A method for recycling ternary lithium batteries based on pre-processing impurity removal

By employing a pre-treatment method combining protective gas roasting, flotation, and acid leaching after dismantling ternary lithium batteries, the problem of incomplete impurity removal in existing technologies has been solved, achieving efficient recycling of ternary lithium batteries and obtaining high-purity lithium carbonate products.

CN120637652BActive Publication Date: 2026-11-17JIANGSU XINLIYUAN TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510738948.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-04
Publication Date
2026-11-17
Estimated Expiration
2045-06-04

AI Technical Summary

Technical Problem

In existing lithium battery recycling processes, both wet and pyrometallurgical processes suffer from incomplete impurity removal, leading to the loss of valuable metals and low recovery rates. In particular, the incomplete removal of impurity ions before acid leaching and dissolution affects the recycling efficiency of ternary lithium batteries.

Method used

A pre-treatment method for removing impurities is adopted, which includes roasting under a protective atmosphere after the ternary lithium battery is disassembled, crushing and screening to remove copper/iron/aluminum/carbon, deep carbon removal by flotation, roasting copper oxide under an oxygen-containing atmosphere, followed by acid leaching to remove impurities, and then combining multi-stage precipitation and ion exchange resin treatment to obtain high-purity impurity-removed ternary black powder.

Benefits of technology

The impurity removal rate reached over 98%, the loss of major metal elements was reduced, the recovery rate was improved, and high-purity lithium carbonate products were obtained. The impurity content was reduced to below 20 ppm, and the Fe and Cu element content was reduced to below 10 ppm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120637652B_ABST
    Figure CN120637652B_ABST
Patent Text Reader

Abstract

This application provides a method for recovering ternary lithium batteries based on pre-treatment impurity removal. The method includes the following steps: Step S1: After discharging and disassembling the ternary lithium battery, a first calcination treatment is performed under a protective gas atmosphere, followed by crushing and screening to obtain current collector material, negative electrode active material, and primary black powder; Step S2: The primary black powder is added to water for flotation carbon removal treatment, and then dried to obtain decarbonized primary black powder; Step S3: The decarbonized primary black powder is subjected to a second calcination treatment under an oxygen-containing atmosphere to obtain calcined black powder; Step S4: The calcined black powder is added to an acid solution for acid leaching treatment to obtain an acid leaching solution and impurity-removed ternary black powder. The impurity removal rate of the ternary black powder obtained by this method can reach over 98%, thereby reducing the impact of impurity elements on the metal elements in the recovered ternary black powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of ternary lithium battery recycling technology, specifically relating to a method for recycling ternary lithium batteries based on pre-processing impurity removal. Background Technology

[0002] With increasing societal focus on the energy crisis and environmental pollution, the new energy industry has experienced rapid development. Lithium-ion batteries, as key energy storage devices in the new energy industry, play a crucial role in electrochemical energy storage and new energy vehicles, with sales increasing year by year. However, during cycling, lithium batteries experience various issues, including positive electrode material particle breakage / irreversible phase transition leading to structural failure, excessive growth / decomposition of the SEI on the negative electrode surface, lithium plating on the negative electrode surface, electrolyte decomposition resulting in gas production and deterioration, increased trace impurities in the system, and corrosion of the current collector causing active material stripping. These phenomena lead to a significant capacity decline after long-term cycling, ultimately resulting in the end of the battery's lifespan. Retired batteries contain large amounts of heavy metals and organic matter; direct landfill disposal causes significant environmental pollution. Furthermore, retired batteries contain large amounts of recyclable resources such as cobalt, nickel, manganese, copper, iron, aluminum, and carbon, which would be a huge waste if directly landfilled. Compared to traditional non-ferrous metal smelting from ores, developing and utilizing non-ferrous metal resources from waste batteries can reduce energy consumption by 80-90% and production costs by 60-80%. Driven by resource conservation, environmental protection, and economic benefits, the retired battery recycling industry has flourished in recent years. However, some technical issues in lithium battery recycling processes still need to be addressed.

[0003] The recycling of ternary lithium batteries is mainly divided into wet and pyrometallurgical processes. The wet process typically involves discharging, dismantling, roasting, crushing, and screening the battery into ternary black powder. Then, a reducing agent and acid are added to dissolve the ternary black powder. Iron is added to remove copper, pH is adjusted to remove iron / aluminum, manganese is extracted using P204 extractant, nickel / cobalt is separated and recovered using P507, and sodium carbonate is added to the raffinate to recover lithium carbonate. This process removes impurities such as aluminum / iron / copper after dissolving the ternary black powder. However, during the precipitation and filtration process, a large amount of dissolved nickel / cobalt / manganese / lithium is trapped, resulting in the loss of valuable metals and a reduced yield. The pyrometallurgical process typically involves discharging, dismantling, roasting, crushing, and screening the battery into ternary black powder. Then, a reducing agent is added to the ternary black powder, and it is roasted at high temperature to obtain nickel / cobalt metals and oxides of manganese and lithium. Nickel, cobalt, and manganese are then recovered through electrolytic refining. During the electrolytic refining process, copper / aluminum / iron impurities are deposited at the cathode, reducing the purity of the finished nickel-cobalt alloy. Therefore, finding a process to remove impurity ions from ternary materials before the wet process of acid leaching and dissolving, and before the pyrometallurgical process of reduction roasting, is an urgent problem to be solved in the ternary lithium battery recycling industry. Summary of the Invention

[0004] In view of this, this application provides a method for recycling ternary lithium batteries based on pre-purification. This method can obtain impurity-free ternary black powder with low impurity element content through pre-purification, thereby reducing the impact of impurity elements on the metal elements in the recycled ternary black powder. Moreover, the loss of nickel, cobalt, manganese and lithium elements in the ternary black powder is small and the recovery rate is high.

