180℃; 4,4'-oxobisbenzenesulfonyl hydrazine (OBSH) is a highly efficient blowing agent that decomposes to produce nitrogen gas at 155-165℃; zinc stearate acts as a blowing aid, adjusting the foaming temperature and efficiency. This system ensures rapid expansion in fire or high-temperature environments, forming a flame-retardant and heat-insulating layer.
[0059] 5. Self-healing system: Composed of epoxy resin core / urea-formaldehyde resin shell microcapsules and boron trifluoride diethyl ether complex catalyst. The microcapsules contain bisphenol A type epoxy resin, and the shell is urea-formaldehyde resin; the boron trifluoride diethyl ether complex (such as products from Shanghai Aladdin Biochemical Technology Co., Ltd.) acts as a latent catalyst for the epoxy resin. When the material is damaged, the microcapsules rupture to release the epoxy resin, which cures and repairs the cracks under the action of the catalyst, restoring the sealing performance.
[0060] The preparation method of epoxy resin core / urea-formaldehyde resin shell microcapsules is as follows: First, add 600 ml of deionized water to a 1000 ml four-necked flask, place it in a mechanical stirrer, and add 2.5 g of polyvinyl alcohol (PVA-217) and 0.5 g of sodium dodecylbenzenesulfonate as emulsifier and dispersant, respectively. Stir at 60 °C until completely dissolved. Then, thoroughly mix 50 g of bisphenol A type epoxy resin (such as DER331 from Dow Chemical Company) with 5 g of cyclohexane to prepare a core material solution. Under the condition of stirring speed of 800 rpm, slowly add the core material solution dropwise to the above aqueous solution to form a water-in-oil emulsion. Continue stirring for 30 minutes to stabilize the emulsion.
[0061] Next, the pH of the system was adjusted to 3.5-4.0 (using a 1% acetic acid solution), and 12.5g of urea, 0.5g of ammonium chloride, and 1.25g of resorcinol were added sequentially, and the mixture was stirred for 15 minutes to ensure complete dissolution. Then, 30g of formaldehyde solution (37wt%) was slowly added dropwise under stirring, the temperature was raised to 75°C, and the reaction was maintained at this temperature for 3 hours to carry out in-situ polymerization of the wall material. After cooling to room temperature, the microcapsules were washed three times sequentially with distilled water and ethanol, and the microcapsules were collected by vacuum filtration and vacuum dried at 40°C for 24 hours to obtain the final product. Preferably, the obtained microcapsules have an average particle size of 50-100μm, a wall thickness of 2-5μm, and a core material content of approximately 75-80wt%.
[0062] It is worth noting that reaction temperature and pH value significantly affect the morphology and structure of the microcapsules during their preparation. Appropriately increasing the reaction temperature can accelerate the polymerization rate of the wall material, but excessively high temperatures (>85°C) can lead to over-crosslinking and brittleness of the wall material. Maintaining a pH value within the range of 3.5-4.0 is beneficial for forming a dense and uniform wall material structure; excessively high or low pH values will affect the formation and strength of the wall material. Furthermore, the stirring speed directly affects the particle size distribution of the microcapsules; generally, stirring speeds within the range of 600-1000 rpm can yield microcapsules with ideal particle sizes.
[0063] 6. Reinforcing Filler System: Composed of fumed silica, modified nano-montmorillonite, and light calcium carbonate. Fumed silica (such as AEROSIL 200 from Evonik Industries, Germany) has a specific surface area of 200 m² / g, providing excellent reinforcing effect; modified nano-montmorillonite provides reinforcement and barrier properties; light calcium carbonate serves as a filler, reducing costs while improving dimensional stability.
[0064] The preparation method of modified nano-montmorillonite is as follows: First, add 100g of sodium-based montmorillonite (such as sodium-based montmorillonite produced by Liaoning Anshan Lier Mining Co., Ltd., with a CEC value of 90-100mmol / 100g) to 2000ml of deionized water, and stir at 8000rpm for 30 minutes using a high-speed disperser to obtain a uniform montmorillonite suspension. Then, transfer the suspension to an 80℃ water bath, continue stirring, and maintain a constant temperature.
