Microfluidic device and method for manufacturing the same

By using electrospinning to form a porous non-woven fabric laminate in a microfluidic device and utilizing a core-shell structure of fluororesin and non-fluororesin, the problems of manufacturing complexity and insufficient liquid repellency are resolved, achieving simple and efficient droplet control.

CN120731354APending Publication Date: 2025-09-30AGC INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202480013700.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-24
Filing Date
2024-01-25
Publication Date
2025-09-30

AI Technical Summary

Technical Problem

The manufacturing process of existing microfluidic devices is complex, and the Teflon layer formed by spin coating may not be sufficiently liquid-repellent, making it difficult to effectively control the movement of droplets.

Method used

The porous layer is formed on the substrate by electrospinning, and the non-woven fabric laminate has a core-shell structure in which the fibers contain fluororesin and non-fluororesin to optimize the liquid repellency of the microfluidic device.

Benefits of technology

A simple manufacturing process is achieved, the liquid repellency of the microfluidic device is significantly improved, and the controllability of droplet movement is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120731354A_ABST
    Figure CN120731354A_ABST
Patent Text Reader

Abstract

A microfluidic device is provided with a laminate in which a porous layer is laminated on a substrate. A method for manufacturing a microfluidic device is performed by spinning a fiber having a core-shell structure by an electrospinning method and depositing the fiber on a substrate to form a porous layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to microfluidic devices and methods of making the same.

[0002] This application claims priority from Japanese Patent Application No. 2023-026913 filed in Japan on February 24, 2023, the contents of which are incorporated herein by reference. Background Art

[0003] Microfluidic devices that utilize electrowetting technology and other techniques for droplet movement are known. In Patent Document 1, a dielectric Parylene C layer is formed on multiple electrodes by CVD to cover the electrodes, and a Teflon (registered trademark) layer is further formed thereon by spin coating to facilitate droplet movement.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2022-20665 Summary of the Invention

[0007] Problems to be solved by the invention

[0008] However, the manufacturing process of the microfluidic device described in Patent Document 1 is complicated.

[0009] Furthermore, although a Teflon layer formed by spin coating has excellent hydrophobicity, its liquid repellency is not necessarily sufficient. In order to facilitate the control of the movement of droplets, further improvement of the liquid repellency is desired.

[0010] The present invention provides a microfluidic device having excellent liquid repellency and a method for manufacturing a microfluidic device having excellent liquid repellency by a simple process.

[0011] Solutions for solving problems

[0012] The present invention provides a microfluidic device having the following structures [1] to

[20] and a method for manufacturing the same.

[0013] [1] A microfluidic device comprising a laminate having a porous layer laminated on a substrate.

[0014] [2] The microfluidic device according to [1], wherein the porous layer is a nonwoven fabric layer.

[0015] [3] The microfluidic device according to [2], wherein the non-woven fabric is formed by electrospinning.

[0016] [4] The microfluidic device according to [2] or [3], wherein the fibers constituting the nonwoven fabric contain a fluororesin.

[0017] [5] The microfluidic device according to [4], wherein the fibers constituting the nonwoven fabric further contain a non-fluorine resin.

[0018] [6] The microfluidic device according to any one of [2] to [5], wherein the fibers constituting the nonwoven fabric have a core-shell structure.

[0019] [7] The microfluidic device according to [6], wherein one of the core and the shell of the core-shell structure comprises a fluororesin and the other comprises a non-fluororesin.

[0020] [8] The microfluidic device according to [4], [5] or [7], wherein the fluororesin is an amorphous fluororesin.

[0021] [9] The microfluidic device according to [4], [5], [7] or [8], wherein the fluororesin comprises a polymer having a unit having a fluorinated aliphatic ring structure constituting the main chain.

[0022]

[10] The microfluidic device according to [9], wherein the unit having a fluorinated aliphatic ring structure constituting the main chain is at least one selected from the group consisting of a unit formed by cyclopolymerization of a diene fluorinated monomer and a unit based on a cyclic fluorinated monomer.

[0023]

[11] The microfluidic device according to [5] or [7], wherein the non-fluororesin is a crystalline non-fluororesin.

[0024]

[12] The microfluidic device according to [5] or [7], wherein the non-fluorine resin is at least one selected from the group consisting of polycaprolactone, polyethylene glycol, polyvinyl alcohol, polyacrylonitrile, polyaniline, acrylic resin, polyurethane, polystyrene, polycarbonate, polyvinyl pyrrolidone, chitosan, gelatin and cellulose acetate.

[0025]

[13] The microfluidic device according to any one of [1] to

[12] , which is a biochip.

[0026]

[14] A method for manufacturing a microfluidic device, the method comprising spinning a fiber having a core-shell structure by an electrospinning method and depositing the fiber on a substrate to form a porous layer.

[0027]

[15] The production method according to

[14] , wherein either the core or the shell of the core-shell structure comprises a fluororesin and the other comprises a non-fluororesin.

[0028]

[16] The production method according to

[15] , wherein the fluororesin is an amorphous fluororesin.

[0029]

[17] The production method according to

[15] or

[16] , wherein the fluororesin comprises a polymer having a unit having a fluorinated aliphatic ring structure constituting a main chain.

[0030]

[18] The production method according to

[17] , wherein the unit having a fluorinated aliphatic ring structure constituting the main chain is at least one selected from the group consisting of a unit formed by cyclopolymerization of a diene fluorinated monomer and a unit based on a cyclic fluorinated monomer.

[0031]

[19] The production method according to any one of

[15] to

[18] , wherein the non-fluororesin is a crystalline non-fluororesin.

[0032]

[20] The production method according to any one of

[15] to

[18] , wherein the non-fluorine resin is at least one selected from the group consisting of polycaprolactone, polyethylene glycol, polyvinyl alcohol, polyacrylonitrile, polyaniline, acrylic resin, polyurethane, polystyrene, polycarbonate, polyvinyl pyrrolidone, chitosan, gelatin and cellulose acetate.

[0033] Effects of the Invention

[0034] The microfluidic device of the present invention has excellent liquid repellency.

[0035] The method for manufacturing a microfluidic device of the present invention can manufacture a microfluidic device having excellent liquid repellency through a simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic cross-sectional view showing an example of a microfluidic device.

[0037] Figure 2 This is a schematic diagram showing the configuration of an example of an electrospinning apparatus used for producing a nonwoven fabric composed of fibers having a core-sheath structure. DETAILED DESCRIPTION

[0038] The meanings and definitions of the terms used in the present invention are as follows.

[0039] The "aliphatic ring structure" refers to a saturated or unsaturated ring structure that does not have aromaticity.

[0040] A "fluorinated aliphatic ring structure" refers to an aliphatic ring structure in which a fluorine atom or a fluorine-containing group is bonded to at least a portion of the carbon atoms constituting the main skeleton of the ring. Examples of the fluorinated group include perfluoroalkyl, perfluoroalkoxy, and =CF2. Substituents other than fluorine atoms and fluorine-containing groups may also be bonded to a portion of the carbon atoms constituting the main skeleton of the ring.

