Vanadium-based metal oxide @rGO composite aerogel, its preparation method and application

The preparation of vanadium-based metal oxide @rGO composite aerogels using microwave reaction and electrostatic self-assembly techniques solves the problems of exposed electroactive sites and structural collapse in vanadium-based cathode materials, thereby improving the electrochemical performance of zinc-ion batteries.

CN120664589BActive Publication Date: 2026-11-17SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510862195.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-25
Publication Date
2026-11-17
Estimated Expiration
2045-06-25

AI Technical Summary

Technical Problem

Existing vanadium-based cathode materials suffer from low exposure of electroactive sites, poor charge transfer kinetics, and structural collapse in zinc-ion batteries, which affect their electrochemical performance.

Method used

Vanadium-based metal oxide nanoparticles were prepared by microwave reaction and then fixed on reduced graphene oxide nanosheets by electrostatic self-assembly. After calcination, vanadium-based metal oxide@rGO composite aerogels were formed, which improved conductivity and inhibited nanoparticle aggregation.

Benefits of technology

It improves the cycle life, rate performance, and discharge specific capacity of zinc-ion battery cathodes, showing good application potential, and the preparation process is safe and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120664589B_ABST
    Figure CN120664589B_ABST
Patent Text Reader

Abstract

This invention discloses a vanadium-based metal oxide @rGO composite aerogel, its preparation method, and its application. The preparation method includes: 1) dissolving a vanadium-based oxide precursor in an organic solvent and reacting it with microwaves to obtain vanadium-based metal oxide nanoparticles; the vanadium-based oxide precursor includes at least one selected from triisopropanol vanadium oxychloride, vanadium trichloride, ammonium metavanadate, and vanadium oxalate; the vanadium-based metal oxide nanoparticles are selected from V₂O₃, V₂O₃, and V₂O₃. 1.52 (OH) 0.77 1) At least one of vanadium-based metal oxide nanoparticles and VO2; 2) The vanadium-based metal oxide nanoparticles are dispersed in a dispersion of graphene oxide nanosheets for electrostatic self-assembly, freeze-dried, and then calcined under a protective atmosphere to obtain vanadium-based metal oxide@rGO composite aerogel. The vanadium-based metal oxide@rGO composite aerogel prepared by the method of the present invention can effectively improve the discharge capacity, rate performance, and cycle performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of zinc-ion battery technology, and relates to a vanadium-based metal oxide @rGO composite aerogel, its preparation method, and its application. Background Technology

[0002] As society's reliance on fossil fuels increases and non-renewable energy sources gradually deplete, the development of energy storage devices compatible with clean energy sources such as solar and wind power has become an urgent priority. Currently, lithium-ion batteries (LIBs) are widely used in various fields due to their high discharge capacity and long cycle life. However, the use of organic electrolytes can easily lead to combustion and safety accidents. Furthermore, the anhydrous and oxygen-free manufacturing environment increases the production cost of LIBs. These factors constrain the development of LIBs.

[0003] In recent years, researchers have made significant progress in developing highly safe aqueous batteries, including monovalent aqueous Na+ batteries. + K + Batteries, divalent aqueous Zn 2+ Mg 2+ Batteries and multivalent aqueous Al 3+ Batteries. Among them, those with low cost, low flammability, and high theoretical specific capacity (820mAh g) are particularly noteworthy. -1 With advantages such as low oxidation-reduction potential (-0.76V), zinc-ion batteries (ZIBs) have become a popular candidate for next-generation energy storage technology.

[0004] A major challenge for Zinc-Based Injections (ZIBs) is developing cathode materials with high discharge capacity and long cycle life. In recent years, researchers have developed many novel ZIB cathode materials, mainly including manganese-based compounds, vanadium-based compounds, Prussian blue analogs, and organic compounds. Among these, vanadium-based compounds have attracted increasing attention due to their advantages such as multi-electron redox reactions, multidimensional ion diffusion pathways, and high specific capacity. However, conventionally synthesized vanadium-based compounds exhibit poor performance in rate characteristics and cycle stability due to their slow electrochemical reaction kinetics and structural collapse issues. Therefore, addressing the slow reaction kinetics and structural collapse problems of vanadium-based compounds is crucial for achieving high-performance AZIBs.

