Oxide enhanced copper-based electric contact material and preparation method thereof

By adopting oxide gradient distribution and sintering extrusion process in copper-based electrical contact materials, the problems of material density and arc erosion resistance are solved, and high-performance electrical contact materials are achieved to meet the high performance requirements of DC contactors.

CN120624878APending Publication Date: 2025-09-12WENZHOU HONGFENG ELECTRICAL ALLOY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510858673.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-25
Publication Date
2025-09-12

AI Technical Summary

Technical Problem

Existing copper-based electrical contact materials have problems such as insufficient density, insufficient arc erosion resistance, poor breaking resistance, and easy adhesion in DC vacuum or inert atmosphere protection contactors, making it difficult to meet high performance requirements.

Method used

By mixing copper-based powders with different oxide contents and going through process steps such as cold isostatic pressing, sintering and hot extrusion, a copper-based electrical contact material with a local gradient distribution of oxides is formed. Combined with the sintering and hot extrusion processes, secondary homogenization and improved density of the material's internal structure are achieved.

Benefits of technology

The electrical properties of the material are significantly improved, including resistance to welding, arc erosion and breaking performance, thus extending the service life of the contactor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120624878A_ABST
    Figure CN120624878A_ABST
Patent Text Reader

Abstract

The invention provides an oxide reinforced copper-based electric contact material and a preparation method thereof, and the method comprises the steps: providing first powder and second powder, and the copper content in the first powder is higher than the copper content in the second powder; the first powder and the second powder are mixed with rare earth oxide powder, copper oxide powder and copper powder, ball milling, cold isostatic pressing and sintering are conducted, and a first billet and a second billet are obtained; the first billet and the second billet are subjected to hot extrusion to form filaments, the filaments are cut short, first short filaments and second short filaments which are the same in length are obtained, and the oxide content in the first short filaments is higher than that in the second short filaments; the multiple first short wires and the multiple second short wires are spliced into a combined ingot; sintering and performing hot extrusion on the combined ingot to obtain an oxide reinforced copper-based strip or wire; and post-processing the oxide reinforced copper-based strip or wire to obtain the oxide reinforced copper-based electric contact material. The electrical performance of the material is remarkably improved, and the high-performance requirements of vacuum direct current or inert atmosphere protection contactors and the like can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrical contact materials, and in particular, to an oxide-reinforced copper-based electrical contact material and a preparation method thereof. Background Art

[0002] DC vacuum or atmosphere-protected contactors and other electrical devices are key components for controlling the connection and disconnection between new energy vehicle battery packs and the DC circuit output of charging stations. During the charging process, these devices quickly disconnect the circuit to prevent overloads and short circuits, reducing the risk of thermal runaway and protecting both the charging equipment and the new energy vehicle's battery system. Furthermore, when starting or ending charging, they connect or isolate the new energy vehicle from the charging station. Therefore, these devices are crucial for safely controlling the current flow between new energy vehicles and DC charging station circuits.

[0003] When a DC vacuum or atmosphere-protected contactor is operating, because the DC arc has no zero crossing point, extinguishing the DC arc is much more difficult than extinguishing an AC arc under the same electrical parameters. This can easily burn the electrical contacts and cause delayed power failure. To ensure the reliable interruption and durability of DC vacuum or atmosphere-protected contactors, the electrical contact materials used as core components of DC contactors must possess excellent arc erosion resistance, high interruption performance, and anti-adhesion properties.

[0004] At present, pure copper, copper alloys or silver-based electrical contact materials are widely used in electrical appliances such as DC vacuum or inert atmosphere protection contactors. This is because under the protection of vacuum or inert atmosphere, Cu will not oxidize, and copper has good electrical and thermal conductivity. Pure copper electrical contact materials have good electrical and thermal conductivity. However, pure copper electrical contacts have poor resistance to arc erosion and high current impact, and are prone to welding and adhesion. Although silver-based materials have excellent electrical conductivity, they are expensive and have insufficient resistance to welding. Although traditional copper alloy electrical contacts have been improved to a certain extent, the distribution of the reinforcing phase is uneven, which limits the overall performance of the material.

[0005] Some technicians have attempted to improve surface contact properties by adding SnO2, SiC, Al2O3, etc. as a second phase to form an ablation-resistant skeleton. Patent CN110508816A uses internal oxidation of copper-aluminum alloy to form an alumina dispersion-strengthened copper matrix, improving the arc ablation resistance of electrical contact materials. However, this process requires multiple pressing and sintering cycles, and the powder used is spherical in shape with pores between the particles. Due to the pressure of the molding method, these pores cannot be completely eliminated, resulting in insufficient material density and high cost. Furthermore, due to the poor plastic forming ability when the Al2O3 content is high, cracks are easily generated during processing. Patent CN1482638A uses hot extrusion to extrude a copper-based mixed powder in a single pass, but its extrusion ratio is only 20-30, which limits the density of the extruded material. This results in insufficient arc ablation resistance and cannot meet the high performance requirements of electrical appliances such as vacuum DC contactors.