[0065] Meanwhile, an organic modifier solution was prepared: 24g of cetyltrimethylammonium bromide (CTAB, ≥99%) was dissolved in 500ml of hot water (60℃) and stirred until completely dissolved. Then, under vigorous stirring (600rpm), the modifier solution was slowly added dropwise to the montmorillonite suspension, with the dropping rate controlled at 5-8ml / min. After the addition was complete, the reaction was continued at 80℃ for 4 hours to allow the organic modifier to fully intercalate into the montmorillonite layers.
[0066] After the reaction was complete, the mixture was cooled to room temperature, and the solid product was collected by centrifugation (4000 rpm, 15 minutes). The sample was washed alternately with ethanol and deionized water 3-5 times until no bromide ions were detected in the washings (using 0.1 mol / L silver nitrate solution). The washed sample was dried in a 70°C oven for 24 hours, then ground through a 200-mesh sieve to obtain modified nano-montmorillonite powder. Finally, it was dried in a vacuum drying oven at 105°C for 4 hours to obtain the final product.
[0067] The modified nano-montmorillonite prepared in this invention has an interlayer spacing of 1.85 nm (determined by XRD), an organic content of approximately 28 wt% (determined by TGA), and a specific surface area of 35 m². 2 / g. This modified nano-montmorillonite exhibits excellent compatibility with the rubber matrix and, after dispersion, forms a nanoscale exfoliated structure, significantly improving the material's mechanical properties, gas barrier properties, and flame retardancy. In particular, compared to unmodified montmorillonite, the dispersibility of the modified nano-montmorillonite in the rubber matrix is improved by approximately 200%, effectively avoiding the problem of easy agglomeration of traditional montmorillonite in rubber.
[0068] 7. Anti-aging system: Composed of antioxidant TMQ, antioxidant 6PPD, hindered phenolic antioxidant 1076, and UV absorber UV-329. These components work synergistically to provide comprehensive anti-aging protection, ensuring stable performance of the product over long-term use.
[0069] Next, the preparation method and embodiments of the present invention will be described in detail.
[0070] Example 1
[0071] The water-thermal dual-response expandable rubber cable conduit plug has the following component ratio (by weight): 100 parts EPDM rubber, 0.5 parts graphene, 0.2 parts silane coupling agent KH550, 10 parts sodium carboxymethyl cellulose, 15 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 8 parts bentonite, 5 parts expandable graphite, 3 parts OBSH foaming agent, 1 part zinc stearate, 2.5 parts peroxide DCP, 2 parts crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 5 parts modified nano-montmorillonite, 20 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, 8 parts naphthenic oil, 10 parts microcapsules, and 0.5 parts boron trifluoride ether complex catalyst.
[0072] The preparation method includes the following steps:
[0073] (1) Graphene predispersion: 0.5 parts graphene, 0.2 parts silane coupling agent KH550 and 3 parts naphthenic oil (3 / 8 of the total amount) were mixed in a high-speed disperser at 3000 rpm and 60°C for 30 minutes. Then, ultrasonic treatment was performed at 400W for 20 minutes to obtain a uniformly dispersed graphene predispersion.
[0074] (2) The refining process is divided into four stages.
[0075] First stage of mixing: Set the internal mixer temperature to 80℃, add 100 parts of EPDM rubber (ethylene content 55%, ENB content 5%), and plasticize for 2 minutes until a continuous strip is formed. Then add the graphene predispersant prepared in step (1) and continue mixing for 2 minutes. Next, add 5 parts of zinc oxide and 1 part of stearic acid, and mix until uniform, for a total time of about 5 minutes.
[0076] The second stage of mixing: Raise the internal mixer temperature to 100℃, and add 30 parts of fumed silica (specific surface area 200 m² / g), 5 parts of modified nano-montmorillonite, and 20 parts of light calcium carbonate (1250 mesh) in three separate additions, mixing for 2-3 minutes after each addition to ensure thorough dispersion. Then add 1.5 parts of antioxidant TMQ, 1 part of antioxidant 6PPD, 0.5 parts of hindered phenolic antioxidant 1076, and 2 parts of UV absorber UV-329, mixing until homogeneous. The total time is approximately 8 minutes.
[0077] The third stage of mixing: Raise the temperature of the internal mixer to 120°C, and add 10 parts of sodium carboxymethyl cellulose, 15 parts of sodium acrylate-acrylamide copolymer, 5 parts of polyvinyl alcohol (PVA-1799), 8 parts of bentonite (sodium-based, 300 mesh), 5 parts of expandable graphite (expansion temperature 180°C) and the remaining 5 parts of naphthenic oil in sequence, and mix until uniform, for a total time of about 5 minutes.