[0041] The "etheric oxygen atom" refers to an oxygen atom (-COC-) existing between carbon atoms.

[0042] The “mass average molecular weight” is a value converted into polymethyl methacrylate (hereinafter, also referred to as “PMMA”) measured by gel permeation chromatography (hereinafter, also referred to as “GPC”).

[0043] In this specification, the group represented by Formula 2 is also referred to as "group 2," and the compound represented by Formula ma1 is also referred to as "compound ma1." The same applies to groups and compounds represented by other formulae.

[0044] "To" indicating a numerical range means that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0045] For convenience of explanation, the scales of components in the drawings may differ from the actual scales.

[0046] Microfluidic devices

[0047] A microfluidic device according to one embodiment of the present invention includes a laminate in which a porous layer is laminated on a substrate.

[0048] The laminate may have a porous layer stacked on one surface of the substrate, or may have a porous layer stacked on one surface and the other surface of the substrate. In addition, the substrate and the porous layer may be in contact with each other, or another layer may be sandwiched between the substrate and the porous layer.

[0049] The microfluidic device according to this embodiment can be similar to a known microfluidic device except that at least a portion of the components of the microfluidic device is the aforementioned laminate.

[0050] In the microfluidic device according to this embodiment, at least a portion of the surface of the porous layer side of the laminate typically forms a microchannel for flowing liquid, and the liquid flowing in the microchannel comes into contact with the porous layer. The liquid typically contains water.

[0051] The microfluidic device may be a type in which droplets circulate in a microchannel or a type in which liquid circulates continuously in the microchannel. The type in which droplets circulate in a microchannel is preferred due to its excellent liquid repellency and high usefulness.

[0052] An example of a microfluidic device in which droplets flow through a microchannel is: Figure 1 As shown, a digital microfluidic device that drives droplets by electrowetting on dielectric layers (EWOD) is provided. However, the microfluidic device of the present invention is not limited to this example.

[0053] Figure 1 The microfluidic device includes a first stack 1 and a second stack 2 .

[0054] The first laminate 1 includes a first substrate 11 having a plurality of electrodes 12 and a first dielectric layer 13 located on the first substrate 11 and provided to cover the plurality of electrodes 12. The first dielectric layer 13 is a porous layer.

[0055] The second laminate 2 includes a second substrate 21 having a common electrode 22 and a second dielectric layer 23 located on the first substrate 11 and provided so as to cover the common electrode 22. The second dielectric layer 23 may or may not be a porous layer.

[0056] The first stack 1 and the second stack 2 are arranged with a gap therebetween so that the first dielectric layer 13 and the second dielectric layer 23 face each other. The gap between the first stack 1 and the second stack 2 forms a microchannel through which the droplets L flow. The width of the gap, that is, the distance between the first stack 1 and the second stack 2, is, for example, 100 to 300 μm.

[0057] Figure 1 The microfluidic device is typically arranged and used such that the first stack 1 is located below the second stack 2 .

[0058] A dielectric layer other than a porous layer may be provided between the plurality of electrodes 12 and the first dielectric layer 13 .

[0059] (Porous layer)

[0060] By laminating a porous layer on a substrate, excellent liquid repellency is achieved. Due to the large number of pores, the porous layer has fine surface irregularities. It is believed that this fine irregularity creates a lotus effect, resulting in excellent liquid repellency. Furthermore, by laminating a porous layer on a substrate, excellent liquid repellency can be imparted, simplifying the manufacturing process.

[0061] Microfluidic devices are Figure 1 In the case of the digital microfluidics device shown, the porous layer is preferably a dielectric layer. A dielectric is a material in which the property of charge being present at both ends of the material (dielectricity) is more dominant than the electrical conductivity.

[0062] Examples of the porous layer include a fiber layer and a porous material layer.

[0063] The fiber layer is a layer composed of fibers, and examples thereof include those obtained by compacting fibers such as nanofibers (eg, nonwoven fabrics), woven fabrics, and knitted fabrics. The fibers themselves may or may not be porous.

[0064] The porous material layer is a layer composed of a porous material. The porous material is a material that is porous itself, and examples thereof include activated carbon, diatomaceous earth, and silica gel.

[0065] Among these, the porous layer is preferably a nonwoven fabric layer because the resulting layer has excellent flatness.

[0066] Among nonwoven fabrics, those formed by electrospinning (also known as electrolytic spinning) are preferred due to their superior liquid repellency. Electrospinning allows for the simple production of nonwoven fabrics composed of fibers with nanometer-scale diameters. Furthermore, nonwoven fabrics formed by electrospinning tend to have smaller pore sizes and more uniform pore size distribution than nonwoven fabrics formed by other methods.

[0067] As the fibers constituting the nonwoven fabric, fibers containing a resin are preferred in terms of superior liquid repellency, anti-biological adhesion properties, and dielectric properties.

[0068] Examples of the resin include fluororesins and non-fluororesins. Fluororesins are preferred due to their excellent liquid repellency and anti-biological adhesion properties. Fluororesins and non-fluororesins may also be used in combination. Fluororesins and non-fluororesins will be described in detail later.

[0069] The fiber containing the resin may further contain additives such as antimicrobial agents, antistatic agents, flame retardants and anti-aging agents.

[0070] The content of the resin in the resin-containing fiber is preferably 20% by mass or more, more preferably 40% by mass or more, and may be 100% by mass, relative to the total mass of the resin-containing fiber.

[0071] The fibers constituting the nonwoven fabric may have a homogeneous structure or a heterogeneous structure in the radial direction of the fibers.

[0072] Examples of fibers having a homogeneous structure include fibers formed from a single resin or fibers formed from a blend of two or more resins. Examples of blended resins include blends of two or more fluororesins, blends of one or more fluororesins and one or more non-fluororesins, and blends of two or more non-fluororesins.

[0073] Examples of fibers having a heterogeneous structure include fibers having a core-sheath structure (hereinafter also referred to as "core-sheath fibers"). Examples of core-sheath fibers include fibers in which one of the core and the sheath comprises a fluororesin and the other comprises a non-fluororesin; fibers in which the core and the sheath comprise different fluororesins; and fibers in which the core and the sheath comprise different non-fluororesins.

[0074] The fibers constituting the nonwoven fabric are preferably core-sheath fibers for superior liquid repellency, and more preferably, at least one of the core and the sheath comprises a fluororesin. Furthermore, for superior molding processability and production costs, it is more preferred that one of the core and the sheath comprises a fluororesin and the other comprises a non-fluororesin.

[0075] When one of the core and the sheath comprises a fluororesin and the other comprises a non-fluororesin, the proportion of the fluororesin relative to the total mass of the core-sheath fibers is preferably 5 to 95% by mass, more preferably 10 to 90% by mass. Furthermore, the proportion of the non-fluororesin relative to the total mass of the core-sheath fibers is preferably 5 to 95% by mass, more preferably 10 to 90% by mass.

[0076] When the core comprises a fluororesin and the shell comprises a non-fluororesin, the proportion of the fluororesin relative to the mass of the core is preferably 20% by mass or more, more preferably 40% by mass or more, and may be 100% by mass. Furthermore, the proportion of the non-fluororesin relative to the mass of the shell is preferably 20% by mass or more, more preferably 40% by mass or more, and may be 100% by mass.