[0006] Therefore, there is an urgent need to develop a method for preparing an oxide-reinforced copper-based electrical contact material to solve at least one of the above technical problems. Summary of the Invention

[0007] In view of one of the defects in the prior art, the purpose of the present application is to provide an oxide-reinforced copper-based electrical contact material and a preparation method thereof.

[0008] In a first aspect of the present application, a method for preparing an oxide-reinforced copper-based electrical contact material is provided, comprising:

[0009] Providing a first powder and a second powder, wherein the copper content in the first powder is higher than the copper content in the second powder;

[0010] The first powder and the second powder are respectively mixed with rare earth oxide powder, copper oxide powder and copper powder, ball-milled, and sequentially cold isostatically pressed and sintered to obtain a first ingot and a second ingot;

[0011] hot-extruding the first billet and the second billet into wires, respectively, and cutting the filaments into short pieces to obtain first short filaments and second short filaments of the same length, respectively, wherein the oxide content in the first short filaments is higher than the oxide content in the second short filaments;

[0012] splicing a plurality of the first short filaments and the second short filaments into a combined ingot;

[0013] sintering and hot-pressing the combined ingot to obtain an oxide-reinforced copper-based strip or wire;

[0014] The oxide-reinforced copper-based strip or wire is post-processed to obtain an oxide-reinforced copper-based electrical contact material.

[0015] Optionally, the providing of the first powder and the second powder, wherein:

[0016] Smelting Cu and Me in a smelting furnace at a mass fraction of Cu:Me = (60-90):(10-40) to obtain a first molten metal, and atomizing the first molten metal to obtain a first powder;

[0017] Smelting Cu and Me in a smelting furnace at a mass fraction of Cu:Me = (30-60): (40-70) to obtain a second molten metal, and atomizing the second molten metal to obtain a second powder;

[0018] The first powder and the second powder both have a core-shell structure with a shell of CuOMeO and a core of CuMe.

[0019] Optionally, the first powder and the second powder are mixed with rare earth oxide powder, copper oxide powder and copper powder respectively, and ball-milled, wherein:

[0020] In terms of mass percentage, the proportions of the components are: 5% to 15% of the first powder, 0% to 2% of the rare earth oxide powder, 0% to 10% of the copper oxide powder, and the balance is Cu powder; and / or, 5% to 15% of the second powder, 0% to 2% of the rare earth oxide powder, 0% to 10% of the copper oxide powder, and the balance is Cu powder.

[0021] Optionally, the method has at least one of the following characteristics:

[0022] - Mixing time is 1 hour to 20 hours;

[0023] - Use wet ball milling;

[0024] -Ball milling time is 2 hours to 30 hours;

[0025] -The ball-to-material ratio of ball milling is 1 to 20;

[0026] -The ball mill speed is 20 rpm to 200 rpm.

[0027] Optionally, the method has at least one of the following characteristics:

[0028] -The pressure of cold isostatic pressing is 50MPa~400MPa;

[0029] -Cold isostatic pressing time is 10 seconds to 120 seconds;

[0030] -Sintering temperature is 700℃~950℃;

[0031] - The sintering atmosphere is any one of vacuum, argon and nitrogen;

[0032] - The sintering time is 1 hour to 8 hours.

[0033] Optionally, the first billet and the second billet are hot extruded into wires respectively, wherein:

[0034] The hot extrusion temperature is 700° C. to 850° C., the hot extrusion atmosphere is a nitrogen atmosphere, and the extrusion ratio is 20 to 300.

[0035] Optionally, splicing multiple first short filaments and second short filaments into a combined ingot includes: evenly arranging the same number of multiple first short filaments and multiple second short filaments, the height of the combined ingot is the same as the length of the short filaments, and the first short filaments and second short filaments in the combined ingot are evenly dispersed along the direction perpendicular to the length of the short filaments.

[0036] Optionally, the sintering and hot extruding the combined ingot includes: placing the combined ingot in a sintering furnace, sintering it for 1 hour to 6 hours in any one of a nitrogen atmosphere, an argon atmosphere and a vacuum environment, then cooling it to room temperature and taking it out of the furnace, and then hot extruding the sintered combined ingot at a temperature of 700°C to 850°C and a nitrogen atmosphere, with an extrusion ratio of 20 to 200.