[0078] Final mixing: Reduce the temperature of the internal mixer to 60°C, and add 2.5 parts of DCP peroxide, 2 parts of TAIC crosslinking agent, 3 parts of OBSH foaming agent, 1 part of zinc stearate, 10 parts of microcapsules (epoxy resin core, urea-formaldehyde resin shell) and 0.5 parts of boron trifluoride diethyl ether complex catalyst in sequence. Mix lightly to avoid microcapsule breakage. The total time is about 3 minutes.
[0079] (3) Refining and Shaping:
[0080] Open mill process: Place the compound obtained in step (2) on an open mill for open milling. Set the temperature of the front roller to 50°C and the temperature of the rear roller to 60°C. Adjust the roller gap to 2-3 mm. Perform 6-8 thin passes on the compound to ensure that it is fully plasticized and uniform. The final sheet thickness is 4-5 mm.
[0081] Extrusion molding: An extruder is used for molding, with a die head temperature of 80℃, a die body temperature of 70℃, a screw speed controlled at 25 rpm, and an extrusion pressure of 9 MPa. Based on the specifications and dimensions of the cable conduit, appropriate molds are used to manufacture sealing devices of specific sizes.
[0082] (4) Vulcanization process:
[0083] First stage of vulcanization: The molded body obtained in step (3) is placed in a molding press for molding vulcanization. The temperature is set to 150°C and the pressure is 10MPa. The vulcanization time is determined by adding 2 minutes to the t90 value measured by the Mooney vulcanizer, which is about 9 minutes.
[0084] Two-stage vulcanization: The product after the first stage vulcanization is placed in an oven for a second stage vulcanization. The temperature is set at 120℃ and the time is 4 hours. The purpose is to eliminate internal stress and stabilize the dimensions.
[0085] (5) Post-processing:
[0086] Surface treatment: The vulcanized product is subjected to plasma treatment to increase the surface energy. The treatment power is 100W and the time is 30 seconds.
[0087] Pre-expansion treatment: The product is placed in an environment of 80℃ and 85%RH for 2 hours, with the expansion rate controlled at 10-15%, to form a pre-expanded layer. After cooling to room temperature, the final product is obtained.
[0088] In this embodiment, the amount of graphene added is 0.5 parts, which is within the lower limit of the scope of this invention. At this ratio, graphene can significantly improve the mechanical properties and thermal stability of the rubber matrix without significantly increasing production costs. Testing showed that the sealing device achieved a tensile strength of 12.5 MPa, an elongation at break of 380%, an expansion rate of 220% after immersion in water at 25°C for 24 hours, and an expansion rate of 160% after heating at 180°C for 10 minutes, demonstrating excellent overall performance.
[0089] Example 2
[0090] The high expansion rate expandable rubber cable conduit plug has the following component ratio (by weight): 100 parts EPDM rubber, 1.0 part graphene, 0.2 parts silane coupling agent KH550, 10 parts sodium carboxymethyl cellulose, 15 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 8 parts bentonite, 5 parts expandable graphite, 3 parts OBSH foaming agent, 1 part zinc stearate, 2.5 parts peroxide DCP, 2 parts crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 5 parts modified nano-montmorillonite, 20 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, 8 parts naphthenic oil, 10 parts microcapsules, and 0.5 parts boron trifluoride diethyl ether complex catalyst.
[0091] The preparation method is basically the same as in Example 1, except that:
[0092] (1) The amount of graphene is increased to 1.0 part, which is the upper limit of the scope of this invention;
[0093] (2) In the pre-dispersion step, the ultrasonic treatment time is extended to 25 minutes to ensure that the high content of graphene is fully dispersed;
[0094] (3) The vulcanization time is extended to 10 minutes to ensure full cross-linking.
[0095] In this embodiment, the mechanical properties and thermal conductivity of the product are further improved due to the increased graphene content to 1.0 part. Testing showed that the tensile strength of the plug reached 14.8 MPa, approximately 18% higher than in Example 1, with an elongation at break of 360% and a thermal conductivity increase of approximately 30%, resulting in more uniform heat distribution and more stable thermal expansion performance under high-temperature conditions.