[0005] In a first aspect, this application provides a method for recycling ternary lithium batteries based on pre-processing impurity removal, comprising the following steps:

[0006] Step S1: After discharging and disassembling the ternary lithium battery, it is subjected to the first calcination treatment under a protective atmosphere, and then crushed and screened to obtain current collector material, negative electrode active material and primary black powder.

[0007] Step S2: Add the primary black powder to water for flotation carbon removal treatment, and dry to obtain carbon-removed primary black powder;

[0008] Step S3: The primary carbon-removed black powder is subjected to a second calcination treatment in an oxygen-containing atmosphere to oxidize the elemental copper in the primary carbon-removed black powder into copper oxide, thereby obtaining calcined black powder.

[0009] Step S4: The roasted black powder is added to an acid solution for acid leaching treatment, so that the non-lithium substances (i.e., impurities) in the roasted black powder react and dissolve with the acid solution to obtain an acid leaching solution and purified ternary black powder; wherein, the acid leaching solution includes Li + Fe 2+ Fe 3+ Al 3+ Cu 2+ Ca 2+ or Mg 2+ At least one of them.

[0010] Based on this application, the method involves using a protective gas for roasting after disassembling a ternary battery, followed by crushing and screening to remove most of the copper / iron / aluminum / carbon, and then deep carbon removal through flotation. The carbon-removed black powder is then roasted a second time in an oxygen-containing atmosphere to oxidize the copper in the impurities of the carbon-removed black powder into copper oxide, which is easily soluble in dilute acid. The iron / aluminum / copper oxide is then dissolved by acid leaching to obtain the impurity-removed ternary black powder. The impurity removal rate of the impurity-removed ternary black powder obtained by this method can reach more than 98%, with the Al element content reduced to below 20 ppm, and the Fe and Cu elements reduced to below 10 ppm. This reduces the impact of impurity elements on the recovery of metal elements in the ternary black powder, and the loss of valuable elements (such as nickel, cobalt, manganese, and lithium) in the ternary black powder is small, resulting in a high recovery rate.

[0011] Specifically, in step S1, the ternary lithium battery undergoes a first calcination treatment under a protective atmosphere. The purpose of this treatment is to remove the volatile electrolyte and binders from the positive and negative electrode sheets, separating the active material layer from the current collector in the electrode sheets. Simultaneously, the components in the active material layer are dispersed. This process is carried out under a protective atmosphere to prevent the carbon element, which is the negative electrode active material, from reacting with oxygen to generate carbon monoxide. This prevents carbon monoxide from reducing the ternary lithium material, which is the positive electrode active material, to easily soluble low-valence oxides, thereby reducing the loss of ternary lithium material in subsequent processing and effectively improving the recovery rate of valuable metal elements (nickel, cobalt, manganese, and lithium) in the ternary lithium material. After calcination, the calcined product is pulverized to fully separate the components in the ternary lithium battery, mainly copper foil, aluminum foil, negative electrode active material, and positive electrode active material. Utilizing the differences in particle size and density of these materials, more than 98% of the copper foil, aluminum foil, and more than 60% of the negative electrode active material can be separated from the ternary lithium material, resulting in a primary black powder whose main material is ternary lithium material.

[0012] In step S2, although some negative electrode active materials were screened in step S1, some negative electrode active materials are still mixed in the primary black powder. Taking advantage of the low density of graphite as a negative electrode active material, the carbon element in the primary black powder can be removed directly by flotation. The low-density carbon element will float to the top and be removed, resulting in decarbonized primary black powder. At the same time, the decarbonization process can reduce the damage to the ternary lithium material in the subsequent second calcination process in an oxygen-containing atmosphere.

[0013] In step S3, the primary carbon-removed black powder is subjected to a second calcination treatment under an oxygen-containing atmosphere. Since the primary carbon-removed black powder contains some elemental copper, which is insoluble in acid, the acid leaching treatment cannot separate the elemental copper from the ternary lithium material. The second calcination treatment is carried out under an oxygen-containing atmosphere. During this process, the elemental copper can be oxidized into easily acid-soluble copper oxide, so that the copper element can be separated from the ternary lithium material through the subsequent acid leaching treatment.

[0014] In step S4, the roasted black powder is subjected to acid leaching treatment. Most of the impurity oxides (such as CuO), impurity elements (such as Fe, Al, etc.), and impurity salts (such as MgCO3, etc.) in the roasted black powder dissolve during the acid leaching process. The ternary lithium material (mainly lithium transition metal composite oxide LiMeO2, where Me includes at least one of Ni, Co, or Mn) is insoluble in the acid solution. Thus, most of the impurity metal elements in the roasted black powder are fixed in the acid leaching solution and separated from the ternary lithium material. The resulting purified ternary black powder has a low content of impurity metal elements, thereby reducing the impact of impurity elements on the subsequent recovery of metal elements in the ternary black powder. At the same time, since the ternary lithium material is insoluble in the acid solution, the recovery rate of each element in the ternary lithium material is high.

[0015] The non-lithium substances include at least one of non-lithium elements, non-lithium oxides, and non-lithium salts, namely, impurity elements, impurity oxides, and impurity salts.

[0016] In some embodiments, in step S1, the conditions for the first calcination treatment include: heating to 300-400°C at a heating rate of 2-10°C / min and holding at that temperature for 0.5-3.5 hours.

[0017] The temperature of the first roasting treatment is selected from any value or any two of 300℃, 320℃, 340℃, 350℃, 360℃, 380℃, and 400℃; the time of the first roasting treatment is selected from any value or any two of 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, and 3.5h.

[0018] In some of the above embodiments, under these conditions, the electrolyte in the ternary lithium battery can be fully volatilized and the binder in the positive and negative electrode sheets can be fully decomposed, thereby allowing the components in the ternary lithium battery to be fully separated. This is beneficial for the components after crushing to fully react in the second calcination treatment and acid leaching treatment, and is also beneficial for the removal of impurity metal elements.

[0019] In some embodiments, the protective atmosphere in step S1 is nitrogen and / or argon.