[0037] Optionally, the post-processing of the oxide-reinforced copper-based strip or wire includes: rolling and compounding the oxide-reinforced copper-based material and the cladding material, and then heat treating and / or punching to obtain the oxide-reinforced copper-based electrical contact material.

[0038] In a second aspect of the present application, an oxide-reinforced copper-based electrical contact material is provided, which is prepared using the above-mentioned method for preparing an oxide-reinforced copper-based electrical contact material.

[0039] The preparation method of the oxide-reinforced copper-based electrical contact material provided by the present application is to form a copper-based electrical contact material with a local gradient distribution of oxides by mixing and assembling wires with different oxide contents into ingots, and combining process steps such as sintering and extrusion. The material has the advantages of high strength, resistance to welding and arc ablation of copper-based wires with high oxide content and good plasticity and low contact resistance of copper-based wires with low oxide content, effectively improving the problems of high surface contact resistance, poor anti-breaking ability, and poor machinability of copper-based electrical contact materials prepared by existing methods, significantly improving the electrical properties of the material, and being able to meet the high performance requirements of electrical appliances such as vacuum DC contactors. In addition, the present application realizes secondary homogenization of the internal structure of the material through sintering and hot extrusion, greatly improving the density of the electrical contact material structure, making the material more resistant to arc ablation, and thus extending the service life of electrical products such as vacuum DC or inert atmosphere protection contactors.

[0040] Other technical effects brought about by the additional features will be further explained in the corresponding embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Other features, objects and advantages of the present application will become more apparent upon reading the detailed description of non-limiting embodiments with reference to the following drawings:

[0042] Figure 1 The figure is a flow chart of a method for preparing an oxide-reinforced copper-based electrical contact material according to an exemplary embodiment. DETAILED DESCRIPTION

[0043] The present application is described in detail below with reference to specific embodiments. The following examples will help those skilled in the art to further understand the present application, but are not intended to limit the present application in any form. It should be noted that, without departing from the concept of the present application, a number of variations and improvements may be made by those skilled in the art, and these all fall within the scope of protection of the present application. Parts not described in detail in the following examples may be implemented using existing technologies.

[0044] Existing methods for preparing electrical contact materials suffer from problems such as insufficient material density, insufficient arc erosion resistance, poor breaking resistance, and easy adhesion. To address these issues, the present invention provides a method for preparing an oxide-reinforced copper-based electrical contact material to address these problems.

[0045] Reference Figure 1 As shown, in one embodiment of the present application, a method for preparing an oxide-reinforced copper-based electrical contact material includes:

[0046] S1. Providing a first powder and a second powder, wherein the copper content in the first powder is higher than the copper content in the second powder;

[0047] S2. Mixing the first powder and the second powder with rare earth oxide powder, copper oxide powder, and copper powder, respectively, ball-milling the mixture, and sequentially cold isostatically pressing and sintering the mixture to obtain a first ingot and a second ingot;

[0048] S3, hot-extruding the first billet and the second billet into wires respectively, and cutting the filaments into short pieces to obtain first short filaments and second short filaments of the same length, respectively, wherein the oxide content in the first short filaments is higher than the oxide content in the second short filaments;

[0049] S4, splicing a plurality of first short filaments and second short filaments into a combined ingot;

[0050] S5, sintering and hot extruding the combined ingot to obtain an oxide-reinforced copper-based strip or wire;

[0051] S6. Post-processing the oxide-reinforced copper-based strip or wire to obtain an oxide-reinforced copper-based electrical contact material.

[0052] In the above-mentioned embodiment of the present application, a copper-based electrical contact material with a local gradient distribution of oxides is formed by mixing and assembling wires with different oxide contents into ingots, and combining process steps such as sintering and extrusion. This material combines the advantages of high strength, resistance to welding and arc ablation of copper-based wires with high oxide content and good plasticity and low contact resistance of copper-based wires with low oxide content. It effectively improves the problems of high surface contact resistance, poor anti-breaking ability, and poor machinability of copper-based electrical contact materials prepared by existing methods, significantly improves the electrical properties of the material, and can meet the high performance requirements of electrical appliances such as vacuum DC contactors. In addition, the present application achieves secondary homogenization of the internal structure of the material through sintering and hot extrusion, greatly improving the density of the electrical contact material structure, making the material more resistant to arc ablation, and thus extending the service life of electrical products such as vacuum DC or inert atmosphere protection contactors.