[0005] In response to the problems of the aforementioned vanadium-based cathode materials, numerous strategies have emerged, mainly focusing on coating materials, defect modulation, and intercalation engineering. These strategies are expected to alleviate the key problems of the aforementioned vanadium-based materials. For example, CN110817958A - A carbon-coated nano-vanadium pentoxide lithium battery cathode material and its liquid-phase in-situ preparation method, the method includes the following steps: (1) dissolving hexadecyltrimethylammonium bromide in water and stirring; (2) adding triisopropanol vanadium oxide solution dropwise to the solution obtained in step (1) and stirring; (3) transferring the mixed solution obtained in step (2) into a reaction vessel for hydrothermal reaction; (4) washing and drying the product obtained in step (3), and then performing low-temperature heat treatment. This method involves mixing a hexadecyltrimethylammonium bromide solution with a triisopropanol vanadium oxide solution and then performing a hydrothermal reaction. The resulting product is then washed, dried, and subjected to low-temperature heat treatment to obtain a carbon-coated nano-vanadium pentoxide lithium battery cathode material. This carbon-coated nano-vanadium pentoxide lithium battery cathode material exhibits high reversible charge-discharge specific capacity, uniform carbon film coating, and is resistant to carbon film detachment, demonstrating excellent electrochemical performance. CN115092960A discloses a defect-rich vanadium disulfide, its preparation method, and its application as a cathode material in aqueous zinc-ion batteries. Firstly, it describes the preparation of defect-rich layered transition metal dichalcogenide compound VS2 powder material. The main preparation process includes a simple one-step hydrothermal method followed by in-situ electrochemical activation under high voltage. The obtained VS2 has a unique structure and exhibits extremely high specific capacity and excellent rate performance when used as a cathode material in aqueous zinc-ion batteries. Secondly, a simple and convenient external weak magnetic field method is used to suppress zinc dendrite growth, significantly improving the cycle life of the VS2 / Zn battery, showing broad application prospects in the field of aqueous zinc-ion batteries.

[0006] Although the above methods can improve the electrochemical performance of cathode materials for aqueous zinc-ion batteries to some extent, they still have drawbacks such as low exposure of electroactive sites and poor charge transfer kinetics. Summary of the Invention

[0007] To address the aforementioned technical problems in the existing technology, the present invention aims to provide a vanadium-based metal oxide@rGO composite aerogel, its preparation method, and its application.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] In this invention, "vanadium-based metal oxide@rGO composite aerogel" refers to a material comprising reduced graphene oxide nanosheets and vanadium-based metal oxide nanoparticles dispersed on the reduced graphene oxide nanosheets.

[0010] In a first aspect, the present invention provides a method for preparing vanadium-based metal oxide@rGO composite aerogel, the method comprising the following steps:

[0011] (1) Dissolve the vanadium-based oxide precursor in an organic solvent to obtain a vanadium-based oxide precursor solution, and perform a microwave reaction on the vanadium-based oxide precursor solution to obtain vanadium-based metal oxide nanoparticles.

[0012] The vanadium-based oxide precursor includes at least one of triisopropanol vanadium oxy (VO(OiPr)3), vanadium trichloride oxy (VOCl3), and vanadium oxalate oxy (VO(C2O4));

[0013] The vanadium-based metal oxide nanoparticles are selected from V₂O₃ and V₂O₃. 1.52 (OH) 0.77 and at least one of VO2;

[0014] (2) The vanadium-based metal oxide nanoparticles are dispersed in a dispersion of graphene oxide nanosheets for electrostatic self-assembly. After freeze-drying, they are calcined under a protective atmosphere to obtain vanadium-based metal oxide@rGO composite aerogel.

[0015] In this invention, vanadium-based metal oxide nanoparticles refer to particles with a diameter of less than 500 nm.