[0077] When the shell comprises a fluororesin and the core comprises a non-fluororesin, the proportion of the fluororesin relative to the mass of the shell is preferably 20% by mass or more, more preferably 40% by mass or more, and may be 100% by mass. Furthermore, the proportion of the non-fluororesin relative to the mass of the core is preferably 20% by mass or more, more preferably 40% by mass or more, and may be 100% by mass.

[0078] The fluororesin is described in detail below, but an amorphous fluororesin is preferred. On the other hand, when the nonwoven fabric is formed by electrospinning, it is preferred that at least one of the core and the shell contain a crystalline non-fluororesin. Therefore, when the nonwoven fabric comprises core-shell fibers formed by electrospinning, it is preferred that one of the core and the shell contain an amorphous fluororesin and the other contain a crystalline non-fluororesin.

[0079] The diameter of the fibers constituting the nonwoven fabric is preferably 20 to 800 nm, more preferably 100 to 700 nm, and particularly preferably 300 to 600 nm. If the diameter of the fibers constituting the nonwoven fabric is below the upper limit, the liquid repellency is further improved, while if it is above the lower limit, the mechanical strength is further improved.

[0080] The fiber diameter is determined by the method described in Examples below.

[0081] When the fibers constituting the nonwoven fabric are core-sheath fibers, the diameter of the core is preferably 2 to 760 nm, more preferably 5 to 670 nm, and particularly preferably 15 to 570 nm.

[0082] The thickness of the shell is preferably 14 to 399 nm, more preferably 48 to 348 nm, and particularly preferably 143 to 293 nm.

[0083] The core diameter was determined by energy dispersive X-ray spectroscopy.

[0084] The thickness of the shell is calculated as (fiber diameter - core diameter) / 2.

[0085] When the fibers constituting the nonwoven fabric are core-sheath fibers, the ratio (hereinafter also referred to as the "sheath / core ratio"), expressed as the mass of the sheath / the mass of the core, is preferably 1 / 1 to 19 / 1, more preferably 2 / 1 to 9 / 1. When the sheath / core ratio is at least the lower limit, liquid repellency is further improved, while when it is at most the upper limit, moldability is further improved.

[0086] The thickness of the porous layer is preferably 5 to 900 μm, more preferably 20 to 300 μm, and particularly preferably 50 to 200 μm. If the thickness of the porous layer is at least the lower limit, liquid repellency and mechanical strength are further improved. If it is at most the upper limit, moldability and productivity are excellent.

[0087] The thickness of the porous layer is measured by the method described in Examples below.

[0088] The water contact angle of the porous layer surface is preferably 100° or greater, more preferably 115° or greater, and particularly preferably 130° or greater. The higher the water contact angle of the porous layer surface, the better. The upper limit is not particularly limited, but is, for example, 160° or less.

[0089] The water contact angle is an indicator of water repellency. The higher the water contact angle, the better the water repellency.

[0090] The water contact angle is measured by the method described in Examples below.

[0091] The surface roughness of the porous layer is preferably 5 to 5000 nm, more preferably 20 to 1000 nm, and particularly preferably 50 to 500 nm, as measured by a laser microscope using the evaluation method specified in ISO 25178. When the Sa (arithmetic mean height) value is within this range, liquid repellency is further improved.

[0092] The density of the porous layer is preferably 2 to 150 g / m 3 , more preferably 5 to 100 g / m 3 , particularly preferably 7 to 80 g / m 3When the density is within the above range, the liquid repellency is further improved.

[0093] Fluororesin

[0094] As the fluororesin, any known fluororesin can be used as long as it can form a porous layer.

[0095] An example of a preferred fluororesin is an amorphous fluororesin. Amorphous fluororesins have excellent solvent solubility and can be used as a solution as a raw material, so a porous layer can be easily formed.

[0096] Examples of amorphous fluororesins include polymers containing a fluorinated aliphatic ring structure in their main chain (hereinafter referred to as "polymer A"). Polymer A, due to the presence of a fluorinated aliphatic ring structure in its main chain, exhibits low absorption from ultraviolet to near-infrared light and exhibits excellent transparency. Polymers containing a fluorinated aliphatic ring structure in their main chain are soluble in solvents. Furthermore, the main chain is resistant to decomposition, resulting in excellent weather resistance.

[0097] The fluorinated aliphatic ring structure may be a carbocyclic structure in which the ring skeleton is composed only of carbon atoms, or a heterocyclic structure in which the ring skeleton contains atoms other than carbon atoms (hereinafter, atoms other than carbon atoms are also referred to as "heteroatoms"). Examples of heteroatoms include oxygen atoms and nitrogen atoms. The number of atoms constituting the ring skeleton of the fluorinated aliphatic ring structure is preferably 4 to 7, particularly preferably 5 to 6. That is, the aliphatic ring structure is preferably a 4- to 7-membered ring, particularly preferably a 5- to 6-membered ring.

[0098] The fluorinated aliphatic ring structure is preferably a heterocyclic structure having an ethereal oxygen atom in the ring skeleton, and particularly preferably a heterocyclic structure having 1 to 2 ethereal oxygen atoms in the ring skeleton, from the viewpoint of better transparency and solvent solubility.

[0099] Examples of the fluorinated aliphatic ring structure include a hydrocarbon ring structure or a heterocyclic ring structure in which a part or all of hydrogen atoms are substituted with fluorine atoms.

[0100] Among them, a fluorinated alicyclic structure in which a part or all of the hydrogen atoms of a heterocyclic structure having an etheric oxygen atom in the ring skeleton are substituted with fluorine atoms is preferred, and a fluorinated alicyclic structure in which a part or all of the hydrogen atoms of a heterocyclic structure having 1 to 2 etheric oxygen atoms in the ring skeleton are substituted with fluorine atoms is particularly preferred.

[0101] The fluorinated aliphatic ring structure is preferably a perfluoroaliphatic ring structure in which all hydrogen atoms in a hydrocarbon ring structure or a heterocyclic ring structure are substituted with fluorine atoms.

[0102] As the polymer A, a polymer having a unit having a fluorinated aliphatic ring structure constituting the main chain (hereinafter also referred to as "unit a1") is preferred. The unit a1 is preferably a perfluorinated unit.

[0103] "Constitute the main chain" of a fluorinated aliphatic ring structure means that at least one of the carbon atoms constituting the ring backbone of the fluorinated aliphatic ring structure is a carbon atom constituting the main chain of the polymer. "Constitute the main chain of the polymer by two carbon atoms derived from polymerizable double bonds" means that one or two adjacent carbon atoms constituting the ring of the fluorinated aliphatic ring structure are carbon atoms derived from a single polymerizable double bond.

[0104] For example, when unit a1 is formed by addition polymerization of a monoolefin monomer, two carbon atoms derived from the polymerizable double bond constitute the main chain, and these two carbon atoms are adjacent carbon atoms of the ring backbone, or one of these two carbon atoms is a carbon atom of the ring backbone. Alternatively, when unit a1 is formed by cyclopolymerization of a diene monomer, a total of four carbon atoms derived from two polymerizable double bonds constitute the main chain, and two to four of these four carbon atoms constitute the ring backbone.