[0096] Example 3
[0097] The high-elasticity expandable rubber cable conduit plug has the following component ratio (by weight): 100 parts EPDM rubber, 0.75 parts graphene, 0.2 parts silane coupling agent KH550, 12 parts sodium carboxymethyl cellulose, 18 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 10 parts bentonite, 5 parts expandable graphite, 3 parts OBSH foaming agent, 1 part zinc stearate, 2.5 parts peroxide DCP, 2 parts crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 25 parts fumed silica, 5 parts modified nano-montmorillonite, 15 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, 10 parts naphthenic oil, 10 parts microcapsules, and 0.5 parts boron trifluoride ether complex catalyst.
[0098] The preparation method is basically the same as in Example 1, except that:
[0099] (1) The amount of graphene used was 0.75 parts, which is the middle value within the scope of this invention;
[0100] (2) The amounts of sodium carboxymethyl cellulose and sodium acrylate-acrylamide copolymer were increased to 12 parts and 18 parts, respectively, to improve water swelling performance;
[0101] (3) The amount of bentonite was increased to 10 parts to further enhance the water swelling effect;
[0102] (4) Reduce the amount of fumed silica to 25 parts and light calcium carbonate to 15 parts to reduce hardness;
[0103] (5) The naphthenic oil was increased to 10 parts to improve the product's elasticity and flexibility.
[0104] In this embodiment, by adjusting the proportion of the water-swellable component and the amount of filler, a higher water expansion rate and better elasticity were obtained. Testing showed that the sealant had a Shore A hardness of 40, making it softer than Examples 1 and 2, with an increased elongation at break of 410% and a water expansion rate of 280%, significantly higher than Examples 1 and 2, making it more suitable for sealing applications in humid environments.
[0105] Example 4
[0106] A high weather-resistant expandable rubber cable conduit plug, comprising (by weight parts): 100 parts EPDM rubber, 0.5 parts graphene, 0.2 parts silane coupling agent KH550, 10 parts sodium carboxymethyl cellulose, 15 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 8 parts bentonite, 6 parts expandable graphite, 4 parts OBSH foaming agent, 1 part zinc stearate, 3 parts peroxide DCP, 2.5 parts crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 6 parts modified nano-montmorillonite, 20 parts light calcium carbonate, 2 parts antioxidant TMQ, 1.5 parts antioxidant 6PPD, 10761 parts hindered phenolic antioxidant, 33 parts UV absorber UV-329, 8 parts naphthenic oil, 12 parts microcapsules, and 0.6 parts boron trifluoride diethyl ether complex catalyst.
[0107] The preparation method is basically the same as in Example 1, except that:
[0108] (1) The amount of expandable graphite and OBSH foaming agent was increased to 6 parts and 4 parts respectively to improve thermal expansion performance;
[0109] (2) The amounts of peroxide DCP and crosslinking agent TAIC were increased to 3 parts and 2.5 parts, respectively, to improve the crosslinking density;
[0110] (3) Increased use of antioxidants and UV absorbers enhances aging resistance;
[0111] (4) The amount of microcapsules was increased to 12 parts, and the amount of boron trifluoride diethyl ether complex catalyst was increased to 0.6 parts to improve the self-repair efficiency;
[0112] (5) The second-stage vulcanization time is extended to 5 hours to further optimize the cross-linked network structure.
[0113] In this embodiment, by increasing the content of anti-aging components and optimizing the crosslinking system, the aging resistance and self-healing ability of the product were significantly improved. Tests showed that the sealer maintained 85% of its performance after 168 hours of high-temperature aging at 150°C, 90% after 1000 hours of UV aging, and achieved a 92% crack self-healing rate, far superior to Examples 1-3, making it particularly suitable for long-term sealing applications in harsh environments.
[0114] Comparative Example 1: Graphene-free system
[0115] A conventional expandable rubber cable conduit plug has the following component ratio (by weight): 100 parts EPDM rubber, 10 parts sodium carboxymethyl cellulose, 15 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 8 parts bentonite, 5 parts expandable graphite, 3 parts OBSH foaming agent, 1 part zinc stearate, 2.5 parts DCP peroxide, 2 parts TAIC co-crosslinking agent, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 5 parts modified nano-montmorillonite, 20 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, 8 parts naphthenic oil, 10 parts microcapsules, and 0.5 parts boron trifluoride ether complex catalyst.