[0053] It should be noted that the local gradient distribution of oxides in copper-based electrical contact materials means that on a certain cross section of the copper-based electrical contact material, its tissue distribution presents a cellular tissue structure, and there is a sudden change in the oxide content in a small area at a random position in the tissue.

[0054] In order to obtain powders with different copper contents, in some specific embodiments of the present application, a first powder and a second powder are provided, wherein: Cu and Me are placed in a smelting furnace at a mass fraction of Cu:Me = (60-90): (10-40) to obtain a first molten metal, and the first molten metal is atomized and powdered to obtain the first powder; Cu and Me are placed in a smelting furnace at a mass fraction of Cu:Me = (30-60): (40-70) to obtain a second molten metal, and the second molten metal is atomized and powdered to obtain a second powder; both the first powder and the second powder have a core-shell structure of CuMe@CuOMeO.

[0055] Specifically, the ratio of Cu to Me in the two powders is determined based on factors such as the mutual solubility of Cu and Me, physical properties of Me (such as its boiling point), and the functional properties of Me. This ensures that Me is evenly dispersed throughout the CuMe alloy, facilitating the subsequent oxidation process to obtain a well-structured CuMe@CuOMeO powder.

[0056] Exemplarily, Me is any one or more of Zn, Zr, Cr, Sn, Al, Ni, Mo, Bi, Sb, Ga, Y or other rare earth elements.

[0057] Specifically, high-pressure oxygen atomization is used to prepare powders to obtain a core-shell structured CuMe@CuOMeO powder. The atomization high-pressure atmosphere can increase the oxidation content in the Cu matrix and achieve uniform distribution of Cu2O or CuO in the matrix.

[0058] The main function of CuO is to form an ablation-resistant skeleton, improve the material's electrical life and increase its strength. The main function of Me and MeO is to improve the agglomeration and coarsening of copper oxide particles, making the distribution of the reinforcing phase more uniform and improving the wettability of the reinforcing phase with the copper matrix. Some rare earths and their oxides precipitate or form at the grain boundaries of the material, which has a pinning effect, thereby improving the strength of the material. The rare earth oxide powder in S2 and the Me and MeO in S2 improve the agglomeration, coarsening, and wettability of the copper oxide particles. In other words, they improve the uniform distribution of the oxide reinforcing phase in the copper matrix and improve the bonding strength between the reinforcing phase and the copper matrix. This solves the problems of abnormal local temperature rise of the electrical contact caused by the agglomeration and coarsening of the reinforcing phase and the poor bonding strength between the reinforcing phase and the copper substrate, greatly improving the quality stability of the electrical contact material.

[0059] Exemplarily, the high-pressure oxygen pressure is 0.3 MPa to 5 MPa, and the time is 1 minute to 60 minutes. The oxygen atomization step allows the atomized droplets and powder to be in situ oxidized during the atomization process to form a core-shell structured multinary oxide powder with a CuOMeO shell and a CuMe core.

[0060] It should be noted that after atomization and pulverization, the powder is sieved through 100-400 meshes to obtain powder of the desired particle size.

[0061] In the above embodiment of the present application, the molten metal is in-situ oxidized into oxide powder by high-pressure oxygen atomization, and then sieved to form oxides of suitable particle size, preparing for the uniform distribution of the reinforcement phase in the copper matrix in the subsequent process.

[0062] In order to obtain ingots with different oxide contents, in some specific embodiments of the present application, the first powder and the second powder are mixed with rare earth oxide powder, copper oxide powder and copper powder, respectively, and ball-milled, wherein: in terms of mass percentage, the proportion of each component is: 5% to 15% of the first powder, 0% to 2% of the rare earth oxide powder, 0% to 10% of the copper oxide powder, and the balance is Cu powder; and / or, 5% to 15% of the second powder, 0% to 2% of the rare earth oxide powder, 0% to 10% of the copper oxide powder, and the balance is Cu powder.

[0063] It should be noted that the amount of each component in the mixed powder is determined based on factors such as the wettability of the oxide and copper, the material's machinability, the material's breaking capacity, and surface contact resistance. If the copper content is too low, the material will be difficult to extrude; if the copper content is too high, the material's performance will be poor and good breaking capacity will not be achieved.

[0064] In the above embodiments of the present application, the amount of each component is set to form a mixed powder that can be subsequently extruded into wire or strip.

[0065] To improve the dispersion of the powders and ensure uniform mixing of the powders, in some embodiments of the present application, the mixing time is 1 to 20 hours. Wet ball milling is used, with a milling time of 2 to 30 hours, a ball-to-material ratio of 1 to 20, and a milling speed of 20 to 200 rpm.