[0020] In some embodiments, in step S1, the particle size of the primary black powder obtained after crushing and screening is less than 0.6 mm. Based on the above embodiments, the reaction rate of each step can be accelerated, and the recovery efficiency can be improved.

[0021] In some embodiments, the primary black powder includes lithium transition metal composite oxide (LiMeO2), elemental carbon (C), Cu, Al, Fe, Mg, and Ca. Based on the above embodiments, lithium and transition metal elements (at least one of Ni, Co, or Mn) originate from ternary lithium materials used as positive electrode active materials, elemental carbon originates from graphite used as negative electrode active materials, Al and Cu elements mainly originate from the current collector, Fe mainly originates from the outer shell, and Mg and Ca elements originate from the decomposition products of some components in ternary lithium batteries. Therefore, it is necessary to separate the lithium transition metal composite oxide from other impurity components in the primary black powder to reduce the impurity content in the ternary black powder.

[0022] In some embodiments, the conditions for the flotation carbon removal process in step S2 include: a solid-liquid ratio of primary black powder to water of (80-200):1 g / L; stirring at 100-300 rpm for 5-30 minutes, followed by settling for 5-30 minutes; and filtering out the floating carbon in the upper layer. This stirring, settling, and filtering process is repeated 2-6 times. Based on the above embodiments, through multiple flotations, the density difference between carbon and other components can be used for separation, resulting in decarbonized primary black powder and reducing the damage to the ternary lithium material structure caused by carbon during subsequent aerobic roasting.

[0023] In some embodiments, in step S3, the volume fraction of oxygen in the oxygen-containing atmosphere is greater than or equal to 60%. Based on the above embodiments, under these conditions, the oxidation efficiency of elemental copper can be improved, allowing the elemental copper in the primary carbon removal black powder to be oxidized more quickly and fully into easily acid-soluble copper oxide, thereby making it easier to reduce the copper content in the black powder through acid leaching treatment.

[0024] The volume fraction of oxygen in the oxygen-containing atmosphere is selected from any value or a range formed by any two of the following: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, and 100%.

[0025] In some embodiments, in step S3, the conditions for the second roasting treatment include: roasting at 400–500°C for 0.5–2 hours. Based on the above embodiments, under these conditions, elemental copper can fully react with oxygen to generate easily acid-soluble copper oxide, thereby making it easier to reduce the copper content in the black powder through acid leaching.

[0026] The temperature of the second roasting treatment is selected from any value or any two of 400℃, 420℃, 440℃, 450℃, 460℃, 480℃, and 500℃; the time of the second roasting treatment is selected from any value or any two of 0.5h, 1h, 1.5h, and 2h.

[0027] In some embodiments, the acid leaching conditions in step S4 include: a solid-liquid ratio of calcined black powder to acid solution of (120-180):1 g / L, acid leaching at 20-80°C for 0.5-2 hours, and controlling the pH of the system to be 1-1.6 during the acid leaching process. Based on the above embodiments, under these conditions, acid-soluble components in the calcined black powder, such as most impurity metal oxides (e.g., CuO), impurity elemental metals (Fe, Al), and impurity metal salts (e.g., MgCO3), will be fully dissolved in the acid solution, thereby separating from the ternary lithium material.

[0028] In the acid leaching process, the solid-liquid ratio of roasted black powder to acid is selected from any value or any two of the following: 120:1g / L, 130:1g / L, 140:1g / L, 150:1g / L, 160:1g / L, 170:1g / L, and 180:1g / L; the acid leaching temperature is selected from any value or any two of the following: 20℃, 30℃, 40℃, 50℃, 60℃, 70℃, and 80℃; the acid leaching time is selected from any value or any two of the following: 0.5h, 1h, 1.5h, and 2h; and the pH of the system during the acid leaching process is controlled to be any value or any two of the following: 1, 1.2, 1.4, and 1.6.

[0029] It should be noted that during the acid leaching process, the pH value of the system will gradually increase as the reaction proceeds. Therefore, the pH value of the system can be maintained at 1 to 1.6 by adding acid, so that the acid-soluble components in the roasted black powder can fully react and dissolve.

[0030] In some embodiments, step S4, after the acid leaching treatment, further includes: filtering to obtain an acid leaching solution and acid-leached roasted black powder; washing the acid-leached roasted black powder with acid solution and drying to obtain impurity-removed ternary black powder. Based on the above embodiments, the surface of the acid-leached roasted black powder may still have some impurity metal ions adsorbed. Further washing with acid solution can remove the impurity metal ions from the surface of the black powder, further reducing the impurity content of the impurity-removed ternary black powder.

[0031] In some embodiments, the pH of the acid solution in the washing process is 1 to 1.6, and the pickling solution obtained from the washing process is used for the acid leaching process. Based on the above embodiments, washing with an acid solution with a pH of 1 to 1.6 is more effective. Furthermore, since the pH change of the pickling solution after washing is relatively small, and the pickling solution still contains eluted impurity metal elements and lithium elements, using it for acid leaching can save costs and allow for the recovery and reuse of the impurity metal elements and lithium elements.

[0032] In some embodiments, the drying conditions in step S4 include drying at 120–350°C for 1–3 hours.

[0033] In some implementations, it also includes:

[0034] Step S5: Add an oxidizing agent to the acid leaching solution to reduce the Fe content in the solution. 2+ Oxidized to Fe 3+ The resulting oxidized acid leaching solution was obtained.

[0035] Step S6: Add a primary alkali solution to the oxidizing acid leaching solution to adjust the pH of the solution for precipitation treatment, so that Fe in the oxidizing acid leaching solution... 3+ And Al 3+Precipitation yields iron-aluminum slag and iron-aluminum-removed filtrate.

[0036] Step S7: Add a secondary alkaline solution to the iron-aluminum removal filtrate to adjust the pH of the solution for precipitation treatment, so that Cu in the iron-aluminum removal filtrate is removed. 2+ and the remaining Fe 3+ And Al 3+ Precipitation yields copper-, iron-, and aluminum-containing slag and copper-, iron-, and aluminum-free filtrate.