[0016] The method of this invention uses a specific type of vanadium-based oxide precursor dissolved in an organic solvent, and employs a microwave reaction to obtain vanadium-based metal oxide nanoparticles with a specific composition. The nanoscale particle size allows for the full exposure of electroactive sites in the material, which is beneficial for Zn… 2+ The insertion / deintercalation process is described. Furthermore, nanoparticles are fixed onto the surface of graphene oxide (GO) nanosheets using electrostatic self-assembly. After calcination, the graphene oxide is converted into reduced graphene oxide (rGO), improving the material's conductivity. The highly conductive reduced graphene oxide enhances charge transfer kinetics, while the layered structure of the reduced graphene oxide also helps to fix the nanoparticles, inhibiting their aggregation during charging and discharging to alleviate structural collapse.

[0017] Using the method of this invention, V₂O₃ nanoparticles can be formed by using triisopropanol vanadium oxide as a vanadium-based oxide precursor, and V₂O₃ nanoparticles can be formed by using trichlorovanadium vanadium oxide as a vanadium-based oxide precursor. 1.52 (OH) 0.77 Ammonium metavanadate and vanadium oxalate, as precursors of vanadium-based oxides, can form VO2.

[0018] In the method of the present invention, the organic solvent needs to meet the following conditions: it must be able to dissolve the vanadium-based oxide precursor and not participate in the synthesis reaction of vanadium-based metal oxide nanoparticles in the microwave reaction.

[0019] The vanadium-based metal oxide @rGO composite aerogel prepared by the method of this invention is used as the positive electrode of zinc-ion batteries. It has good cycle life, rate performance and high discharge specific capacity, and has good application potential.

[0020] The method of this invention utilizes simple microwave synthesis, electrostatic self-assembly, and calcination processes, with straightforward steps. Moreover, the reaction process is safe and reliable, causing no harm or pollution to personnel or the environment, and is easy to promote and use.

[0021] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The technical objectives and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.

[0022] Preferably, the organic solvent in step (1) includes at least one of benzyl alcohol, ethylene glycol and diethylene glycol.

[0023] Preferably, the concentration of the vanadium-based oxide precursor in the vanadium-based oxide precursor solution in step (1) is 100 mmol / L to 200 mmol / L, for example, it can be 100 mmol / L, 120 mmol / L, 130 mmol / L, 150 mmol / L, 160 mmol / L, 170 mmol / L, 180 mmol / L, 190 mmol / L or 200 mmol / L, etc.

[0024] Preferably, the temperature of the microwave reaction in step (1) is 180℃~220℃, for example, it can be 180℃, 185℃, 190℃, 195℃, 200℃, 205℃, 210℃, 215℃ or 220℃, etc.

[0025] Preferably, the microwave reaction in step (1) is carried out in the microwave reactor, which is equipped with a microwave reaction tube. The microwave reaction tube is used to hold the reactants and the microwave reactor is heated to a set temperature under a certain power.

[0026] Preferably, the power is 500W to 1200W, for example, it can be 500W, 550W, 600W, 650W, 700W, 750W, 800W, 850W, 900W, 950W, 1000W, 1050W, 1100W, 1150W, or 1200W. If the power is too low, the precursor reaction will be insufficient; if the power is too high, the heating rate will be too fast, the reaction will be more violent, the nanoparticle size distribution will be larger, and some particles will agglomerate, affecting the material properties.

[0027] Preferably, the microwave reaction time in step (1) is 10 min to 30 min, for example, it can be 10 min, 15 min, 20 min, 25 min or 30 min.

[0028] Preferably, the microwave reaction in step (1) is accompanied by stirring, and the stirring speed is 500 rpm to 700 rpm, for example, 500 rpm, 550 rpm, 600 rpm, 650 rpm or 700 rpm.

[0029] As a preferred technical solution of the preparation method of the present invention, in step (2), the mass ratio of the vanadium-based metal oxide nanoparticles to the graphene oxide nanosheets is 1:(0.1 to 0.5), for example, it can be 1:0.1, 1:0.2, 1:0.3, 1:0.4 or 1:0.5, etc.

[0030] Preferably, in step (2), the method of dispersing the vanadium-based metal oxide nanoparticles in a dispersion of graphene oxide nanosheets includes:

[0031] First, the vanadium-based metal oxide nanoparticles are dispersed in an aqueous solution of a surfactant to obtain a first solution. Then, the dispersion of graphene oxide nanosheets is mixed with the first solution and stirred until homogeneous.