[0066] Specifically, high copper content powder (or low copper content powder), rare earth oxide powder, copper oxide powder and copper powder are mixed in proportion to obtain a mixed powder; then, the mixed powder and liquid medium are placed in a ball mill, and nitrogen is filled in for wet ball milling.

[0067] In the above-mentioned embodiment of the present application, the mixed powder and liquid medium are placed in a ball mill and wet-milled to increase the surface activity of the powder, thereby improving the bonding strength between the reinforcement phase and the copper matrix. Through the high-energy ball milling step and the setting of various parameters, the mixed powder is refined under high-energy collision and rolling, forming a uniform and ultrafine composite powder with ultrafine copper particles on the outside, an oxide layer in the middle, and a copper core. This increases the surface activity of the powder and further improves the bonding strength between the reinforcement phase and the copper matrix.

[0068] To form a dense, chip-free billet, in some specific embodiments of the present application, the cold isostatic pressing pressure is 50 MPa to 400 MPa, the cold isostatic pressing time is 10 to 120 seconds, the sintering temperature is 700°C to 950°C, the sintering atmosphere is any one of vacuum, argon, and nitrogen, and the sintering time is 1 to 8 hours.

[0069] Specifically, the ball-milled powder is cold isostatically pressed to produce an ingot with a high copper oxide content. This ingot is then sintered in a sintering furnace and then removed from the furnace after cooling to room temperature to produce a billet. The cold isostatic pressing and sintering process for the low-copper oxide billet is identical to that for the high-copper oxide billet and will not be further described.

[0070] In the above-mentioned embodiment of the present application, through the cold isostatic pressing and sintering steps, good neck bonding is formed between the powders, and the pores between the particles are reduced and shrunk to form a dense ingot, thereby protecting the copper matrix from oxidation.

[0071] To improve material density, in some specific embodiments of the present application, the first and second billets are separately hot-extruded into wires at a temperature of 700°C to 850°C, in a nitrogen atmosphere, and at an extrusion ratio of 20 to 300. The specific extrusion ratio is determined based on factors such as the physical properties of the elements.

[0072] In the above-mentioned embodiments of the present application, through the extrusion process steps, a large deformation amount of extrusion is used to pressurize the material from multiple directions, so that the density of the material is significantly higher than that of conventional pressing products and is more resistant to arc erosion.

[0073] In order to obtain a combined ingot using short filaments, in some specific embodiments of the present application, multiple first short filaments and second short filaments are spliced ​​into a combined ingot, including: evenly arranging the same number of multiple first short filaments and multiple second short filaments, the height of the combined ingot is the same as the length of the short filament (first short filament or second short filament), and the first short filament and the second short filament in the combined ingot are evenly dispersed along the direction perpendicular to the length of the short filament.

[0074] Exemplarily, along the direction perpendicular to the length of the short filaments, the same number of 10 or more short filaments with high copper oxide content and short filaments with low copper oxide content are spliced ​​into a combined ingot, wherein the height of the combined ingot is the same as the length of the short filaments, and the short filaments are uniformly dispersed in the position of the combined ingot along the direction perpendicular to the length of the short filaments, that is, the first short filament and the second short filament are uniformly dispersed on the cross section of the combined ingot.

[0075] In the above-mentioned embodiment of the present application, short filaments with different oxide contents are assembled and combined to form a combined ingot with a local gradient distribution of oxides along the direction perpendicular to the length of the short filaments.

[0076] In order to further improve the density of the material, in some specific embodiments of the present application, the sintering and hot extrusion of the combined ingot includes: placing the combined ingot in a sintering furnace, sintering it for 1 hour to 6 hours in any one of a nitrogen atmosphere, an argon atmosphere and a vacuum environment, and then cooling it to room temperature and taking it out of the furnace, and then hot extruding the sintered combined ingot at a temperature of 700°C to 850°C and a nitrogen atmosphere, with an extrusion ratio of 20 to 200.

[0077] In the above-mentioned embodiments of the present application, metallurgical bonding is formed between short filaments with different oxide contents through sintering, and extrusion processing applies pressure to the combined ingot material from multiple directions, thereby further improving the density of the material, making it more resistant to arc erosion, and making the extruded material have a local gradient distribution structure, thereby combining the advantages of arc erosion resistance, high breaking force, and high strength of high-oxide reinforced copper-based materials and good plasticity and low resistance of low-oxide reinforced copper-based materials.

[0078] The above embodiments of the present application, based on high-energy ball milling, further combine the extrusion method to further improve the wettability of the reinforcement phase and the copper matrix, increase the bonding strength between the reinforcement phase and the copper matrix, and effectively improve the arc erosion resistance of the product.