[0037] Step S8: Pass the iron-, aluminum-, and copper-removed filtrate through an ion exchange resin to allow Ca to be removed. 2+ and Mg 2+ Remove the impurities to obtain a purified solution;

[0038] Step S9: Add a tertiary alkaline solution to the purified liquid to carry out a lithium precipitation reaction to obtain lithium carbonate product;

[0039] The tertiary alkaline solution includes sodium carbonate solution and / or potassium carbonate solution.

[0040] In some of the above embodiments, since some lithium elements exist in the form of lithium carbonate in the ternary lithium battery, the acid dissolves in the acid leaching solution in the form of, for example, lithium sulfate during the acid leaching process. The impurity metal elements in the acid leaching solution can be removed by the above steps, and then a lithium carbonate product with high purity can be prepared by adding carbonate.

[0041] Specifically, by using an oxidizing agent to oxidize ferrous ions into ferric ions with a lower pH value, and since the Ksp values ​​of the hydroxides corresponding to both ferric and aluminum ions are low, the Fe in the acid leaching solution can be simultaneously oxidized by adding a primary alkaline solution. 3+ And Al 3+ Precipitation yields an iron-aluminum slag primarily composed of iron-aluminum sulfate. This slag may also contain ferric hydroxide and aluminum hydroxide. Further addition of a secondary alkaline solution increases the pH of the system, thereby reducing the Cu content in the system. 2+ And the Fe that was not completely precipitated in the previous step 3+ And Al 3+ After sufficient precipitation, a copper-aluminum slag containing copper hydroxide as the main component, and small amounts of iron hydroxide and aluminum hydroxide, is obtained. Subsequently, the iron-aluminum-copper filtrate is passed through an ion exchange resin to remove high-valence metal ions (such as Ca) from the system. 2+ and Mg 2+ The purified solution has a low content of impurity metal elements due to ion exchange removal. By adding tertiary alkali solution to replenish carbonate ions, lithium ions are precipitated in the form of lithium carbonate, resulting in a lithium carbonate product with high purity.

[0042] In some embodiments, in step S5, the oxidant is hydrogen peroxide, and the molar amount of the oxidant is 1 to 3 times the molar amount of iron in the acid leaching solution. Based on the above embodiments, an appropriate excess of oxidant can fully convert iron existing in the form of ferrous ions into ferric ions, while using hydrogen peroxide as an oxidant can reduce the introduction of impurity ions.

[0043] In some embodiments, the primary alkaline solution includes at least one of sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, sodium carbonate aqueous solution, and potassium carbonate aqueous solution, and the precipitation treatment conditions include precipitation for 0.5 to 2 hours at a pH of 3.8 to 4.3. Based on the above embodiments, under the above conditions, the Fe in the system... 3+ And Al 3+ It will react with hydroxide ions to precipitate, yielding iron-aluminum slag with iron-aluminum alum as the main component. When using primary alkaline solution for precipitation treatment, the pH is selected from any value or a range formed by any two of the following: 3.8, 3.9, 4.0, 4.1, 4.2, and 4.3.

[0044] In some embodiments, in step S7, the secondary alkaline solution includes at least one of sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, sodium carbonate aqueous solution, and potassium carbonate aqueous solution, and the precipitation treatment conditions include precipitation for 0.5 to 2 hours at a pH of 6.5 to 7. Based on the above embodiments, under the above conditions, the Cu in the system... 2+ It will react with hydroxide ions to precipitate copper hydroxide, while the Fe that was not completely precipitated in the previous step will also be precipitated. 3+ And Al 3+ It will further precipitate and transform into ferric hydroxide and aluminum hydroxide. When using a secondary alkaline solution for precipitation treatment, the pH is selected from any value or a range formed by any two of the following: 6.5, 6.6, 6.7, 6.8, 6.9, and 7.0.

[0045] In some embodiments, in step S9, the conditions for the lithium precipitation reaction include: the molar amount of carbonate ions in the tertiary alkaline solution is equal to the molar amount of Li in the purified solution. + The molar amount is 0.5 to 0.75 times; lithium is precipitated at 60 to 98°C for 0.2 to 3 hours. Based on the above embodiments, under the above conditions, the Li in the purified solution can be reduced. + It is fully precipitated and converted into lithium carbonate.

[0046] In some embodiments, both the primary and secondary alkaline solutions are near-saturated solutions. A near-saturated solution is defined as an alkaline solution with a saturation concentration of C0 and a concentration of C1 satisfying the condition: 0.9C0 ≤ C1 ≤ C0. Under this condition, the introduction of water can be reduced, thus lowering subsequent recovery costs.

[0047] In some embodiments, the ion exchange resin can be At least one of the following: resin and 732 cation exchange resin.

[0048] In some embodiments, in step S9, the purified solution is concentrated before the lithium precipitation reaction, and the concentration of lithium ions in the concentrated purified solution is 20-30 g / L. Based on the above embodiments, due to the Li in the purified solution... + The lithium ions mainly originate from the negative electrode of ternary lithium batteries, so the concentration of lithium ions in the purification solution is low. After concentration treatment, the lithium ions in the purification solution are more likely to precipitate, and less tertiary alkaline solution is consumed.

[0049] In some embodiments, in step S9, before the lithium precipitation reaction, acid is added to the purified solution to adjust the pH to 1-1.6. The pH-adjusted purified solution is then used for acid leaching and / or washing in step S4 to enrich the lithium ion concentration in the purified solution to 20-30 g / L. Based on the above embodiments, since the lithium ion concentration in the purified solution is low, and heating and evaporation to concentrate it would increase the recovery cost, adjusting the pH to 1-1.6 by adding acid and using it for acid leaching and / or washing in step S4 allows for the collection of lithium elements from different batches of ternary lithium batteries through multiple acid leaching and washing processes, thereby enriching the lithium ions in the purified solution and effectively reducing the recovery cost.