[0116] The preparation method is the same as in Example 1, but the graphene pre-dispersion step is omitted, and the mixture is directly subjected to intensive mixing.
[0117] The only difference between this comparative example and Example 1 is that it does not contain graphene and silane coupling agent, and is used to verify the effect of graphene modification on product performance.
[0118] Comparative Example 2: No self-healing system
[0119] An expandable rubber cable conduit plug without self-healing function has the following component ratio (by weight): 100 parts EPDM rubber, 0.5 parts graphene, 0.2 parts silane coupling agent KH550, 10 parts sodium carboxymethyl cellulose, 15 parts sodium acrylate-acrylamide copolymer, 5 parts polyvinyl alcohol, 8 parts bentonite, 5 parts expandable graphite, 3 parts OBSH foaming agent, 1 part zinc stearate, 2.5 parts peroxide DCP, 2 parts crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 5 parts modified nano-montmorillonite, 30 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, and 8 parts naphthenic oil.
[0120] The preparation method is the same as in Example 1, but without adding microcapsules and boron trifluoride diethyl ether complex catalyst, and the amount of light calcium carbonate is increased accordingly to maintain the total amount of the formula.
[0121] The difference between this comparative example and Example 1 is that it does not contain a self-healing system, and it is used to verify the impact of the self-healing system on the product's service life.
[0122] Comparative Example 3: Water-swelling system only
[0123] A single-response expandable rubber cable conduit plug, comprising (by weight parts): 100 parts EPDM rubber, 0.5 parts graphene, 0.2 parts silane coupling agent KH550, 15 parts sodium carboxymethyl cellulose, 20 parts sodium acrylate-acrylamide copolymer, 8 parts polyvinyl alcohol, 12 parts bentonite, 2.5 parts peroxide DCP, 2 parts co-crosslinking agent TAIC, 5 parts zinc oxide, 1 part stearic acid, 30 parts fumed silica, 5 parts modified nano-montmorillonite, 25 parts light calcium carbonate, 1.5 parts antioxidant TMQ, 1 part antioxidant 6PPD, 0.5 parts hindered phenolic antioxidant 1076, 2 parts UV absorber UV-329, 8 parts naphthenic oil, 10 parts microcapsules, and 0.5 parts boron trifluoride diethyl ether complex catalyst.
[0124] The preparation method is the same as in Example 1, but expandable graphite, OBSH foaming agent and zinc stearate are not added, and the amount of water-swellable component and filler is increased accordingly.
[0125] The difference between this comparative example and Example 1 is that it contains only a water-swelling system and no thermal expansion function, which is used to verify the necessity of the dual response mechanism.
[0126] Performance Testing and Evaluation
[0127] To comprehensively evaluate the performance of the product of this invention, systematic performance tests were conducted on the above-described embodiments and comparative samples. The test methods are as follows:
[0128] 1. Basic physical performance testing:
[0129] Density: determined according to GB / T533-2008;
[0130] Hardness: Shore A hardness was determined according to GB / T531.1-2008;
[0131] Tensile properties: Tensile strength and elongation at break were determined in accordance with GB / T528-2009;
[0132] Tear strength: determined according to GB / T529-2008;
[0133] Compression set: Measured according to GB / T7759-2015, at 70℃ for 24h.
[0134] 2. Expansion performance test:
[0135] Water swelling rate: The sample was soaked in distilled water at 25℃ for 24 hours, and the volume change rate was measured.
[0136] Thermal expansion rate: The sample was heated in an oven at 180℃ for 10 minutes, and the rate of volume change was measured.
[0137] Expansion pressure: Using a self-made expansion pressure testing device, the maximum pressure generated during the expansion process was recorded.
[0138] 3. Sealing performance test:
[0139] Water tightness: Leakage was tested under a water pressure of 2 bar according to the method of GB / T17626.8-2006;
[0140] Air tightness: Monitor the pressure drop change over 24 hours at 0.5 bar.
[0141] 4. Weather resistance test:
[0142] Thermal aging: Performance changes were tested after aging at 150℃ for 168 hours according to GB / T3512-2014 method;
[0143] Ozone aging: According to GB / T7762-2003, age at 40℃ for 96 hours at a concentration of 50 pphm;
[0144] UV aging: 1000 hours of UV-B 313nm irradiation according to GB / T16422.2-2014 method;
[0145] Salt spray test: Test for 1000 hours in 5% NaCl solution according to GB / T10125-2012 method.