[0032] Preferably, the surfactant includes 2-(2-(2-methoxyethoxy)ethoxy)acetic acid and sodium dodecylbenzenesulfonate.

[0033] Preferably, the concentration of the aqueous solution of the surfactant is 40 mL / L to 60 mL / L, for example, it can be 40 mL / L, 45 mL / L, 50 mL / L, 55 mL / L, or 60 mL / L. This concentration refers to the volume of surfactant contained in 1 L of aqueous solution. Taking an aqueous solution concentration of 40 mL / L as an example, it means that 1 L of aqueous solution contains 40 mL of surfactant.

[0034] Preferably, the dispersion method is ultrasonic dispersion.

[0035] Preferably, the concentration of vanadium-based metal oxide nanoparticles in the first solution is 10 mg / mL to 20 mg / mL, for example, it can be 10 mg / mL, 12 mg / mL, 13 mg / mL, 14 mg / mL, 15 mg / mL, 16 mg / mL, 18 mg / mL or 20 mg / mL, etc.

[0036] Preferably, the gas in the protective atmosphere in step (2) includes at least one of nitrogen, helium, argon or neon.

[0037] Preferably, the calcination temperature in step (2) is 250℃~300℃, for example, it can be 250℃, 260℃, 270℃, 280℃, 290℃ or 300℃.

[0038] Preferably, the calcination time in step (2) is 1h to 3h, for example, it can be 1h, 1.5h, 2h, 2.5h or 3h.

[0039] Preferably, the heating rate of the calcination in step (2) is 1℃ / min to 5℃ / min, for example, it can be 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min or 5℃ / min.

[0040] Secondly, the present invention provides a vanadium-based metal oxide @rGO composite aerogel, wherein the vanadium-based metal oxide @rGO composite aerogel is prepared by the preparation method described in the first aspect, and the vanadium-based metal oxide @rGO composite aerogel comprises reduced graphene oxide nanosheets and vanadium-based metal oxide nanoparticles dispersed on the reduced graphene oxide nanosheets, wherein the vanadium-based metal oxide is selected from V₂O₃, V₂O₃, and V₂O₃. 1.52 (OH) 0.77 At least one of VO2.

[0041] Thirdly, the present invention provides a positive electrode comprising the vanadium-based metal oxide@rGO composite aerogel described in the first aspect.

[0042] Fourthly, the present invention provides an aqueous zinc-ion battery, wherein the aqueous zinc-ion battery includes the positive electrode described in the third aspect.

[0043] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0044] Compared with existing technologies, the present invention has the following beneficial effects:

[0045] (1) The method of the present invention uses a specific type of vanadium-based oxide precursor dissolved in an organic solvent, and uses a microwave reaction method to obtain vanadium-based metal oxide nanoparticles with a specific composition. The nanoscale particle size can fully expose the electroactive sites in the material, which is beneficial to Zn 2+The insertion / deintercalation process is described. Furthermore, nanoparticles are fixed onto the surface of graphene oxide (GO) nanosheets using electrostatic self-assembly. After calcination, the graphene oxide is converted into reduced graphene oxide (rGO), improving the material's conductivity. The highly conductive reduced graphene oxide enhances charge transfer kinetics, while the layered structure of the reduced graphene oxide also helps to fix the nanoparticles, inhibiting their aggregation during charging and discharging to alleviate structural collapse.

[0046] (2) The vanadium-based metal oxide @rGO composite aerogel prepared by the method of the present invention is used as the positive electrode of zinc-ion batteries. It has good cycle life, rate performance and high discharge specific capacity, and has good application potential.

[0047] (3) The method of the present invention utilizes simple microwave synthesis, electrostatic self-assembly and calcination processes, and the steps are simple. Moreover, the reaction process is safe and reliable, and will not cause harm or pollution to personnel or the environment, making it easy to promote and use. Attached Figure Description

[0048] Figure 1 A schematic diagram of the preparation process of vanadium-based metal oxide@rGO composite aerogel. Detailed Implementation

[0049] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0050] The specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention.