[0050] Compared with the prior art, the beneficial effects of this application are as follows:

[0051] (1) This application uses protective gas to protect the roasting process after the ternary battery is disassembled, and then removes most of the copper / iron / aluminum / carbon by crushing and screening, and then removes carbon by flotation. The carbon-removed black powder is roasted twice under oxygen-rich conditions to oxidize the copper in the carbon-removed black powder impurities into copper oxide that is easily dissolved by dilute acid. Then, the iron, aluminum, copper, calcium, magnesium and other elements are dissolved by dilute acid leaching. The black powder after acid leaching is washed and dried by dilute acid countercurrent to obtain the impurity-removed ternary black powder. The impurity removal rate of the obtained impurity-removed black powder can reach more than 98%.

[0052] (2) The acid leaching solution is precipitated by adding alkali stepwise to obtain iron / aluminum / copper, and then calcium and magnesium are removed by exchange resin to obtain high-purity lithium carbonate products with a purity of over 99%. Attached Figure Description

[0053] Figure 1 This is a process flow diagram of a pre-process for recycling ternary lithium batteries based on an embodiment of this application. Detailed Implementation

[0054] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0055] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with an embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0056] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0057] The main objective of this application is to provide a method for recycling ternary lithium batteries based on pre-processing impurity removal, which aims to solve the problems existing in the prior art.

[0058] To achieve the above objectives, this application provides a method for recycling ternary lithium batteries based on pre-treatment impurity removal, which includes the following steps:

[0059] S1 involves disassembling and discharging a ternary lithium battery, then roasting it under a protective atmosphere to remove volatile electrolytes and binders from the active materials. After roasting, the battery is crushed and screened to remove most of the copper, iron, aluminum, and carbon, resulting in primary black powder.

[0060] S2, the primary black powder obtained in S1 is added to deionized water for flotation to remove carbon.

[0061] S3, after flotation to remove carbon and drying, is roasted a second time under oxygen-rich conditions to oxidize the copper in the impurities into copper oxide that is easily dissolved in dilute acid. After the second roasting is completed, roasted black powder is obtained.

[0062] In step S4, the roasted black powder obtained in step S3 is mixed with dilute acid for acid leaching. During acid leaching, calcium and magnesium impurities, iron, aluminum, copper oxide, and some lithium ions dissolve into the dilute acid solution. After acid leaching, acid-leached black powder and acid leaching solution are obtained. The acid-leached black powder is then washed countercurrently with dilute acid and dried to obtain the purified ternary black powder. The washing solution is returned to the dilute acid leaching process for recycling.

[0063] S5 involves adding an oxidizing agent to the acid leaching solution obtained in S4 to oxidize the ferrous iron precipitated in the solution with a high pH value to ferric iron precipitated with a low pH value.

[0064] S6, after oxidation is complete, a primary alkali solution is added to precipitate iron and aluminum. After precipitation, the residue is filtered to obtain iron-aluminum slag and iron-aluminum-removed filtrate. The iron-aluminum slag can be used for further iron and aluminum recovery.

[0065] S7, the iron and aluminum removal filtrate is precipitated with a secondary alkaline solution to precipitate iron hydroxide / aluminum hydroxide / copper hydroxide. After precipitation, the filtrate is filtered to obtain iron, aluminum and copper removal filtrate and iron hydroxide / aluminum hydroxide / copper hydroxide precipitate. The iron hydroxide / aluminum hydroxide / copper hydroxide precipitate is mainly composed of copper hydroxide, which can be used for further recovery of copper.

[0066] S8, the obtained iron / aluminum / copper filtrate is passed through an ion exchange resin to remove calcium, magnesium and high-valence cation impurities to obtain a purified solution.

[0067] S9 involves concentrating the purified solution obtained in S8 and adding a tertiary alkali solution to precipitate lithium ions, thereby obtaining a portion of lithium carbonate product.

[0068] In further step S1 above, the initial calcination temperature is 300–400℃, the calcination time is 0.5–3.5 h, the heating rate is 2–10℃ / min, and the calcination atmosphere is nitrogen or argon. The protective gas is used to prevent the CO generated from the reaction of carbon and oxygen during calcination from damaging the ternary material structure and to avoid the CO reducing the ternary material to easily soluble low-valence oxides in dilute acids, thus preventing the loss of the ternary material. The purpose of the initial calcination is to remove the volatile electrolyte in the electrode and to break down and decompose the binder in the active material, thereby separating the positive and negative electrode active materials from the copper and aluminum foils, while simultaneously converting the active material into easily dispersible powder.

[0069] In the further step S1 above, the crushing and screening process involves crushing and screening the material after the initial roasting to separate the aluminum foil, copper foil, and some graphite from the powdered electrode material based on differences in particle size, density, and other factors. This step can separate over 98% of the copper and aluminum foil, and over 60% of the graphite from the electrode material. The electrode material obtained after further crushing and screening has a particle size of less than 0.6 mm. The screened copper, aluminum, and graphite can be sold as by-products.

[0070] In the further step S2 above, the solid-liquid ratio for flotation carbon removal is (80-200):1 g / L, the stirring speed is 100-300 rpm, stirring time is 5-30 min, and after stirring, the mixture is allowed to stand for 5-30 min. The floating carbon powder on the upper layer is then filtered out to obtain graphite material. This stirring, standing, and carbon filtration process is repeated 2-6 times to obtain decarbonized black powder. The filtrate can be recycled for the flotation carbon removal process. The purpose of carbon removal is to prevent the CO generated during the secondary oxygen-enriched roasting process from damaging the ternary material structure and to avoid the CO reducing the ternary material to easily soluble low-valence oxides in dilute acids, thus preventing the loss of the ternary material.