[0146] 5. Self-healing performance test:
[0147] Crack repair rate: A crack with a length of 10 mm and a depth of 1 mm was created on the sample surface using a sharp blade. After being placed at 25°C for 72 hours, the degree of crack healing was measured.
[0148] The test results for each embodiment and comparative example are shown in the table below:
[0149] Table 1. Results of Basic Physical Performance Tests
[0150]
[0151] Table 2. Test results of expansion and sealing performance
[0152]
[0153] Table 3. Test results of weather resistance and self-healing properties
[0154]
[0155]
[0156] The test results above show that:
[0157] 1. Graphene Modification Effect: Comparing the results of Example 1 and Comparative Example 1, it can be seen that after adding 0.5 parts of graphene, the tensile strength of the product increased from 9.6 MPa to 12.5 MPa, an increase of approximately 30%; the tear strength increased from 20.1 kN / m to 26.5 kN / m, an increase of approximately 32%; and the heat aging performance retention rate increased from 60% to 82%, an increase of approximately 37%. This demonstrates the significant effect of graphene as a nano-reinforcing phase. Through its interaction with rubber molecular chains, it forms a three-dimensional conductive network and physical cross-linking points, while simultaneously improving heat distribution and enhancing heat aging resistance.
[0158] 2. Effect of Graphene Dosage: Comparing the results of Example 1 (0.5 parts graphene) and Example 2 (1.0 parts graphene), with the increase of graphene dosage, the tensile strength increased from 12.5 MPa to 14.8 MPa, the tear strength increased from 26.5 kN / m to 29.8 kN / m, and the coefficient of thermal expansion increased from 160% to 175%. This indicates that within the range of this invention (0.5-1.0 parts), the graphene dosage can significantly improve product performance, and users can choose the appropriate dosage according to specific application requirements and cost factors.
[0159] 3. Importance of the Dual Response Mechanism: Comparing the results of Example 1 and Comparative Example 3, although the water expansion rate of Comparative Example 3 (water-only expansion system) was as high as 320%, its thermal expansion rate was almost zero (<5%), and its airtightness was also poor (pressure drop 7.5% / 24h). This demonstrates the necessity of the water-thermal dual response mechanism, especially in applications that may face high-temperature environments, where the thermal expansion function can provide additional sealing protection.
[0160] 4. Value of self-healing function: Comparing the results of Example 1 and Comparative Example 2, their basic physical properties and expansion properties are similar, but the crack repair rate of Comparative Example 2 (without self-healing system) is less than 5%, while the crack repair rate of Example 1 is as high as 85%. This shows that the microcapsule self-healing system can effectively repair the damage caused to the material during use and extend the product life.
[0161] 5. Weather Resistance Optimization: Example 4 achieved optimal aging resistance by increasing the content of anti-aging components and optimizing the crosslinking system. Its heat aging performance retention rate reached 90%, and its UV aging performance retention rate reached 92%, far superior to other examples and comparative examples. This indicates that by rationally adjusting the formulation, the long-term performance of the product can be further improved to meet the needs of different environmental conditions.
[0162] Comprehensive analysis shows that this invention, through an innovative combination of graphene modification, a water-thermal dual-response system, and microcapsule self-healing function, has successfully developed an expandable rubber cable conduit plug with excellent overall performance. This product can provide reliable sealing protection under various environmental conditions, exhibits long-term weather resistance and self-healing capabilities, and meets the sealing needs of cable conduits in fields such as power, communications, rail transportation, marine engineering, and petrochemicals.
[0163] The expandable rubber cable conduit plug of this invention has been tested in a large substation renovation project. Located in a rainy region of southern China, the cable conduits frequently faced water leakage problems, and traditional sealing solutions were ineffective. After adopting the product of this invention, the sealing effect of the 110kV cable conduits was significantly improved, completely preventing water leakage during the rainy season. Installation time was reduced to one-third of traditional methods, and the device can be reassembled and disassembled more than 50 times, resulting in a 40% reduction in overall cost. Inspection after one year of use showed that the product's performance was stable and showed no signs of aging, proving the application value of this invention in practical engineering.
