In-situ monitoring method for fatigue damage of cord thread / rubber composite material interface

By introducing a carbon nanotube conductive network at the interface of the cord/rubber composite material, the problems of complex and costly monitoring in the prior art are solved, achieving efficient and convenient interface fatigue damage monitoring while maintaining interface adhesion performance.

CN121068706APending Publication Date: 2025-12-05CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511442720.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-10
Publication Date
2025-12-05

AI Technical Summary

Technical Problem

Existing technologies are insufficient for effectively monitoring fatigue damage at the interface of cord/rubber composite materials, especially since sensor solutions are complex, costly, and may affect interfacial adhesion performance.

Method used

By introducing a carbon nanotube dispersion onto the surface of the cord and performing ultrasonic swelling treatment to form a conductive network, and then combining it with rubber for resistance response monitoring, the conductive network is directly constructed within the interface layer, avoiding the need for additional sensors.

Benefits of technology

It enables efficient, convenient, and non-destructive monitoring of the cord/rubber interface, maintains the interface adhesion performance, reduces monitoring costs, and improves accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the field of material detection, in particular to an in-situ monitoring method for fatigue damage of a cord thread / rubber composite material interface. The method comprises the following steps: carrying out ultrasonic swelling treatment on a cord thread coated with an RFL coating by using a carbon nanotube dispersion liquid, and then preparing an H extraction sample with rubber; and then connecting a circuit, fixing the obtained H extraction sample on an electronic fatigue testing machine, forming a closed loop circuit between the H extraction sample and the source meter, carrying out fatigue testing and measuring contact resistance, and carrying out resistance signal processing to obtain a resistance change rate deltaR / R0. The method provided by the invention is efficient and convenient, and the interface fatigue damage of the cord thread / rubber composite material can be visually and effectively monitored.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the field of material detection, in particular to a cord / rubber composite material interface fatigue damage in-situ monitoring method. BACKGROUND

[0002] As the main load-bearing material of products such as tires and air springs, cord / rubber composite materials need to withstand periodic loads, and the expected fatigue life has a huge impact on the safety performance and economic benefits of products. The adhesion of common synthetic cords (such as nylon, aramid, etc.) and general rubber materials is usually poor due to differences in polarity, modulus, etc. The industry usually uses a resorcinol-formaldehyde-latex (RFL) impregnation system to treat the surface of the cord. The main components in RFL can produce strong hydrogen bond interactions with the surface of common cords, and at the same time, co-vulcanization and mechanical interlocking structures with the rubber matrix, and the modulus between the two can play a transitional role. This undoubtedly greatly enhances the adhesion between the cord and the rubber. Studies have shown that the fatigue process of such composite materials usually goes through the following three stages: first, microcracks are initiated at the interface between the cord and the rubber; then in the second stage, as the fatigue level deepens, the cracks gradually develop; finally, in the third stage, the cracks form through the rubber material, and the mechanical properties drop sharply, leading to the failure of the material. Therefore, the damage of the adhesion interface between the cord and the rubber is crucial to the fatigue life of the composite material, and the identification and monitoring of the interface damage are of great significance to the study of the fatigue behavior of cord / rubber composite materials, and are key technologies for developing the next generation of cord / rubber composite materials with "self-diagnosis" and "self-sensing" functions.

[0003] For the identification and monitoring of composite material damage, there are usually two evaluation strategies: destructive and non-destructive. However, in practical applications, the safety performance of the product itself is far superior to the monitoring itself. Therefore, the application prospect of non-destructive methods is more promising.

[0004] Among the widely used non-destructive detection schemes, X-ray and ultrasonic monitoring technologies are difficult to carry out real-time testing under dynamic conditions due to various conditions. X-ray monitoring technology requires placing the tire in a specific light source under static or quasi-static conditions. Since the light source intensity often cannot meet the requirements of synchrotron radiation level, it usually needs several minutes of scanning test and imaging analysis, which is far from real-time monitoring standards. Ultrasonic detection technology needs to overcome huge noise interference in dynamic testing. In addition, there are also defects such as laborious and time-consuming, high cost, poor effect, long inspection period, and blind spots.