[0051] In this embodiment of the invention, nanoparticles refer to particles with a diameter of less than 500 nm.

[0052] Example 1

[0053] This embodiment provides a method for preparing vanadium-based metal oxide@rGO composite aerogel, including the following steps:

[0054] (1) Weigh 183.15 mg of triisopropanol vanadium oxide and measure 5 ml of anhydrous benzyl alcohol into a 10 ml microwave reaction tube, and stir until the solid powder is completely dissolved. Insert the microwave reaction tube into the inner cavity of the microwave reactor and set the parameters of the microwave reactor as follows: heating power of 800 W, maximum temperature of 200 °C, and heating time of 20 min. Centrifuge the product after the reaction to collect the precipitate, and wash it several times with diethyl ether to obtain V2O3 nanoparticles.

[0055] (2) V2O3 nanoparticles were dispersed in an aqueous solution containing the surfactant MEEAA (MEEAA concentration was 50 mL / L) to obtain a first solution. The concentration of V2O3 nanoparticles in the first solution was 15 mg / mL. Then, a dispersion of graphene oxide (GO) nanosheets (GO concentration was 5 mg / mL) was added. The mass ratio of V2O3 nanoparticles to GO nanosheets was controlled to be 1:0.2. After stirring evenly, the mixture was freeze-dried to obtain V2O3@GO composite aerogel.

[0056] (3) V2O3@GO was placed in a tube furnace and calcined at 300℃ and N2 atmosphere for 2h. Graphene oxide was reduced to reduced graphene oxide rGO, and finally V2O3@rGO composite aerogel was obtained.

[0057] Example 2

[0058] This embodiment provides a method for preparing vanadium-based metal oxide@rGO composite aerogel, including the following steps:

[0059] (1) Weigh 129.98 mg of vanadium oxychloride and measure 5 ml of anhydrous benzyl alcohol into a 10 ml microwave reaction tube, and stir until the solid powder is completely dissolved. Insert the microwave reaction tube into the inner cavity of the microwave reactor and set the parameters of the microwave reactor as follows: heating power of 600 W, maximum temperature of 200 °C, and heating time of 20 min. Centrifuge the product after the reaction to collect the precipitate, and wash it several times with diethyl ether to obtain VO 1.52 (OH) 0.77 Nanoparticles.

[0060] (2) VO 1.52 (OH) 0.77 Nanoparticles were dispersed in an aqueous solution containing the surfactant MEEAA (MEEAA concentration of 50 mL / L) to obtain a first solution. The VO in the first solution... 1.52 (OH) 0.77 The concentration of nanoparticles was 15 mg / mL, followed by the addition of a graphene oxide (GO) nanosheet dispersion (GO concentration 5 mg / mL), and the VO2 content was controlled. 1.52 (OH) 0.77 The nanoparticles and GO nanosheets were mixed at a mass ratio of 1:0.2 and then freeze-dried to obtain VO. 1.52 (OH) 0.77 @GO composite aerogel.

[0061] (3) VO 1.52 (OH) 0.77 @GO was placed in a tube furnace and calcined at 300℃ in a N2 atmosphere for 2 hours to finally obtain VO. 1.52 (OH)0.77 @rGO composite aerogel.

[0062] Example 3

[0063] This embodiment provides a method for preparing vanadium-based metal oxide@rGO composite aerogel, including the following steps:

[0064] (1) Weigh 150.20 mg of triisopropanol vanadium oxide and measure 5 ml of anhydrous benzyl alcohol into a 10 ml microwave reaction tube, and stir until the solid powder is completely dissolved. Insert the microwave reaction tube into the inner cavity of the microwave reactor and set the parameters of the microwave reactor as follows: heating power of 1000 W, maximum temperature of 180 °C, and heating time of 30 min. Centrifuge the product after the reaction to collect the precipitate, and wash it several times with diethyl ether to obtain V2O3 nanoparticles.