Claims
1. An expandable rubber cable conduit plug, characterized in that, The expandable rubber cable conduit plug is composed of the following components in parts by weight: 100 parts of EPDM rubber, wherein the EPDM rubber has an ethylene content of 55% and a third monomer ENB content of 5%; 0.5-1.0 parts of graphene, wherein the graphene is multilayer graphene with 5-10 layers; 0.2 parts of silane coupling agent KH550; 10 parts of sodium carboxymethyl cellulose; 15 parts of sodium acrylate-acrylamide copolymer; Five parts of polyvinyl alcohol, wherein the polyvinyl alcohol is of type PVA-1799; Eight parts of bentonite, wherein the bentonite is sodium-based bentonite with a particle size of 300 mesh; Five parts of expandable graphite, wherein the expansion temperature of the expandable graphite is 180°C; 3 parts of 4,4'-oxobisbenzenesulfonylhydrazine foaming agent; 1 part zinc stearate; 2.5 parts of DCP peroxide; 2 parts of crosslinking agent TAIC; 5 parts zinc oxide; 1 part stearic acid; 30 parts of fumed silica, wherein the specific surface area of the fumed silica is 200 m². 2 / g; Five parts of modified nano-montmorillonite; 20 parts of light calcium carbonate, wherein the particle size of the light calcium carbonate is 1250 mesh; Anti-aging agent TMQ 1.5 parts; Anti-aging agent 6 PPD 1 part; Hindered phenolic antioxidant 107 60.5 parts; 2 parts of UV absorber UV-329; 8 parts naphthenic oil; Ten portions of microcapsules, wherein the microcapsules are composed of an epoxy resin core and a urea-formaldehyde resin shell; 0.5 parts of boron trifluoride diethyl ether complex catalyst.
2. The expandable rubber cable conduit plug according to claim 1, characterized in that, The expandable rubber cable conduit plug has a dual water-thermal response expansion function. The water expansion rate reaches 200-300% after soaking at 25°C for 24 hours, and the thermal expansion rate reaches 150-200% after heating at 180°C for 10 minutes. The water tightness performance is leak-free under 2 bar water pressure, and the air tightness performance is that the pressure drop does not exceed 5% under 0.5 bar air pressure for 24 hours.
3. The expandable rubber cable conduit plug according to claim 1, characterized in that, The expandable rubber cable conduit plug has a self-healing function. When cracks appear on the material surface, the microcapsules rupture and release the epoxy resin core material, which is cured and repaired under the action of the boron trifluoride ether complex catalyst. The crack repair rate is not less than 85%, and the service life is extended by not less than 30%.
4. The expandable rubber cable conduit plug according to claim 1, characterized in that, The physical performance indicators of the expandable rubber cable conduit plug are as follows: density 1.15±0.05g / cm³, Shore A hardness 45±5 degrees, tensile strength not less than 12MPa, elongation at break not less than 350%, tear strength not less than 25kN / m, and compression set not greater than 20% after 24 hours at 70°C.
5. The expandable rubber cable conduit plug according to claim 1, characterized in that, The weather resistance performance indicators of the expandable rubber cable conduit plug are as follows: after 168 hours of thermal aging at 150°C, the performance retention rate is not less than 80%; after 96 hours of ozone aging at 40°C with a concentration of 50pphm, there is no cracking; after 1000 hours of UV aging at UV-B 313nm, the performance retention rate is not less than 85%; after 1000 hours of salt spray testing in 5% sodium chloride solution, there is no obvious corrosion; the operating temperature range is -40°C to +150°C; and the service life is not less than 20 years.