[0071] Further, the carbon black powder filtered out in step S2 above is dried at 250℃ for 1–3 hours, followed by a second calcination. During the second calcination, the calcination temperature is 400–500℃. At this temperature, copper reacts with oxygen to form copper oxide, which is readily soluble in dilute acid. Aluminum and iron impurities do not react with oxygen at this temperature. The second calcination time is 0.5–2 hours, and the oxygen concentration during the calcination process is greater than 60%. Increasing the oxygen concentration helps improve the oxidation efficiency of copper.

[0072] In the further step S4 above, during the dilute acid leaching, the solid-liquid ratio of the roasted black powder to the acid solution is (120~180):1g / L, the stirring speed during the acid leaching process is 100~300rpm, the acid leaching time is 0.5~2h, the acid leaching process temperature is controlled at 20~80℃, and the acid leaching process pH is controlled at 1~1.6.

[0073] In further step S4 above, the pH of the pickling solution during the countercurrent pickling process is 1 to 1.6, the number of countercurrent washes is 2 to 10, and the drying temperature of the black powder after further washing is 120 to 350°C, and the drying time is 1 to 3 hours.

[0074] Further, in step S5 above, the oxidant is either hydrogen peroxide or ozone, and the molar amount of the oxidant is 1 to 3 times the molar amount of iron in the solution. The concentration of the hydrogen peroxide used is 8 to 30 wt%. Further, in steps S6 and S7 above, the primary and secondary alkaline solutions used can be sodium hydroxide, potassium hydroxide, sodium carbonate, or potassium carbonate. Further, the concentrations of the primary and secondary alkaline solutions are near-saturated solutions (the saturated concentration of the alkaline solution is C0, and the concentration of the near-saturated alkaline solution is C1, satisfying 0.9C0≤C1≤C0). Further, in the process of adding the primary alkaline solution to precipitate iron and aluminum, the pH value of the solution is controlled at 3.8 to 4.3, and the precipitation time is 0.5 to 2 hours. Further, in the process of adding the secondary alkaline solution to precipitate iron, aluminum, and copper, the pH value of the solution is controlled at 6.5 to 7, and the precipitation time is 0.5 to 2 hours. Further, in step S8 above, the ion exchange resin used is... Resins, such as 732 cation exchange resin, are used to deeply remove high-valence cation impurities such as calcium and magnesium.

[0075] Further, in step S9 above, the purified solution is concentrated, and the lithium ion concentration after concentration is 20-30 g / L. The purified solution can also be used to prepare dilute sulfuric acid and then returned to the acid leaching or acid leaching washing process, where lithium ions are enriched multiple times before concentration and lithium precipitation. Further, in step S9 above, the tertiary alkaline solution is a sodium carbonate or potassium carbonate solution, and the concentration range of the alkaline solution is 150-350 g / L. The molar amount of sodium carbonate or potassium carbonate in the alkaline solution is equal to the molar amount of Li in the solution. + The molar amount is 0.5 to 0.75 times. The lithium precipitation temperature is 60 to 98°C, and the precipitation time is 0.2 to 3 hours.

[0076] The solution of this application will be described below with reference to the following specific embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available products, and the devices or equipment used are all purchased from conventional market sales channels.

[0077] Example 1

[0078] Based on the pre-processing and impurity removal of ternary lithium batteries, the specific process flow diagram is as follows: Figure 1 As shown, 20 18650 ternary lithium-ion batteries were disassembled and discharged. The positive electrode material was NCM622. 596.4g of positive and negative electrode sheets were obtained. These sheets were calcined at 350℃ for 2 hours under a nitrogen atmosphere. After crushing and screening, 267.1g of electrode material was obtained. The elemental contents after crushing and screening are shown in Table 1-1. After calcination, 2.5L of deionized water was added, and the mixture was stirred at 150rpm / min for 30 minutes, then allowed to stand for 10 minutes before carbon removal by flotation. This stirring / standing / flotation carbon removal process was repeated three times. After carbon removal, the black powder was dried at 180℃ for 2 hours, yielding 260.98g of decarbonized black powder. The elemental contents after carbon removal are shown in Table 1-2. The dried decarbonized black powder was then calcined in an 80% oxygen atmosphere at 400℃ for 1 hour, yielding 260.99g of calcined black powder. The roasted black powder was added to 2.37 L of sulfuric acid solution with a pH of 1.2 (solid-liquid ratio of 110.12 g / L). Concentrated sulfuric acid was added during the dissolution process, and the pH was controlled between 1 and 1.6. The acid leaching time was 1 h, the acid leaching temperature was 60 °C, and stirring was applied at 200 rpm / min during the acid leaching process. The final pH value of the acid leaching was 1.5. After acid leaching, acid-leached black powder and acid leaching solution were obtained. The acid-leached black powder was washed countercurrently 5 times with sulfuric acid solution with a pH of 1.3. After acid washing, it was washed with deionized water. After washing with deionized water, the black powder was dried at 280 °C for 3 h to obtain 252.2 g of purified black powder. The content of each element after crushing and screening is shown in Table 1-3. The impurities have been removed relatively completely.

[0079] Add 2.8g of 8% hydrogen peroxide to the acid leaching solution to oxidize the ferrous ions (the molar amount of H2O2 is 1 times the molar amount of iron). Then add 65.27mL of 200g / L sodium carbonate solution to the acid leaching solution to perform an iron-aluminum precipitation process. During the precipitation process, control the pH at 3.8–4.3 and allow the precipitation time to be 2 hours. After precipitation, filter to obtain iron-aluminum precipitate and iron-aluminum-removed filtrate. Add 3.57mL of 200g / L sodium carbonate solution to the iron-aluminum-removed filtrate to perform an iron-aluminum-copper precipitation process. During the precipitation process, control the pH at 6.5–7 and allow the precipitation time to be 2 hours. After precipitation, filter to obtain iron-aluminum-copper precipitate (ferric hydroxide / aluminum hydroxide / copper hydroxide) and iron-aluminum-copper-removed filtrate. The resin was used to deeply remove impurities from the iron, aluminum, and copper-containing filtrate to obtain a purified solution. The purified solution was then concentrated to 159.2 mL by heating, at which point the lithium ion concentration was 23 g / L. 93.2 mL of a 300 g / L sodium carbonate solution was added to the purified solution, and the precipitation process was carried out at 90℃ for 1 hour. After precipitation, filtration, and washing with water, 17.92 g of lithium carbonate with a purity of 99.92% was obtained.