[0105] Examples of the unit a1 include units formed by cyclopolymerization of a diene fluorinated monomer, units based on a cyclic fluorinated monomer, etc. These units may be used alone or in combination of two or more.

[0106] A diene fluorinated monomer is a monomer having two polymerizable double bonds and a fluorine atom. In the case of a diene fluorinated monomer, unit a1 is formed by cyclopolymerization. The polymerizable double bond is not particularly limited, but is preferably a vinyl group, an allyl group, an acryloyl group, or a methacryloyl group. In these polymerizable double bonds, some or all of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine atoms.

[0107] As the diene fluorinated monomer, compound ma1 is preferred.

[0108] CF2=CF-Q-CF=CF2···Formula ma1

[0109] Here, Q is a perfluoroalkylene group having 1 to 6 carbon atoms, a part of the fluorine atoms of which may be substituted with a halogen atom other than a fluorine atom, and the group may have an ethereal oxygen atom.

[0110] In formula ma1, the carbon number of the perfluoroalkylene group in Q is 1 to 6, preferably 1 to 5, and particularly preferably 1 to 3. The perfluoroalkylene group is preferably linear or branched, and particularly preferably linear.

[0111] A portion of the fluorine atoms in the perfluoroalkylene group may be substituted with a halogen atom other than a fluorine atom. Examples of the halogen atom other than a fluorine atom include a chlorine atom and a bromine atom.

[0112] The perfluoroalkylene group may have an ethereal oxygen atom.

[0113] As Q, a perfluoroalkylene group having an etheric oxygen atom is preferred. In this case, the etheric oxygen atom in the perfluoroalkylene group may be present at one end of the perfluoroalkylene group, at both ends of the perfluoroalkylene group, or between carbon atoms of the perfluoroalkylene group. In terms of better cyclopolymerization properties, it is preferably present at one end of the perfluoroalkylene group.

[0114] As Q, group q1 or group q2 is preferred.

[0115] -(CR 11 R 12 )h-···Formula q1

[0116] -(CR 13 R 14 ) i O(CR 15 R 16 ) j -···Formula q2

[0117] Among them, R 11 、R 12 、R 13 、R 14 、R 15 and R 16 Each independently represents a fluorine atom, a chlorine atom, a trifluoromethyl group or a trifluoromethoxy group. h is an integer from 2 to 4, and multiple R 11 and R 12 are the same or different, i and j are each an integer from 0 to 3, and i+j is an integer from 1 to 3. When i is 2 or 3, multiple R 13 and R 14 They may be the same or different. When j is 2 or 3, multiple R 15 and R 16 They may be the same or different.

[0118] Preferably h is 2 or 3, preferably R 11 and R 12 All are fluorine atoms, or all except one or two are fluorine atoms. Preferably, i is 0, and j is 1 or 2, and preferably R 15 and R 16 All are fluorine atoms, or all except one or two are fluorine atoms.

[0119] Specific examples of the compound ma1 include the following compounds.

[0120] CF2=CFOCF2CF=CF2,

[0121] CF2=CFOCF(CF3)CF=CF2、

[0122] CF2=CFOCF2CF2CF=CF2,

[0123] CF2=CFOCF2CF(CF3)CF=CF2,

[0124] CF2=CFOCF(CF3)CF2CF=CF2,

[0125] CF2=CFOCFClCF2CF=CF2、

[0126] CF2=CFOCCl2CF2CF=CF2,

[0127] CF2=CFOCF2OCF=CF2、

[0128] CF2=CFOC(CF3)2OCF=CF2、

[0129] CF2=CFOCF2CF(OCF3)CF=CF2,

[0130] CF2=CFCF2CF=CF2、

[0131] CF2=CFCF2CF2CF=CF2、

[0132] CF2=CFCF2OCF2CF=CF2.

[0133] Examples of the cyclic fluorinated monomer include: a monomer comprising a fluorinated aliphatic ring and having a polymerizable double bond between carbon atoms constituting the fluorinated aliphatic ring; and a monomer comprising a fluorinated aliphatic ring and having a polymerizable double bond between a carbon atom constituting the fluorinated aliphatic ring and a carbon atom outside the fluorinated aliphatic ring; etc.

[0134] As the cyclic fluorinated monomer, compound ma2 or compound ma3 is preferred.

[0135]

[0136] Among them, X 1 、X 2 、X 3 、X 4 、Y 1 and Y 2 are each independently a fluorine atom, a perfluoroalkyl group optionally having an ethereal oxygen atom, or a perfluoroalkoxy group optionally having an ethereal oxygen atom, X 3 and X 4 They are optionally bonded to each other to form a ring.

[0137] In formula ma2 and ma3, X1 、X 2 、X 3 、X 4 、Y 1 and Y 2 The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 7, more preferably 1 to 5, and particularly preferably 1 to 4. The perfluoroalkyl group is preferably linear or branched, and linear is particularly preferred. The perfluoroalkyl group is preferably trifluoromethyl, pentafluoroethyl, or heptafluoropropyl, and trifluoromethyl is particularly preferred.

[0138] As X 1 、X 2 、X 3 、X 4 、Y 1 and Y 2 The perfluoroalkoxy group in the above-mentioned group may be a group in which an oxygen atom (—O—) is bonded to the above-mentioned perfluoroalkyl group, and a trifluoromethoxy group is particularly preferred.

[0139] When the carbon number of the perfluoroalkyl group or the perfluoroalkoxy group is 2 or more, an etheric oxygen atom (—O—) may be interposed between carbon atoms of the perfluoroalkyl group or the perfluoroalkoxy group.

[0140] In formula ma2, X 1 A fluorine atom is preferred.

[0141] X 2 A fluorine atom, a trifluoromethyl group or a perfluoroalkoxy group having 1 to 4 carbon atoms is preferred, and a fluorine atom or a trifluoromethoxy group is particularly preferred.

[0142] X 3 and X 4 Each independently is preferably a fluorine atom or a perfluoroalkyl group having 1 to 4 carbon atoms, and particularly preferably a fluorine atom or a trifluoromethyl group.

[0143] X 3 and X 4 The number of atoms constituting the ring skeleton of the ring is preferably 4 to 7, more preferably 5 to 6.

[0144] In formula ma3, Y 1 and Y 2 A fluorine atom, a perfluoroalkyl group having 1 to 4 carbon atoms, or a perfluoroalkoxy group having 1 to 4 carbon atoms are each independently preferred, and a fluorine atom or a trifluoromethyl group is particularly preferred.

[0145] Preferred specific examples of the compound ma2 include compounds ma21 to ma25.

[0146] Preferred specific examples of the compound ma3 include compounds ma31 and ma32.

[0147]

[0148] The unit a1 is preferably at least one selected from the group consisting of the following units a11 to a16.