6. A method for preparing the expandable rubber cable conduit plug according to any one of claims 1-5, characterized in that, Includes the following steps: A. Graphene pre-dispersion: Graphene, silane coupling agent KH550 and 3 parts naphthenic oil are mixed in a high-speed disperser at 3000 rpm and 60°C for 30 minutes. Then, ultrasonic treatment is performed at 400W for 20 minutes. B. Secret mixing process: B1. First stage of mixing: At a temperature of 80°C, add EPDM rubber to a mixer and plasticize for 2 minutes, then add the pre-dispersed graphene mixture obtained in step A, then add zinc oxide and stearic acid, and mix for 5 minutes. B2. Second stage of mixing: Raise the temperature to 100°C, add fumed silica, modified nano montmorillonite, and light calcium carbonate in batches and ensure full dispersion. Then add antioxidant TMQ, antioxidant 6PPD, hindered phenolic antioxidant 1076 and UV absorber UV-329. The mixing time is 8 minutes. B3. Third stage of mixing: Raise the temperature to 120°C, add sodium carboxymethyl cellulose, sodium acrylate-acrylamide copolymer, polyvinyl alcohol, bentonite, expandable graphite and the remaining naphthenic oil, and mix for 5 minutes; B4. Final mixing: Reduce the temperature to 60°C, add peroxide DCP, crosslinking agent TAIC, 4,4'-oxobisbenzenesulfonylhydrazine foaming agent, zinc stearate, microcapsules and boron trifluoride diethyl ether complex catalyst, mix lightly to avoid microcapsule breakage, and the mixing time is 3 minutes. C. Refining and Shaping: C1. Open milling process: The compound obtained in step B is placed on an open mill for open milling. The front roll temperature is 50°C, the rear roll temperature is 60°C, the roll gap is 2-3mm, the number of thin passes is 6-8, and the sheet thickness is 4-5mm. C2. Extrusion Molding: The extruder is used for molding, with a die head temperature of 80°C, a die body temperature of 70°C, a screw speed of 20-30 rpm, and an extrusion pressure of 8-10 MPa. The plugs are made to specific specifications according to the cable conduit size. D. Vulcanization process: D1. First stage vulcanization: The molded body obtained in step C is subjected to compression vulcanization at a temperature of 150°C, a pressure of 10MPa, and a time of t90+2 minutes, or 8-10 minutes. D2. Second-stage vulcanization: The product after the first-stage vulcanization is placed in an oven for second-stage vulcanization at a temperature of 120°C for 4 hours. The purpose is to eliminate internal stress and stabilize the dimensions. E. Post-processing: E1. Surface treatment: The vulcanized product is subjected to plasma treatment to improve the surface energy. The power is 100W and the time is 30 seconds. E2. Pre-expansion treatment: Place the product in an environment of 80°C and 85%RH for 2 hours, controlling the expansion rate to 10-15%, to obtain the final product.
7. The method according to claim 6, characterized in that, In the graphene pre-dispersion step, a combination of high-speed dispersion and ultrasonic treatment is used to form a uniform and stable dispersion of graphene in naphthenic oil, with the graphene agglomerate size being less than 2 μm.
8. The method according to claim 6, characterized in that, The internal mixing process adopts a segmented heating method, gradually increasing the temperature from 80°C to 120°C and then decreasing it to 60°C. The filler is added in batches, with each batch of filler not exceeding 30% of the total filler amount, to ensure the uniformity of the mixed rubber compound. The internal mixing rotor speed is 30-50 rpm, and the temperature of the internally mixed rubber compound exiting the mixing process does not exceed 130°C.
9. The method according to claim 6, characterized in that, The vulcanization process employs a combination of single-stage and two-stage vulcanization. The single-stage vulcanization uses compression molding, with the degree of vulcanization controlled above 95%. The vulcanization time is determined based on the t90 value measured by a Mooney vulcanizer. The two-stage vulcanization uses dry heat curing to achieve dimensional stability and performance uniformity of the product. The crosslinking density of the vulcanized product is 1.5 × 10⁻⁶. -4 Up to 2.0×10 -4 mol / cm³.
10. The method according to claim 6, characterized in that, The pre-expansion treatment in the post-processing step, by controlling the combination of temperature and humidity, enables the product to partially pre-expand, forming a gradient expansion structure. The internal density remains the same, while an expansion layer is formed on the outside. The thickness of the expansion layer is 0.5-1.0 mm. This provides the product with an initial sealing pressure of not less than 0.3 MPa in actual applications, ensuring that a preliminary seal is formed immediately after installation. Upon contact with moisture or an increase in temperature, it further expands to form a complete seal.
Citation Information
Patent Citations
Water swellable rubber composition having stable swelling property at high temperatures
US20130269787A1
Water swellable rubber composition having stable swelling property at high temperatures
US9540501B2
High-efficiency environment-friendly flame-retardant thermoplastic vulcanized rubber material and preparation method thereof
CN106751028A
Flexible fireproof pipe for wires and cables and application thereof
CN111825935A