[0080] Table 1-1 Content of each element after crushing and screening

[0081] element Al Fe Cu C Li Ni Co Mn Proportion 0.60% 0.13% 0.02% 2.10% 6.87% 34.86% 11.67% 10.88%

[0082] Table 1-2 Contents of various elements after carbon removal

[0083] element Al Fe Cu C Li Ni Co Mn Proportion 0.61% 0.13% 0.02% 0.08% 7.01% 35.58% 11.91% 11.10%

[0084] Table 1-3 Element Contents of Impurity-Removed Ternary Black Powder

[0085] element Al Fe Cu Li Ni Co Mn Proportion 12ppm 8ppm 3ppm 5.80% 36.81% 12.32% 11.49%

[0086] Example 2

[0087] Twenty 18650 ternary lithium-ion batteries were disassembled, with NCM811 as the positive electrode material. 588g of positive and negative electrode sheets were obtained. These sheets were calcined at 350℃ for 2 hours under a nitrogen atmosphere. After crushing and screening, 266.2g of electrode material was obtained. The elemental contents after crushing and screening are shown in Table 2-1. After calcination, 2.5L of deionized water was added, and the mixture was stirred at 150rpm / min for 30 minutes, then allowed to stand for 10 minutes before carbon removal by flotation. This stirring / standing / flotation carbon removal process was repeated three times. After carbon removal, the black powder was dried at 180℃ for 2 hours, yielding 257.70g of decarbonized black powder. The elemental contents after carbon removal are shown in Table 2-2. The dried decarbonized black powder was then calcined at 450℃ for 1.5 hours under a 60% oxygen atmosphere, yielding 257.71g of calcined black powder. 257.71g of roasted black powder was added to 2.15L of sulfuric acid solution with a pH of 1.2 (solid-liquid ratio of 119.87g / L). Concentrated sulfuric acid was added during the dissolution process, and the pH was controlled between 1 and 1.6. The acid leaching time was 1 hour, the acid leaching temperature was 80℃, and stirring was applied at 200rpm / min during the acid leaching process. The final pH value of the acid leaching was 1.2. After acid leaching, acid-leached black powder and acid leaching solution were obtained. The acid-leached black powder was washed countercurrently 5 times with sulfuric acid solution with a pH of 1.2. After acid washing, it was washed with deionized water. After washing with deionized water, the black powder was dried at 280℃ for 3 hours to obtain 249.1g of purified black powder. The content of each element after crushing and screening is shown in Table 2-3. The impurities have been removed relatively completely.

[0088] Add 3.0g of 8% hydrogen peroxide to the acid leaching solution to oxidize the ferrous ions (the molar amount of H2O2 is 1 times the molar amount of iron). Then, slowly add 90.71mL of a 200g / L sodium carbonate solution to the acid leaching solution to precipitate iron and aluminum. During the precipitation process, control the pH at 3.8–4.3 and allow the precipitation time to be 2 hours. After precipitation, filter to obtain iron-aluminum precipitate and iron-aluminum-removed filtrate. Add 4.38mL of a 200g / L sodium carbonate solution to the iron-aluminum-removed filtrate to precipitate iron, aluminum, and copper. During the precipitation process, control the pH at 6.5–7 and allow the precipitation time to be 2 hours. After precipitation, filter to obtain iron-aluminum-copper precipitate (ferric hydroxide / aluminum hydroxide / copper hydroxide) and iron-aluminum-copper-removed filtrate. The resin was used to deeply remove impurities from the iron, aluminum, and copper-containing filtrate to obtain a purified solution. The purified solution was then concentrated by heating to 161.2 mL, at which point the lithium ion concentration was 20 g / L. 82.37 mL of a 300 g / L sodium carbonate solution was added to the purified solution, and the precipitation process was carried out at 90℃ for 1 hour. After precipitation, filtration, and washing with water, 15.85 g of lithium carbonate with a purity of 99.97% was obtained.

[0089] Table 2-1 Content of each element after crushing and screening

[0090] element Al Fe Cu C Li Ni Co Mn Proportion 0.73% 0.14% 0.028% 3.0% 6.77% 45.8% 5.75% 5.36%

[0091] Table 2-2 Content of each element after carbon removal

[0092]

[0093]

[0094] Table 2-3 Element Content of Impurity-Removed Ternary Black Powder

[0095] element Al Fe Cu Li Ni Co Mn Proportion 13ppm 7ppm 6ppm 5.92% 48.83% 6.13% 5.71%

[0096] Based on the results of Examples 1 and 2 above, it is evident that the method for recovering ternary lithium batteries based on pre-processing impurity removal provided in this application yields black powder with Al content below 15 ppm and Fe and Cu content below 10 ppm, which helps reduce the impact of these impurity metal elements on the subsequent recovery process of ternary black powder. Simultaneously, this application can recover lithium elements existing in the form of lithium carbonate from ternary lithium batteries, obtaining high-purity lithium carbonate products.

[0097] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the principles of this application should be included within the protection scope of this application.