[0065] (2) V2O3 nanoparticles were dispersed in an aqueous solution containing the surfactant MEEAA (MEEAA concentration was 60 mL / L) to obtain a first solution. The concentration of V2O3 nanoparticles in the first solution was 20 mg / mL. Then, a dispersion of graphene oxide (GO) nanosheets (GO concentration was 7 mg / mL) was added. The mass ratio of V2O3 nanoparticles to GO nanosheets was controlled to be 1:0.1. After stirring evenly, the mixture was freeze-dried to obtain V2O3@GO composite aerogel.

[0066] (3) V2O3@GO was placed in a tube furnace and calcined at 250°C under N2 atmosphere for 3 hours. Graphene oxide was reduced to reduced graphene oxide rGO, and finally V2O3@rGO composite aerogel was obtained.

[0067] Example 4

[0068] This embodiment provides a method for preparing vanadium-based metal oxide@rGO composite aerogel, including the following steps:

[0069] (1) Weigh 170.55 mg of vanadium oxychloride 173.3 g and measure 5 ml of anhydrous benzyl alcohol, respectively, and transfer them to a 10 ml microwave reaction tube. Stir until the solid powder is completely dissolved. Insert the microwave reaction tube into the inner cavity of the microwave reactor and set the parameters of the microwave reactor as follows: heating power of 800 W, maximum temperature of 220 °C, and heating time of 10 min. Centrifuge the product after the reaction to collect the precipitate, and wash it several times with diethyl ether to obtain VO 1.52 (OH) 0.77 Nanoparticles.

[0070] (2) VO 1.52 (OH) 0.77Nanoparticles were dispersed in an aqueous solution containing the surfactant MEEAA (MEEAA concentration of 40 mL / L) to obtain a first solution. The concentration of V₂O₃ nanoparticles in the first solution was 10 mg / mL. Subsequently, a dispersion of graphene oxide (GO) nanosheets (GO concentration of 5 mg / mL) was added to control the V₂O₃ concentration. 1.52 (OH) 0.77 The nanoparticles and GO nanosheets were mixed at a mass ratio of 1:0.5 and then freeze-dried to obtain VO. 1.52 (OH) 0.77 @GO composite aerogel.

[0071] (3) VO 1.52 (OH) 0.77 @GO was placed in a tube furnace and calcined at 275℃ in a N2 atmosphere for 1.5 hours to finally obtain VO. 1.52 (OH) 0.77 @rGO composite aerogel.

[0072] Example 5

[0073] The difference between this embodiment and embodiment 1 is that in step (1), the maximum temperature and heating time of microwave heating are the same, but the heating power is changed to 200W.

[0074] Example 6

[0075] The difference between this embodiment and embodiment 1 is that in step (1), the maximum temperature and heating time of microwave heating are the same, but the heating power is changed to 1500W.

[0076] Example 7

[0077] The difference between this embodiment and embodiment 1 is that in step (2), the mass ratio of V2O3 nanoparticles to GO nanosheets is controlled to be 1:0.03.

[0078] Example 8

[0079] The difference between this embodiment and embodiment 1 is that in step (2), the mass ratio of V2O3 nanoparticles to GO nanosheets is controlled to be 1:0.6.

[0080] Comparative Example 1

[0081] The difference between this comparative example and Example 1 is that triisopropanol vanadium is replaced with ammonium vanadate, and anhydrous benzyl alcohol is replaced with deionized water. The amount of vanadium used is controlled in the same way as in Example 1.

[0082] Comparative Example 2

[0083] The difference between this comparative example and Example 1 is that steps (2) and (3) were not performed, and the product was VO. 1.52(OH) 0.77 Nanoparticles, without reduced graphene oxide.

[0084] Preparation of zinc-ion batteries:

[0085] (1) Preparation of the positive electrode sheet: Using the products of each embodiment and comparative example as the positive electrode material, the positive electrode material, conductive carbon black, and polyvinylidene fluoride were dispersed in an appropriate amount of N-methylpyrrolidone at a mass ratio of 7:2:1. After stirring evenly to form a slurry of suitable consistency, the slurry was coated onto commercial titanium foil and dried at 80°C under vacuum to obtain the positive electrode sheet. The loading of the positive electrode material was 1 ± 0.1 mg / cm³. 2 ;

[0086] (2) Preparation of negative electrode sheet: The surface oxide layer of commercial zinc foil is removed by sanding with sandpaper, and after being wiped clean with alcohol, it is stamped into a circular sheet to obtain the negative electrode sheet;

[0087] (3) Preparation of electrolyte: A 2 mol / L zinc sulfate solution was prepared using zinc sulfate heptahydrate as solute and deionized water as solvent as zinc ion battery electrolyte.