[0079] In order to obtain the desired electrical contact material product, in some specific embodiments of the present application, post-processing of oxide-reinforced copper-based strips or wires includes: rolling composite oxide-reinforced copper-based materials and clad materials, and then heat treating and / or punching to obtain oxide-reinforced copper-based electrical contact materials.

[0080] It should be noted that conventional extruded materials are typically formed into strips or wires, depending on their extrusion characteristics. Other shapes, such as triangles, rhombuses, and trapezoids, are prone to extrusion cracking and are difficult to process. The cladding material and the oxide-reinforced copper-based material are typically arranged one above the other, but other configurations are possible, such as creating a through-groove, then inserting the cladding material, and then rolling.

[0081] In the above-mentioned embodiment of the present application, a copper contact of a desired size and shape that can be well welded to the support member can be obtained through post-processing.

[0082] In order to achieve a stable connection between the electrical contact material and the support, in some specific embodiments of the present application, the composite material is any one of pure silver, pure copper, pure nickel, silver alloy, copper alloy, silver-copper-phosphorus and copper-phosphorus.

[0083] In the above embodiments of the present application, the composite material acts as a transition material, thereby ensuring that the copper oxide-reinforced copper-based electrical contact material layer of the copper contact is firmly welded to the support member.

[0084] The above-mentioned embodiments of the present application adopt secondary large deformation extrusion combined with high-pressure oxygen atomization and assembly of short wires of different oxides into ingots to improve the density of the copper-based electrical contact material tissue. At the same time, it also combines the multiple advantages of copper-based electrical contact materials with different oxide contents, making the material more resistant to arc erosion, with better breaking performance and longer service life; at the same time, multiple extrusions are used to redistribute the material tissue, break the original particle interface, achieve secondary homogenization of the internal tissue structure, and improve the electrical properties of the material.

[0085] The oxide-reinforced copper-based electrical contact material prepared using the method in the above embodiments of the present application has the advantages of high resistance to welding, high breaking, anti-adhesion, arc erosion resistance, and long life, and can meet the high breaking and durability requirements of electrical appliances such as DC vacuum or inert atmosphere protection contactors.

[0086] The preferred features of the above embodiments can be used alone in any embodiment, or in any combination without conflict. In addition, parts not described in detail in the embodiments can be implemented using existing technologies.

[0087] The following further illustrates the present application in conjunction with specific application examples / comparative examples to facilitate a better understanding of the above technical solutions of the present application. It should be understood that the following are merely partial examples and are not intended to limit the present application.

[0088] Application examples:

[0089] Continue to refer to Figure 1 In this application example, a method for preparing a Cu / CuOY2O3 electrical contact material comprises the following steps:

[0090] Step 1: Copper and yttrium are placed in a smelting furnace at a mass ratio of 80:20 to obtain a high-copper content molten metal, and the high-copper content molten metal is atomized and pulverized using high-pressure oxygen at a pressure of 2 MPa. The oxygen flow time is 3 minutes, and the powder is passed through a 300-mesh sieve to obtain a high-copper content powder of CuY@CuOY2O3 with a shell-core structure; Copper and yttrium are placed in a smelting furnace at a mass ratio of 40:60 to obtain a low-copper content molten metal, and the low-copper content molten metal is atomized and pulverized using high-pressure oxygen at a pressure of 1 MPa. The oxygen flow time is 5 minutes, and the powder is passed through a 300-mesh sieve to obtain a low-copper content powder of CuY@CuOY2O3 with a shell-core structure;

[0091] Step 2: Mix high copper content powder, rare earth oxide La2O3, CuO and copper powder in proportion for 12 hours to obtain a mixed powder, wherein the mass fraction of each powder is: high copper content powder: 12%, La2O3 powder: 0.5%, CuO powder: 2.5%, and the balance is Cu powder; then, place the mixed powder and ethanol in a ball mill with a ball-to-material ratio of 5, and fill it with nitrogen, and wet ball mill at a speed of 180 rpm for 4 hours; then, cold isostatically press the ball-milled powder for 20 seconds at a cold isostatic pressing pressure of 250 MPa to obtain an ingot with a high copper oxide content; then, place the ingot with a high copper oxide content in a sintering furnace, sinter it at a sintering temperature of 880°C for 2.5 hours under a nitrogen atmosphere, and then cool it to room temperature and take it out of the furnace to obtain an ingot with a high copper oxide content.