[0149] Units a11 to a14 are formed by cyclopolymerization of compound ma1. Cyclopolymerization of compound ma1 generates at least one of units a11 to a14. In this case, units a11 to a14 are likely to have a structure in which the number of atoms constituting the ring backbone of the fluorinated aliphatic ring is 5 or 6. Polymers containing two or more of these units may also be generated.

[0150] In other words, the compound ma1 preferably has a structure in which the number of atoms constituting the ring skeleton, including the atoms in Q, in the following units a11 to a14 is 5 or 6.

[0151] The unit a15 described below is a unit formed from the compound ma2, and the unit a16 described below is a unit formed from the compound ma3.

[0152]

[0153] As the unit a1, a unit formed by cyclopolymerization of a diene fluorinated polymer is preferred in view of its superior chemical stability.

[0154] The unit a1 contained in the polymer A may be one type or two or more types.

[0155] The content of the units a1 in the polymer A is preferably 30 mol% or more, more preferably 50 mol% or more, further preferably 70 mol% or more, and may be 100 mol% based on the total of all units constituting the polymer A. When the content of the units a1 is at least the lower limit, transparency and solubility in solvents are further improved.

[0156] The polymer A may further have other units (hereinafter also referred to as "units a2") in addition to the units a1, if necessary.

[0157] Unit a2 is not particularly limited, as long as it is based on a monomer copolymerizable with the monomer forming unit a1. Examples of unit a2 include units based on monomers having a reactive functional group and a polymerizable double bond (hereinafter also referred to as "unit a21"), units based on fluorinated olefins such as tetrafluoroethylene, and units based on fluorinated vinyl ethers. Polymer A may contain one or more units a2.

[0158] Examples of the polymerizable double bond include CF2=CF-, CF2=CH-, CH2=CF-, CFH=CF-, CFH=CH-, CF2=C-, and CF=CF-.

[0159] Reactive functional groups are groups with the following reactivity: when drying, for example, polymer molecules containing the reactive functional group react with each other, or the polymer reacts with substances other than the polymer (such as metals and alloys) to form chemical bonds (such as hydrogen bonds and covalent bonds). Examples of reactive functional groups include carboxyl groups, acyl halide groups, alkoxycarbonyl groups, carbonyloxy groups, carbonate groups, sulfonyl groups, phosphonyl groups, hydroxyl groups, mercapto groups, silanol groups, and coupling groups. Unit a21 may have an ester group or an amide group.

[0160] As the unit a2, a perfluorinated unit is preferred except for the unit a21. In the case of the unit a21, it is preferred that no hydrogen atom is bonded to a carbon atom except for the portion of the reactive functional group.

[0161] As an example of the unit a21, the unit a21-1 can be given.

[0162] Unit a21-1 can be made to work by making CF2=CF-OR f -X is formed by polymerization.

[0163]

[0164] Among them, R f It is a perfluoroalkylene group which may have an ethereal oxygen atom, X is COOH, COOR, SO2F, SO3R or SO3H, and R is an alkyl group having 1 to 5 carbon atoms.

[0165] In formula a21-1, R f The perfluoroalkylene group in is preferably linear or branched. The number of carbon atoms in the perfluoroalkylene group is preferably 2 to 10, more preferably 2 to 7, and particularly preferably 2 to 5.

[0166] The perfluoroalkylene group may have an etheric oxygen atom. In this case, the number of etheric oxygen atoms in the perfluoroalkylene group may be one or two or more.

[0167] As R f Specific examples of include the following groups.

[0168] -CF2CF2CF2-,

[0169] -CF2CF(CF3)OCF2CF2-、

[0170] -CF2CF2CF(CF3)OCF2CF2-、

[0171] -CF2CF(CF3)OCF2CF2CF2-.

[0172] The alkyl group of R in COOR and SO3R is preferably linear or branched. The alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, and a methyl group is particularly preferred.

[0173] As X, COOCH3, SO2F, COOH or SO3H is preferred.

[0174] As unit a21-1, -OR in the formula is preferred f -X is any of the following.

[0175] -OCF2CF(CF3)OCF2CF2COOCH3,

[0176] -OCF2CF2CF2COOCH3,

[0177] -OCF2CF(CF3)OCF2CF2SO2F,

[0178] -OCF2CF2CF2COOH,

[0179] -OCF2CF(CF3)OCF2CF2CF2COOCH3,

[0180] -OCF2CF(CF3)OCF2CF2SO3H.

[0181] Polymer A may have a functional group at the end of the main chain. Examples of the functional group include an alkoxycarbonyl group having an alkoxy group having 1 to 3 carbon atoms (hereinafter also referred to as an "ester group"), an amide group having a coupling group, a carboxyl group, and a carboxylic acid fluoride group.

[0182] The alkoxy group in the ester group may be linear or branched. The number of carbon atoms in the alkoxy group is preferably 1 or 2, particularly preferably 1. Therefore, as the ester group, a methoxycarbonyl group or an ethoxycarbonyl group is preferred, and a methoxycarbonyl group is particularly preferred.

[0183] By having an amide group having a coupling group, excellent adhesion is exhibited.

[0184] Examples of the coupling group include a silane coupling group and a phenol group. A silane coupling group is preferred because it provides better adhesion.

[0185] As the coupling group, Group 2 is preferred in terms of better adhesion to the substrate.

[0186] -SiR 1 R 2 R 3 Formula 2

[0187] Among them, R 1、R 2 and R 3 Each independently represents an alkoxy group having 1 to 3 carbon atoms or an alkyl group having 1 to 3 carbon atoms, R 1 、R 2 and R 3 At least one of them is the aforementioned alkoxy group.

[0188] R 1 、R 2 and R 3 In the example, the alkoxy group may be linear or branched. The alkyl group may be linear or branched.

[0189] By R 1 、R 2 and R 3 At least one of the R groups is an alkoxy group, thereby achieving better adhesion to the substrate. 1 、R 2 and R 3 When there are alkoxy groups in , the number of alkoxy groups is preferably 2 or 3.

[0190] As SiR 1 R 2 R 3 Specific examples include a methyldiethoxysilyl group, a methyldimethoxysilyl group, a trimethoxysilyl group, and a triethoxysilyl group.

[0191] Examples of the amide group having Group 2 include Group 3.

[0192] -CONH-R 4 -SiR 1 R 2 R 3 Formula 3

[0193] Among them, R 1 、R 2 and R 3 As shown in the above formula 2, R 1 、R 2 and R 3 As defined, R 4 It is an alkylene group, a group having an imino group between carbon atoms of the alkylene group, or an arylene group.

[0194] R 4 In the alkylene group, the alkylene group may be linear or branched. The number of carbon atoms in the alkylene group is preferably 1 to 10, more preferably 1 to 4. In groups having an imino group between carbon atoms in the alkylene group, the number of carbon atoms in the alkylene group is preferably 2 to 10, and the number of imino groups is preferably 1 to 3. The number of carbon atoms in the arylene group is preferably 6 to 10.

[0195] As R 4Specific examples include -(CH2)3-, -(CH2)2NH(CH2)3-, and phenylene.

[0196] The mass average molecular weight (Mw) of the fluororesin is preferably 10,000 to 500,000, more preferably 30,000 to 200,000. When Mw is at least the lower limit, the toughness of the fluororesin is further improved, while when it is at most the upper limit, the solubility in solvents and moldability are further improved.