[0088] (4) Assemble the battery cell and inject electrolyte in the following order: negative electrode shell - negative electrode plate - separator - positive electrode plate - gasket - spring plate - positive electrode shell, to obtain a zinc-ion battery. The electrolyte used is 150 mL, the battery shell model is CR2032, and the separator model is glass fiber separator (GF / D).

[0089] Performance testing:

[0090] (a) Discharge capacity test: After the battery is activated, it is discharged at a constant current of 1A / g in the voltage range of 0.3 to 1.4V to obtain the discharge capacity.

[0091] (ii) Rate performance test: Under the voltage range of 0.3 to 1.4V, constant current discharge is performed at a current of 10A / g to obtain the discharge capacity of 10A / g. The ratio of this capacity to the discharge capacity of 1A / g is the rate performance.

[0092] (III) Cyclic performance test: Under the voltage range of 0.3 to 1.4V, constant current charge and discharge cycle is performed at a current of 1A / g, with 500 cycles. The ratio of the discharge capacity of 500 cycles to the discharge capacity of the first cycle is the cycle capacity retention rate. The higher the cycle capacity retention rate, the better the cycle performance.

[0093] The results are shown in Table 1.

[0094] Table 1

[0095]

[0096] In summary, the method of this invention uses a specific type of vanadium-based oxide precursor dissolved in an organic solvent, and utilizes a microwave reaction to obtain vanadium-based metal oxide nanoparticles with a specific composition. Furthermore, the nanoparticles are fixed onto the surface of graphene oxide (GO) nanosheets via electrostatic self-assembly, and calcined to obtain a vanadium-based metal oxide@rGO composite aerogel. This vanadium-based metal oxide@rGO composite aerogel can effectively improve the discharge capacity, rate performance, and cycling performance of the material. The capacity retention is 189.4 mAh / g or higher, preferably 261.5 mAh / g or higher; the rate performance is 44.2% or higher, preferably 57.8% or higher; and the capacity retention after 500 cycles is 71.2% or higher, preferably 88.4% or higher.

[0097] A comparison of Examples 1 and 5-6 shows that when the microwave power is low, the reaction is incomplete, and some precursors are converted into nanoparticles, resulting in insufficient capacity utilization. When the microwave power is too high, the reaction is complete, and the capacity utilization of nanoparticles is relatively high. However, the high power leads to a more intense reaction, and some nanoparticles aggregate, resulting in a rate performance lower than that of Example 1.

[0098] A comparison of Examples 1 and 7-8 shows that when the graphene loading is low, the nanoparticles are unevenly dispersed in the slurry, with some agglomeration, affecting the discharge capacity, and resulting in significant degradation of rate performance and cycle performance. When the loading is high, all performance characteristics decrease due to process and yield factors.

[0099] A comparison between Example 1 and Comparative Example 1 shows that, in the absence of benzyl alcohol solvent and when the precursor used is not a vanadium-based oxide, the precursor cannot be converted into nanoparticles to form large particles larger than 1 micrometer. The performance of these particles is significantly different from that of nanoparticles, and they fail before reaching 500 cycles.

[0100] The comparison between Example 1 and Comparative Example 2 shows that without a load on rGO, nanoparticles tend to agglomerate, resulting in a deterioration in discharge capacity, rate performance, and cycle performance.