[0005] The sensor based on piezoelectric effect has been widely used due to its high sensitivity. When the transmitter converts the signal, the sensor compares the received signal with the reference signal. If there is damage or failure, it will change the inherent frequency and phase of the structure, and the sensor will send an alarm. Another Fiber Bragg Grating (FBG) technology based on the periodic refractive index of the fiber core. The sensor can reflect a specific wavelength of light. When the external strain changes, the accuracy of the strain can be accurately calculated by measuring the wavelength shift, and the position sensing accuracy is as high as 2 nm. At the same time, the two schemes can also form an array composite to improve the detection accuracy and simplify. However, the two schemes require additional equipment and corresponding data channel sets, and the wiring and data processing, the complexity of the structure will also increase significantly with the increase of the number of component devices.

[0006] The technology of using the resistance response of continuous conductive composites as a health monitoring signal also has a certain influence. However, this structure health monitoring scheme based on electrical response has a narrow application range and is initially only applied to intrinsically conductive composites. With the development of research and the in-depth study of conductive doped particles such as graphene and carbon nanotubes (CNT), it has gradually developed. However, the above method still has some problems and difficulties for cord / rubber composites:

[0007] The application in intrinsically conductive materials, such as using the electrical response of carbon fibers themselves to monitor the internal damage state of continuous carbon fiber reinforced materials. But through the resistance characteristic change of conductive fibers themselves, the damage form that can be monitored can only be fiber breakage. In cord / rubber composites, the modulus of the skeleton fiber is much higher than that of the rubber matrix, which is not easy to cause fatigue damage, but the low modulus matrix and the interface where the crack source is easily formed cannot be effectively characterized.

[0008] CNT, as a carbon fiber allotrope, also has excellent electrical conductivity and large specific surface area. Only a small amount of CNT needs to be dispersed uniformly in the insulating composite to obtain ideal electrical conductivity. It is also because of this that in various attempts in insulating materials, the method of using CNT to construct a conductive network has the most remarkable effect.

[0009] Firstly, the research idea of adding conductive particles to build a conductive network in the matrix. By adding CNTs to the insulating polymer matrix to make the composite matrix partially conductive, various damage forms dominated by the matrix can be monitored by measuring the contact resistance and other methods. Among them, the representative work comes from Chou et al. They added 0.5wt.% of CNTs to the matrix of glass fiber reinforced epoxy resin composites (GFRPs) by three-roll calendering process, and then evaluated the damage evolution process in the composite by measuring the resistance characteristics of the orthotropic laminated composite under tensile loading in real time, successfully analyzing the resistance response of damage behaviors such as interlaminar separation, transverse crack propagation and fiber fracture. Subsequently, a large number of research works focus on the resistance response of composites under different loading forms, such as quasi-static loading, impact loading, cyclic loading, etc. In fact, the monitoring method of building a conductive network by adding CNTs to the matrix cannot effectively monitor the damage of the interface region between the skeleton fiber and the matrix. The weak response signal in this part will be diluted by the matrix with higher volume ratio. Therefore, in the research of the interface damage mechanism of the cord and rubber, this is not a suitable solution.