[0197] Fluororesins may be commercially available or produced by known methods. Preferred commercially available examples of fluororesins include CYTOP (registered trademark) (perfluoro(3-butenyl vinyl ether) cyclopolymer) from AGC Corporation, Teflon (registered trademark) AF (tetrafluoroethylene / perfluoro(2,2-dimethyl-1,3-dioxole) copolymer) from The Chemours Company, Hyflon (registered trademark) AD (tetrafluoroethylene / perfluoro(4-methoxy-1,3-dioxole) copolymer) from Solvay, and FluoroPel PFC1601V and PFC1101V from CYTONIX Corporation.

[0198] These fluororesins may be used alone or in combination of two or more.

[0199] <Non-fluorine resin>

[0200] Non-fluorine resin is a resin that does not contain fluorine resin.

[0201] As the non-fluorine resin, any known non-fluorine resin can be used as long as it can form a porous layer.

[0202] A preferred example of a non-fluorocarbon resin is a crystalline non-fluorocarbon resin. Crystalline non-fluorocarbon resins are non-fluorocarbon resins that, when cured by lowering the temperature, have crystalline portions with regularly arranged molecules. Nonwoven fabrics containing fibers containing crystalline non-fluorocarbon resins exhibit superior chemical resistance and mechanical strength.

[0203] Examples of the non-fluorine-containing resin include polycaprolactone, polyethylene glycol, polyvinyl alcohol, polyacrylonitrile, polyaniline, acrylic resins, polyurethane, polystyrene, polycarbonate, polyvinyl pyrrolidone, chitosan, gelatin, and cellulose acetate.

[0204] Examples of the crystalline non-fluorine resin include polycaprolactone, polyethylene glycol, polyacrylonitrile, polyaniline, chitosan, gelatin, and cellulose acetate.

[0205] Among these, polycaprolactone and polyacrylonitrile are preferred in terms of superior molding processability and mechanical strength.

[0206] These non-fluorine resins may be used alone or in combination of two or more.

[0207] (Base material)

[0208] The substrate may be a material known as a substrate for a microfluidic device, and examples thereof include glass substrates, polycarbonate, polyimide, and silicon wafers. The thickness of the substrate is, for example, 0.01 to 10 mm.

[0209] Other layers may be formed on the surface of the substrate.

[0210] Examples of the other layers include electrodes and dielectric layers that are not porous layers. The electrodes and dielectric layers that are not porous layers may be formed in sequence on the substrate.

[0211] Examples of the material of the electrode include metals, metal mixtures, metal-semiconductor mixtures, and conductive resins. The thickness of the electrode is, for example, 0.001 to 10 mm.

[0212] Examples of non-porous dielectric layers include layers of dielectrics (e.g., Parylene C) formed by CVD and layers of dielectrics (e.g., fluororesins such as ethylene-tetrafluoroethylene copolymer) formed by wet coating methods such as spin coating. The thickness of the non-porous dielectric layer is, for example, 0.1 to 1000 μm.

[0213] 〔use〕

[0214] The uses of microfluidic devices are not particularly limited, and examples include: biochips, clinical on-site instant diagnosis of diseases, biosensors, cell culture (for example, the supply of insulin and penicillin to culture medium), drug delivery applications, FDA applications in food safety, microfluidic fuel cells and energy uses, and microfluidic reactors (for example, lipid nanoparticle (LNP) synthesis).

[0215] Examples of biochip applications include enzyme analysis (e.g., glucose and lactate determination), DNA analysis (e.g., PCR and high-throughput sequencing), DNA cloning, antibody purification, production, and analysis, immunological testing, and proteome analysis. "Proteome" is a new term that combines the words protein and genome. A genome refers to all the genetic information possessed by an organism, while a proteome refers to all proteins expressed (with the potential for expression) within a cell. When a microfluidic device is used as a biochip, it is desirable that the biochip maintain its liquid repellency even after a certain period of contact with various biological test fluids used.

[0216] [Method for manufacturing microfluidic device]

[0217] A method for manufacturing a microfluidic device according to one embodiment of the present invention is as follows: core-shell fibers are electrospun and deposited on a substrate to form a porous layer (electrospinning step). In the electrospinning step, a nonwoven fabric layer composed of the core-shell fibers is formed as the porous layer.

[0218] (Electrospinning process)

[0219] The electrospinning step can be performed by a known method.

[0220] Reference Figure 2 , an example of the electrospinning process is described.

[0221] Figure 2 This is a schematic diagram showing the configuration of an example of an electrospinning apparatus used for producing a nonwoven fabric layer composed of fibers having a core-sheath structure.

[0222] The electrospinning apparatus of this example includes a needle-shaped nozzle 31, a first syringe pump 32 for supplying a core solution to the nozzle 31, and a second syringe pump 33 for supplying a shell solution to the nozzle 31. The electrospinning apparatus also includes a power supply 34 for applying a voltage to the core solution and the shell solution at the tip of the nozzle 31, and a collecting electrode 35.

[0223] The nozzle 31 is a core-shell coaxial spinneret, comprising an outer cylinder and an inner cylinder coaxially disposed therein. Axially, the position of the inner cylinder's front end is roughly aligned with the position of the outer cylinder's front end. The inner side of the inner cylinder's front end periphery serves as the core solution outlet, while the area between the inner cylinder's front end periphery and the outer cylinder's front end periphery serves as the shell solution outlet. The shell solution outlet annularly surrounds the core solution outlet.

[0224] The inner tube is longer in the axial direction than the outer tube, with its base end protruding toward the outer tube. A first syringe pump 32 is connected to the base end of the inner tube. The operation of this first syringe pump 32 supplies the core solution into the inner tube, which is then discharged from the distal opening (i.e., the core solution outlet). A second syringe pump 33 is connected to the base end of the outer tube. The operation of this second syringe pump 33 supplies the shell solution into the outer tube, which is then extruded from the distal opening (i.e., the shell solution outlet).

[0225] In manufacturing a nonwoven fabric layer using the electrospinning apparatus of this example, a substrate is placed on the collecting electrode 35 , a core solution and a shell solution are supplied to the nozzle 31 , and a voltage is applied.

[0226] When the dispersion force of the core and shell solutions extruded from nozzle 31 exceeds the surface tension, a cone called a Taylor cone forms at the tip of nozzle 31, extending toward collector 35. The elongated solution stream thins as the solvent evaporates, destabilizing the flow and forming a whipping state, expanding from a single, thin stream. Depending on the conditions, the stream further splits. This stream is deposited on the substrate, forming a layer of nonwoven fabric.

[0227] The core solution is a solution in which the core-forming resin is dissolved in a solvent, and the shell solution is a solution in which the shell-forming resin is dissolved in a solvent.

[0228] Preferred embodiments of the core and shell are as described above.

[0229] The resin concentration of the core solution is, for example, 1 to 20% by mass relative to the total mass of the core solution.

[0230] The resin concentration of the shell solution is, for example, 1 to 20% by mass relative to the total mass of the shell solution.