[0092] Low copper content powder, La2O3, CuO and copper powder are mixed in proportion for 8 hours to obtain a mixed powder, wherein the mass fraction of each powder is: low copper content powder: 10%, La2O3 powder: 1.5%, CuO powder: 2.5%, and the balance is Cu powder; then, the mixed powder and ethanol are placed in a ball mill with a ball-to-material ratio of 5, and nitrogen is filled in, and wet ball milled at a speed of 150 rpm for 6 hours; then, the ball-milled powder is cold isostatically pressed for 40 seconds at a cold isostatic pressing pressure of 150 MPa to obtain an ingot with low copper oxide content; then, the low copper oxide content ingot is placed in a sintering furnace, sintered at a sintering temperature of 840°C for 4 hours under a nitrogen atmosphere, and then cooled to room temperature and taken out of the furnace to obtain an ingot with low copper oxide content.

[0093] Step 3: hot-extrude the high-copper oxide content ingot and the low-copper oxide content ingot into wires under a nitrogen atmosphere at an extrusion temperature of 800° C. with an extrusion ratio of 120, and cut the filaments into short pieces to obtain 20 short filaments with a high copper oxide content and 20 short filaments with a low copper oxide content, each with a length of 150 mm.

[0094] Step 4: Along the direction perpendicular to the length of the short wires, 20 short wires with high copper oxide content and 20 short wires with low copper oxide content are spliced ​​into a combined ingot with a height of 150 mm, wherein there are 20 short wires with high copper oxide content and 20 short wires with low copper oxide content, and the short wires are evenly dispersed along the direction perpendicular to the length of the short wires at the position of the combined ingot.

[0095] Step 5: Place the combined ingot in a sintering furnace and sinter it under vacuum for 2 hours. Then cool it to room temperature and take it out of the furnace. Then, hot extrude the sintered combined ingot at a temperature of 820°C, an extrusion ratio of 80, and a nitrogen atmosphere to obtain an oxide-reinforced copper-based strip.

[0096] Step 6: Rolling the composite oxide reinforced copper-based strip and the AgCuP15 strip, followed by heat treatment and punching to obtain a Cu / CuOY2O3 copper-based electrical contact of desired size and shape.

[0097] Comparative Example:

[0098] A copper electrical contact prepared by the method of patent CN 110508816 A is used as a comparative example. The preparation method of the copper electrical contact includes the following steps:

[0099] Step 1: Weigh oxygen-free copper rod and pure aluminum block as raw materials, with 99.9% copper and 0.1% aluminum by weight;

[0100] Step 2: Place the oxygen-free copper rod and pure aluminum block in the above ratio into a vacuum atomization device, first evacuate to 10Pa, heat and melt at a melting temperature of 1200°C, and when the oxygen-free copper rod is completely melted, vacuum gas atomize to prepare a copper-aluminum alloy powder with a particle size of -100 mesh;

[0101] Step 3: The copper and aluminum powders prepared above are placed in a high-pressure reactor, oxygen with a purity of 99.9% is introduced, and the reaction mixture is heated to 600°C to fully oxidize the copper and aluminum powders to form copper oxide and aluminum oxide powder. The temperature is kept at this temperature for 2 hours. The reaction mixture is then vacuumed to 0.2 Pa and hydrogen with a purity of 99.5% is introduced to reduce the copper oxide to pure copper. The aluminum oxide particles are dispersed in the copper powder to form dispersion-strengthened copper powder.

[0102] Step 4: Add 0.1% W to the dispersion-strengthened copper powder prepared by internal oxidation, and then mix them in a ball mill, wherein the ball-to-material ratio is 1:5 and the ball milling time is 1 hour;

[0103] Step 5: The mixed alloy powder is pressed into a green body using a press with a pressing pressure of 500 MPa and a holding time of 1 second;

[0104] Step 6: Sinter the pressed green body in a vacuum sintering furnace at a maximum sintering temperature of 800°C for 1 hour;

[0105] Step 7: re-press the sintered compact at a pressure of 1000 MPa;

[0106] Step eight: the re-pressed green block is subjected to secondary sintering at a sintering temperature of 500° C. and a holding time of 1 hour, thereby obtaining the copper electrical contact of the comparative example.

[0107] The performance of the two electrical contacts was tested, and the results are shown in Table 1.

[0108] Table 1 Performance test results

[0109]

[0110]

[0111] For electrical contact materials, density and hardness reflect their compactness, while resistance to welding and breaking capacity are reflected in factors such as the material's electrical life, temperature rise, and hardness. Electrical life and hardness play a major role in resistance to welding. The results in Table 1 show that compared to the molded copper electrical contact material described in CN110508816A, the Cu / CuOY2O3 electrical contact material prepared in the aforementioned application examples of this application exhibits higher density, better resistance to welding, and longer electrical life.