[0101] The applicant declares that the detailed method of the present invention is illustrated by the above embodiments, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a vanadium-based metal oxide@rGO composite aerogel, characterized in that, The preparation method includes the following steps: (1) A vanadium-based oxide precursor is dissolved in an organic solvent to obtain a vanadium-based oxide precursor solution. The vanadium-based oxide precursor solution is subjected to a microwave reaction at a temperature of 180℃~220℃, a power of 500W~1200W, and a reaction time of 10min~30min to obtain vanadium-based metal oxide nanoparticles. The vanadium-based oxide precursor includes at least one of triisopropanol vanadium oxytrichlorovanadium and vanadium oxalate oxytrichlorovanadium. said vanadium-based metal oxide nanoparticles are selected from at least one of V2O3, VO 1.52 (OH) 0.77 and VO2; (2) First, the vanadium-based metal oxide nanoparticles are dispersed in an aqueous solution of a surfactant to obtain a first solution. The dispersion of graphene oxide nanosheets is mixed with the first solution and stirred evenly to perform electrostatic self-assembly. After freeze-drying, the mixture is calcined at 250°C to 300°C under a protective atmosphere to obtain vanadium-based metal oxide@rGO composite aerogel. The surfactants include 2-(2-(2-methoxyethoxy)ethoxy)acetic acid and sodium dodecylbenzenesulfonate.

2. The preparation method according to claim 1, characterized in that, The organic solvent in step (1) includes at least one of benzyl alcohol, ethylene glycol and diethylene glycol.

3. The preparation method according to claim 1, characterized in that, The concentration of the vanadium-based oxide precursor in the vanadium-based oxide precursor solution in step (1) is 100 mmol / L to 200 mmol / L.

4. The preparation method according to claim 1, characterized in that, The microwave reaction in step (1) is carried out in the microwave reactor, which is equipped with a microwave reaction tube. The microwave reaction tube is used to hold the reactants and the microwave reactor is heated to the set temperature at a power of 500W~1200W.

5. The preparation method according to claim 1, characterized in that, The microwave reaction in step (1) is accompanied by stirring, and the stirring speed is 500 rpm to 700 rpm.

6. The preparation method according to claim 1, characterized in that, In step (2), the mass ratio of the vanadium-based metal oxide nanoparticles to the graphene oxide nanosheets is 1:(0.1~0.5).

7. The preparation method according to claim 1, characterized in that, The concentration of the aqueous solution of the surfactant is 40 mL / L to 60 mL / L.

8. The preparation method according to claim 1, characterized in that, The dispersion method is ultrasonic dispersion.

9. The preparation method according to claim 1, characterized in that, The concentration of vanadium-based metal oxide nanoparticles in the first solution is 10 mg / mL to 20 mg / mL.

10. The preparation method according to claim 1, characterized in that, The gas in the protective atmosphere in step (2) includes at least one of nitrogen, helium, argon or neon.

11. The preparation method according to claim 1, characterized in that, The calcination time in step (2) is 1h to 3h.

12. The preparation method according to claim 1, characterized in that, The heating rate of calcination in step (2) is 1℃ / min to 5℃ / min.

13. A vanadium-based metal oxide@rGO composite aerogel, characterized in that, The vanadium-based metal oxide @rGO composite aerogel is prepared by the preparation method according to any one of claims 1-12. The vanadium-based metal oxide @rGO composite aerogel comprises reduced graphene oxide nanosheets and vanadium-based metal oxide nanoparticles dispersed on the reduced graphene oxide nanosheets. The vanadium-based metal oxide is selected from V₂O₃ and V₂O₃. 1.52 (OH) 0.77 At least one of VO2.

14. A positive electrode, characterized in that, The positive electrode includes the vanadium-based metal oxide@rGO composite aerogel as described in claim 13.

15. An aqueous zinc-ion battery, characterized in that, The aqueous zinc-ion battery includes the positive electrode as described in claim 14.

Citation Information

Patent Citations

  • Carbon coated nano vanadium pentoxide lithium battery anode material and liquid-phase in-situ preparation method thereof

    CN110817958A

  • Defect-rich vanadium disulfide, preparation method thereof and application of defect-rich vanadium disulfide as positive electrode material in aqueous zinc ion battery

    CN115092960A

  • Preparation method and application of self-supporting binder-free zinc ion battery positive electrode

    CN117542949A

  • Vanadium-based oxide positive electrode material for aqueous zinc ion battery and preparation method of vanadium-based oxide positive electrode material

    CN119797425A