[0231] The solvent of the core solution may be any solvent that dissolves the core-forming resin and may be appropriately selected from various known solvents. The same applies to the solvent of the shell solution.

[0232] Examples of the solvent include protic solvents and aprotic solvents. "Protic solvent" refers to a solvent having proton-donating properties. "Aprotic solvent" refers to a solvent not having proton-donating properties.

[0233] Examples of the protic solvent include the following protic fluorinated solvents.

[0234] Examples of the protic fluorinated solvent include trifluoroethanol, 2,2,3,3,3-pentafluoro-1-propanol, 2-(perfluorobutyl)ethanol, 2-(perfluorohexyl)ethanol, 2-(perfluorooctyl)ethanol, 2-(perfluorodecyl)ethanol, 2-(perfluoro-3-methylbutyl)ethanol, 2,2,3,3-tetrafluoro-1-propanol, 2,2,3,3,4,4,5,5-octafluoro-1-pentanol, 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoro-1-heptanol, and 2,2,3,3,4,4,5,5,6,6,7,7,8,8-hexafluoro-1-nonanol. Fluorinated alcohols such as alcohol, 1,1,1,3,3,3-hexafluoro-2-propanol and 1,3,3,4,4,4-hexafluoro-2-butanol, trifluoroacetic acid, perfluoropropionic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, perfluorononanoic acid, perfluorodecanoic acid, 1,1,2,2-tetrafluoropropionic acid, 1,1,2,2,3,3,4,4-octafluoropentanoic acid, 1,1,2,2,3,3,4,4,5,5-dodecafluoroheptanoic acid and 1,1,2,2,3,3,4,4,5,5,6,6-hexafluorononanoic acid, and fluorinated sulfonic acids such as trifluoromethanesulfonic acid and heptadecafluorooctanesulfonic acid.

[0235] Examples of the aprotic solvent include the following aprotic fluorinated solvents.

[0236] Examples of the aprotic fluorinated solvent include polyfluoro aromatic compounds such as 1,4-bis(trifluoromethyl)benzene, polyfluorotrialkylamine compounds such as perfluorotributylamine, polyfluorocycloalkane compounds such as perfluorodecalin, polyfluorocyclic ether compounds such as perfluoro(2-butyltetrahydrofuran), perfluoropolyethers, polyfluoroalkane compounds, and hydrofluoroethers (HFE).

[0237] These solvents may be used alone or in combination of two or more. In addition to these, a wide range of compounds can also be used.

[0238] The amount of the core solution supplied to the nozzle 31 per unit time (hereinafter also referred to as "the flow rate of the core solution") is preferably 0.1 to 10 mL / hour, more preferably 0.3 to 3 mL / hour.

[0239] The amount of the shell solution supplied to the nozzle 31 per unit time (hereinafter also referred to as "the flow rate of the shell solution") is preferably 0.5 to 15 mL / hour, more preferably 1 to 6 mL / hour.

[0240] The ratio represented by the flow rate of the shell solution / the flow rate of the core solution (hereinafter also referred to as "shell / core flow rate ratio") is preferably 0.5 / 10 to 15 / 0.1, and more preferably 1 / 3 to 6 / 0.3.

[0241] The distance between the tip of the nozzle 31 and the collecting electrode 35 is, for example, 50 to 250 mm.

[0242] The applied voltage is, for example, 5 to 35 kV.

[0243] By appropriately adjusting the resin concentration and flow rate of the core solution, the resin concentration and flow rate of the shell solution, the applied voltage, and the distance between the front end of the nozzle 31 and the collecting electrode 35, the diameter of the fibers constituting the non-woven fabric, the surface roughness and density of the non-woven fabric layer, etc. can be adjusted.

[0244] After the electrospinning step, the laminated body obtained in the electrospinning step, in which the porous layer is laminated on the substrate, can be used to assemble a microfluidic device. In this case, after the electrospinning step and before assembling the microfluidic device, the laminated body can be heated or heat-pressed to improve the uniformity of the porous layer and the adhesion to the substrate.

[0245] After the electrospinning process, the porous layer on the substrate can also be transferred to another substrate (hereinafter also referred to as the "transfer process"), and the microfluidic device can be assembled using the laminate obtained in the transfer process. When the transfer process is performed, the collecting electrode 35 can be used as the substrate in the electrospinning process. When the transfer process is performed, in order to improve the uniformity of the porous layer, the laminate with the porous layer stacked on the substrate before transfer can be heated, or heated and compressed. When the transfer process is performed, after the transfer process and before assembling the microfluidic device, in order to improve the uniformity of the porous layer and the adhesion to the substrate, the laminate can be heated, or the laminate can be heated and pressed.

[0246] The method of assembling a microfluidic device using the laminated body may be the same as that of a known microfluidic device, except that the laminated body is used in at least a part of the components of the microfluidic device.

[0247] Example

[0248] The present invention will be described in more detail below based on Examples and Comparative Examples, but the present invention is not limited to the following Examples unless the gist of the invention is exceeded. Examples 1 to 4 are Examples, and Examples 5 and 6 are Comparative Examples.

[0249] (Measurement method)

[0250] Fiber diameter

[0251] The diameter of the fibers constituting the nonwoven fabric was measured using a laser microscope VK-8710 (manufactured by KEYENCE CORPORATION).

[0252] <Nonwoven fabric thickness>

[0253] The thickness of the nonwoven fabric was measured using a laser microscope VK-8710 (manufactured by KEYENCE CORPORATION).

[0254] Initial water contact angle

[0255] The contact angle of approximately 2 μL of distilled water placed on the nonwoven fabric surface of the laminate (in Examples 5 and 6, the fluororesin layer surface) was measured using a contact angle meter, DropMaster DMo-701SA (manufactured by Kyowa Interface Science Co., Ltd.). Measurements were taken at five different locations on the surface layer, and the average value was calculated as the water contact angle. The contact angle was calculated using the 2θ method.

[0256] <Resistance test to biological test fluids>

[0257] 100 μL of a protein standard substance ("Analytical Standard 200 mg / mL BSA" manufactured by Sigma-Aldrich) placed on the surface of the laminate was left as is for 1 hour. After 1 hour, the protein standard substance was wiped with a dry towel, the surface was washed with distilled water, and the surface was dried with a nitrogen stream. The water contact angle was measured using the method described above for the "initial water contact angle" and used as the water contact angle after the test. It can be confirmed that the closer the water contact angle after the test is to the initial water contact angle (the smaller the change in the water contact angle), the better the resistance to biological test fluids. When the difference between the initial water contact angle and the water contact angle after the test is 56° or less, the resistance to biological test fluids is evaluated as high.

[0258] (Materials used)

[0259] Fluororesin solution-1: a solution of a perfluoro(3-butenyl vinyl ether) cyclopolymer (“CTL-107MK” manufactured by AGC Corporation, solid content: 7% by mass, solvent: “CT-SOLV100E” manufactured by AGC Corporation).

[0260] Fluororesin solution-2: a solution of a perfluoro(3-butenyl vinyl ether) cyclopolymer (“CTL-809M” manufactured by AGC Corporation, solid content: 9% by mass, solvent: “CT-SOLV180” manufactured by AGC Corporation).