[0112] The above describes some specific embodiments of the present application. It should be understood that the present application is not limited to the above specific embodiments, and those skilled in the art may make various variations or modifications within the scope of the claims, which do not affect the substantive content of the present application. The above preferred features may be used in any combination as long as they do not conflict with each other.

Claims

1. A method for preparing an oxide-reinforced copper-based electrical contact material, characterized in that: include: Providing a first powder and a second powder, wherein the copper content in the first powder is higher than the copper content in the second powder; The first powder and the second powder are respectively mixed with rare earth oxide powder, copper oxide powder and copper powder, ball-milled, and sequentially cold isostatically pressed and sintered to obtain a first ingot and a second ingot; hot-extruding the first billet and the second billet into wires, respectively, and cutting the filaments into short pieces to obtain first short filaments and second short filaments of the same length, respectively, wherein the oxide content in the first short filaments is higher than the oxide content in the second short filaments; splicing a plurality of the first short filaments and the second short filaments into a combined ingot; sintering and hot-pressing the combined ingot to obtain an oxide-reinforced copper-based strip or wire; The oxide-reinforced copper-based strip or wire is post-processed to obtain an oxide-reinforced copper-based electrical contact material.

2. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, wherein: The first powder and the second powder are provided, wherein: Smelting Cu and Me in a smelting furnace at a mass fraction of Cu:Me = (60-90):(10-40) to obtain a first molten metal, and atomizing the first molten metal to obtain a first powder; Smelting Cu and Me in a smelting furnace at a mass fraction of Cu:Me = (30-60): (40-70) to obtain a second molten metal, and atomizing the second molten metal to obtain a second powder; The first powder and the second powder both have a core-shell structure with a shell of CuOMeO and a core of CuMe.

3. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, wherein: The first powder and the second powder are mixed with rare earth oxide powder, copper oxide powder and copper powder respectively, and ball-milled, wherein: In terms of mass percentage, the proportions of the components are: 5% to 15% of the first powder, 0% to 2% of the rare earth oxide powder, 0% to 10% of the copper oxide powder, and the balance is Cu powder; and / or, 5% to 15% of the second powder, 0% to 2% of the rare earth oxide powder, 0% to 10% of the copper oxide powder, and the balance is Cu powder.

4. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, wherein: Have at least one of the following characteristics: - Mixing time is 1 hour to 20 hours; - Use wet ball milling; -Ball milling time is 2 hours to 30 hours; -The ball-to-material ratio of ball milling is 1 to 20; -The ball mill speed is 20 rpm to 200 rpm.

5. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, wherein: Have at least one of the following characteristics: -The pressure of cold isostatic pressing is 50MPa~400MPa; -Cold isostatic pressing time is 10 seconds to 120 seconds; -Sintering temperature is 700℃~950℃; - The sintering atmosphere is any one of vacuum, argon and nitrogen; - The sintering time is 1 hour to 8 hours.

6. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, wherein: The first billet and the second billet are hot-extruded into wires respectively, wherein: The hot extrusion temperature is 700° C. to 850° C., the hot extrusion atmosphere is a nitrogen atmosphere, and the extrusion ratio is 20 to 300.

7. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, characterized in that: The method of splicing the plurality of the first short filaments and the second short filaments into a combined ingot includes: evenly arranging the same number of the plurality of the first short filaments and the plurality of the second short filaments, the height of the combined ingot being the same as the length of the filaments, and the first short filaments and the second short filaments in the combined ingot being evenly dispersed along a direction perpendicular to the length of the filaments.

8. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, characterized in that: The sintering and hot extruding of the combined ingot includes: placing the combined ingot in a sintering furnace, sintering it for 1 hour to 6 hours in any one of a nitrogen atmosphere, an argon atmosphere, and a vacuum environment, then cooling it to room temperature and taking it out of the furnace, and then hot extruding the sintered combined ingot at a temperature of 700°C to 850°C and a nitrogen atmosphere, with an extrusion ratio of 20 to 200.

9. The method for preparing an oxide-reinforced copper-based electrical contact material according to claim 1, wherein: The post-processing of the oxide-reinforced copper-based strip or wire comprises: rolling and compounding the oxide-reinforced copper-based material and the cladding material, and then heat treating and / or punching to obtain the oxide-reinforced copper-based electrical contact material.

10. An oxide-reinforced copper-based electrical contact material, characterized in that: The oxide-reinforced copper-based electrical contact material is prepared using the preparation method of the oxide-reinforced copper-based electrical contact material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of contact material of high-voltage and direct-current relay

    CN110508816A