Claims

1. A method for recycling ternary lithium batteries based on pre-processing impurity removal, characterized in that, Includes the following steps: Step S1: After discharging and disassembling the ternary lithium battery, it is subjected to the first calcination treatment under a protective atmosphere, and then crushed and screened to obtain current collector material, negative electrode active material and primary black powder. Step S2: Add the primary black powder to water for flotation carbon removal treatment, and dry to obtain carbon-removed primary black powder; Step S3: The primary carbon-removed black powder is subjected to a second calcination treatment in an oxygen-containing atmosphere to oxidize the elemental copper in the primary carbon-removed black powder into copper oxide, thereby obtaining calcined black powder. Step S4: Add the roasted black powder to an acid solution for acid leaching treatment, so that the non-lithium substances in the roasted black powder react and dissolve with the acid solution to obtain an acid leaching solution and impurity-removed ternary black powder. The acid immersion solution comprises at least one of Li + , Fe 2+ , Fe 3+ , Al 3+ , Cu 2+ , Ca 2+ , or Mg 2+ . The conditions for the first calcination treatment include heating to 300~400℃; Carbon elements are removed from primary black powder by flotation. The impurity-removing ternary black powder includes lithium transition metal composite oxide LiMeO2, where Me includes at least one of Ni, Co, or Mn; In step S3, the volume fraction of oxygen in the oxygen-containing atmosphere is greater than or equal to 60%. In step S4, the pH of the system is controlled to be 1~1.6 during the acid leaching process; The impurity-removed ternary black powder is subjected to wet acid leaching and dissolution treatment with a reducing agent and acid, or the impurity-removed ternary black powder is subjected to pyrometallurgical reduction roasting treatment.

2. The method according to claim 1, characterized in that, In step S1, the conditions for the first calcination treatment include: heating to 300-400°C at a heating rate of 2-10°C / min, and holding the temperature for calcination for 0.5-3.5 hours.

3. The method according to claim 1, characterized in that, The protective atmosphere is selected from at least one of nitrogen and argon.

4. The method according to claim 1, characterized in that, The primary black powder includes lithium transition metal oxide, elemental carbon (C), Cu, Al, Fe, Mg, and Ca.

5. The method according to claim 1, characterized in that, In step S2, the conditions for the flotation carbon removal treatment include: the solid-liquid ratio of primary black powder to water is (80~200):1g / L, stirring at 100~300rpm for 5~30min, letting stand for 5~30min, and filtering out the floating carbon in the upper layer; repeating the stirring, standing, and filtering operation 2~6 times.

6. The method according to claim 1, characterized in that, In step S3, the conditions for the second calcination treatment include: calcination at 400~500℃ for 0.5~2 hours.

7. The method according to claim 1, characterized in that, In step S4, the acid leaching conditions include: a solid-liquid ratio of calcined black powder to acid solution of (120~180):1g / L, and acid leaching at 20~80℃ for 0.5~2h.

8. The method according to claim 1, characterized in that, In step S4, the acid leaching treatment further includes: After acid leaching, the solution was filtered to obtain acid leaching liquid and roasted black powder after acid leaching. The roasted black powder after acid leaching was washed with acid solution and dried to obtain impurity-free ternary black powder.

9. The method according to claim 8, characterized in that, The pH of the acid solution in the washing process is 1 to 1.6, and the acid solution obtained from the washing process is used for the acid leaching process.

10. The method according to any one of claims 1 to 9, characterized in that, Also includes: Step S5: Add an oxidizing agent to the acid leaching solution to reduce the Fe content in the solution. 2+ Oxidized to Fe 3+ The resulting oxidized acid leaching solution was obtained. Step S6: Add a primary alkali solution to the oxidizing acid leaching solution to adjust the pH of the solution for precipitation treatment, so that Fe in the oxidizing acid leaching solution... 3+ And Al 3+ Precipitation yields iron-aluminum slag and iron-aluminum-removed filtrate. Step S7: Add a secondary alkaline solution to the iron-aluminum removal filtrate to adjust the pH of the solution for precipitation treatment, so that Cu in the iron-aluminum removal filtrate is removed. 2+ and the remaining Fe 3+ And Al 3+ Precipitation yields copper-, iron-, and aluminum-containing slag and copper-, iron-, and aluminum-free filtrate. Step S8: Pass the iron-, aluminum-, and copper-removed filtrate through an ion exchange resin to allow Ca to react. 2+ and Mg 2+ Remove the impurities to obtain a purified solution; Step S9: Add a tertiary alkaline solution to the purified liquid to carry out a lithium precipitation reaction to obtain lithium carbonate product; The tertiary alkaline solution includes sodium carbonate solution and / or potassium carbonate solution.

11. The method according to claim 10, characterized in that, The method satisfies at least one of the following conditions: (1) In step S5, the oxidant is either hydrogen peroxide or ozone, and the molar amount of the oxidant is 1 to 3 times the molar amount of iron in the acid leaching solution; (2) In step S6, the primary alkaline solution includes at least one of sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, sodium carbonate aqueous solution, and potassium carbonate aqueous solution, and the precipitation treatment conditions include precipitation for 0.5 to 2 hours at a pH of 3.8 to 4.3; (3) In step S7, the secondary alkaline solution includes at least one of sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, sodium carbonate aqueous solution, and potassium carbonate aqueous solution, and the precipitation treatment conditions include precipitation for 0.5 to 2 hours at a pH of 6.5 to 7; (4) In step S9, the conditions for the lithium precipitation reaction include: the molar amount of carbonate ions in the tertiary alkaline solution is equal to the molar amount of Li in the purified solution. + 0.5 to 0.75 times the molar amount; lithium is precipitated at 60 to 98°C for 0.2 to 3 hours; (5) In step S9, before the lithium precipitation reaction, the purified liquid is concentrated and the lithium ion concentration in the purified liquid after concentration is 20~30g / L.

12. The method according to claim 10, characterized in that, In step S9, before the lithium precipitation reaction, acid is added to the purification solution to adjust the pH to 1~1.

6. The purified solution after pH adjustment is used for acid leaching and / or washing treatment in step S4 to enrich the lithium ion concentration in the purification solution to 20~30g / L.

Citation Information

Patent Citations

  • Method for separating and recycling valuable metal of ternary lithium battery

    CN117867281A

  • Recycling method of graphite in waste negative electrode, graphite negative electrode material, secondary battery and electric equipment

    CN119898768A