[0261] Fluororesin solution-3: a solution of tetrafluoroethylene / perfluoro(2,2-dimethyl-1,3-dioxole) copolymer (“Teflon (registered trademark) AF 1604” manufactured by The Chemours Company, solid content 4% by mass, solvent “FC40” manufactured by 3M Company).

[0262] PCL solution: a solution of polycaprolactone having a number average molecular weight (Mn) of 70,000 to 90,000 (solid content: 10% by mass, solvent: trifluoroethanol).

[0263] (Examples 1 to 4)

[0264] Prepare Figure 2 The electrospinning device has the structure shown.

[0265] A glass substrate is placed on the collecting electrode 35 of the electrospinning device.

[0266] Electrospinning was performed at 29°C and 35% RH, with the types of core and shell solutions, flow rates of the core and shell solutions, distance between the tip of the nozzle 31 and the collecting electrode 35, and electrospinning voltage values ​​as shown in Table 1. This deposited core-shell fibers on a substrate, yielding a laminate comprising a nonwoven fabric layer serving as a porous layer laminated on the substrate. Table 1 shows the diameter of the fibers constituting the nonwoven fabric, the thickness of the nonwoven fabric, and the initial water contact angle of the surface of the nonwoven fabric.

[0267] A resistance test to biological test fluids was conducted on the laminate of Example 4. The water contact angle after the test was 128°.

[0268] [Table 1]

[0269]

[0270] (Example 5)

[0271] Fluororesin Solution 3 was applied to a substrate (glass) using a spin coater at 4000 rpm for 20 seconds and calcined at 330°C for 60 minutes to produce a laminate comprising a non-porous fluororesin layer laminated on the substrate. The initial water contact angle of the fluororesin layer was 121°. Resistance to biological test fluids was also tested. The post-test water contact angle was 64°.

[0272] (Example 6)

[0273] Fluororesin Solution 2 was applied to a substrate (glass) using a spin coater at 4000 rpm for 10 seconds. After pre-drying at 60°C for 10 minutes, the solution was calcined at 190°C for 60 minutes to produce a laminated product comprising a non-porous fluororesin layer laminated on the substrate. The initial water contact angle of the fluororesin layer was 115°. Furthermore, resistance tests to biological test fluids were conducted. The water contact angle after the resistance test was 55°.

[0274] As shown in the above results, the nonwoven fabric-side surfaces of the laminates of Examples 1 to 4 exhibited higher initial water contact angles and superior liquid repellency than the fluororesin layer-side surfaces of the laminates of Examples 5 and 6. Furthermore, the nonwoven fabric-side surfaces of the laminate of Example 4 exhibited superior resistance to biological test fluids compared to the fluororesin layer-side surfaces of the laminates of Examples 5 and 6.

[0275] Industrial applicability

[0276] The microfluidic device of the present invention has excellent liquid repellency and can be used, for example, in biochips (enzyme analysis (examples: glucose and lactate determination), DNA analysis (examples: PCR, high-throughput sequencing), DNA cloning, antibody purification, production and analysis, immunological testing, proteomic analysis), clinical point-of-care diagnosis of diseases, biosensors, cell culture (examples: supply of insulin and penicillin to culture media), drug delivery applications, FDA applications in food safety, microfluidic fuel cells and energy uses, and microfluidic reactors (example: lipid nanoparticle (LNP) synthesis).

[0277] Description of Reference Numerals

[0278] 1…first stack, 2…second stack, 11…first substrate, 12…electrode, 13…first dielectric layer, 21…second substrate, 22…common electrode, 23…second dielectric layer, L…droplet, 31…nozzle, 32…first injection pump, 33…second injection pump, 34…power supply, 35…collecting electrode.

Claims

1. A microfluidic device comprising a laminate comprising a porous layer laminated on a substrate.

2. The microfluidic device according to claim 1, wherein The porous layer is a non-woven fabric layer.

3. The microfluidic device according to claim 2, wherein The non-woven fabric is formed by an electrospinning method.

4. The microfluidic device according to claim 2 or 3, wherein The fibers constituting the nonwoven fabric contain a fluororesin.

5. The microfluidic device according to claim 4, wherein The fibers constituting the nonwoven fabric further contain a non-fluorine resin.

6. The microfluidic device according to claim 2 or 3, wherein The fibers constituting the nonwoven fabric have a core-sheath structure.

7. The microfluidic device according to claim 6, wherein In the core-shell structure, one of the core and the shell contains a fluorine resin, and the other contains a non-fluorine resin.

8. The microfluidic device according to claim 4, wherein The fluororesin is an amorphous fluororesin.

9. The microfluidic device according to claim 4, wherein The fluororesin includes a polymer having a unit having a fluorinated aliphatic ring structure constituting a main chain.

10. The microfluidic device according to claim 9, wherein The unit having a fluorinated aliphatic ring structure constituting the main chain is at least one selected from the group consisting of a unit formed by cyclopolymerization of a diene fluorinated monomer and a unit based on a cyclic fluorinated monomer.

11. The microfluidic device according to claim 5, wherein The non-fluorine resin is a crystalline non-fluorine resin.

12. The microfluidic device according to claim 5, wherein The non-fluorine resin is at least one selected from the group consisting of polycaprolactone, polyethylene glycol, polyvinyl alcohol, polyacrylonitrile, polyaniline, acrylic resin, polyurethane, polystyrene, polycarbonate, polyvinyl pyrrolidone, chitosan, gelatin, and cellulose acetate. 13 . The microfluidic device according to claim 1 , which is a biochip.

14. A method for manufacturing a microfluidic device, wherein: Fibers having a core-shell structure are spun by electrospinning and deposited on a substrate to form a porous layer.

15. The manufacturing method according to claim 14, wherein: In the core-shell structure, one of the core and the shell contains a fluorine resin, and the other contains a non-fluorine resin.

16. The manufacturing method according to claim 15, wherein: The fluororesin is an amorphous fluororesin.

17. The manufacturing method according to claim 15 or 16, wherein: The fluororesin includes a polymer having a unit having a fluorinated aliphatic ring structure constituting a main chain.

18. The manufacturing method according to claim 17, wherein: The unit having a fluorinated aliphatic ring structure constituting the main chain is at least one selected from the group consisting of a unit formed by cyclopolymerization of a diene fluorinated monomer and a unit based on a cyclic fluorinated monomer.

19. The manufacturing method according to claim 15 or 16, wherein: The non-fluorine resin is a crystalline non-fluorine resin.

20. The manufacturing method according to claim 15 or 16, wherein: The non-fluorine resin is at least one selected from the group consisting of polycaprolactone, polyethylene glycol, polyvinyl alcohol, polyacrylonitrile, polyaniline, acrylic resin, polyurethane, polystyrene, polycarbonate, polyvinyl pyrrolidone, chitosan, gelatin, and cellulose acetate.

Citation Information

Patent Citations

  • Device and method for analyzing samples

    JP2022020665A

  • Image blur correction device, method for controlling the same, program, and storage medium

    JP2023026913A