[0010] Another research approach is to modify the surface of the insulating fiber. By coating CNT on the surface of the insulating fiber to prepare self-sensing fiber, the composite interface can be given partial conductivity, thus effectively overcoming the limitations of the first method and realizing the monitoring of the deformation and damage behavior of the interface region. Mader et al. first proposed a CNT dispersion process based on a water-based solution, and coated the prepared CNT-containing slurry on the surface of glass fiber (GF). By controlling the CNT content on the surface of GF, the initial resistance of the interface conductive network and the sensitivity of the resistance response under mechanical loading were optimized, and finally the micro-damage of the interface region before GF fracture failure was successfully monitored in the quasi-static tensile and cyclic loading test. Bilotti et al. prepared thermoplastic polyurethane / CNT (TPU / CNT) composite fibers with high conductivity through a continuous extrusion process. Further, they coated a TPU / CNT conductive composite coating on the surface of commercial spandex yarns to verify the feasibility of self-sensing yarns. In order to prepare a CNT conductive network on the surface of insulating fibers, various coating preparation processes have been involved, including electrophoretic deposition (EPD), chemical vapor deposition (CVD), electro-spraying and spraying processes. For example, He et al. prepared a directional arrangement of CNT coating on the surface of GF by CVD process and applied it in the in-situ damage monitoring of GFRPs under bending loading; Zhang et al. used a simple spraying process to coat CNT on the CF preform, and found that the resistance response of the composite material has a strong correlation with the crack propagation process during in-situ damage monitoring. However, the defect of the above method is that the added conductive particle layer between the fiber and the matrix will affect the original interface components. Therefore, the research is mainly based on epoxy resin and polyurethane matrix materials with liquid prepolymer, so as to have better wettability with the conductive particle layer. However, the flowability and processability of rubber are worse and more complex than the first two kinds of matrix. The stability of the composite system in the cord / rubber composite material is more dependent on the adhesion strength of the RFL layer of the interface, and once damaged, it will cause serious safety hazards. Therefore, this method has great disadvantages for cord / rubber composite materials.

[0011] Both of the two methods mentioned above have certain difficulties in the construction of CNT conductive network in the cord / rubber composite: if the method of adding CNT to the rubber matrix is adopted, the high viscosity of the rubber matrix is not conducive to the uniform dispersion of CNT; if the method of directly modifying the surface of the cord with a CNT layer is adopted, the adhesion between the commercial cord and the rubber will be damaged. In 2014, Coleman et al. first proposed a swelling process, in which a rubber bracelet was immersed in a graphene organic solvent dispersion, and the rubber bracelet absorbed graphene during the swelling process, thereby preparing a graphene / rubber bracelet with high dispersibility and excellent conductivity and successfully applying it to the field of wearable smart devices. After that, Busfield et al. first used the swelling process to successfully prepare a CNT conductive network on the surface of a GF cord coated with chlorosulfonated polyethylene (CSM). They used three different organic solvents to prepare CNT dispersions, including methylpyrrolidone (NMP), dimethylformamide (DMF), and acetone (Acetone), all of which achieved uniform distribution of CNTs inside the RFL coating layer on the surface of the cord. In their research, the conductive network constructed by CNTs was swelled into the CSM layer with strong polarity, which existed as an internal component of the impregnated layer that played a role in adhesion between the skeleton cord and the rubber interface layer. However, it is obvious that the base rubber and the interface impregnated layer used by them are both strong polar specific material combinations to ensure compatibility matching. This obviously cannot be applied to the commonly used strong polar synthetic cord / non-polar rubber system. At the same time, this also changes the original composition of the interface layer, and may even affect the original fatigue failure mechanism.

[0012] In summary, the main defects of strain sensor technology are multiple components, complex system, and high cost. A large number of sensor response / receiving devices need to be laid inside and outside the product. Whether the strain sensor is based on piezoelectric materials or optical fiber arrays, the essence is to convert the strain signal into an optical, electrical, magnetic, or thermal signal that can be detected by an instrument. The additional integrated sensing device is a very complex and costly burden. In products such as tires, which have limited space, this undoubtedly greatly increases the use restrictions. In addition, the number of external sensors is often limited and occupies a certain space volume, and each sensor can cover a limited effective monitoring site. That is, the actual precision of the sensor and the size of the blind spot area are highly related to the density of the sensor layout. In addition, the current external sensor solution converts the macro force signal reflecting the fatigue information into a signal that can be detected by an external sensor and then fed back. In theory, after several layers of signal relay transmission, the fatigue information reflected will be distorted to varying degrees, which is not conducive to precise quantitative analysis for life prediction.

[0013] In the envisaged scheme of constructing carbon nanotube conductive network for health monitoring based on resistance response, the introduction of CNT is a more difficult problem. The plating scheme often needs to spend a high cost. And only relying on this kind of surface plating means, usually only the CNT conductive layer is formed on the surface and cannot penetrate into the material inside. This will cause great loss of the mechanical properties of the bonded part, and has an immeasurable impact on the safety performance. Although the work of Busfield et al. mentioned in the foregoing does not have the obvious defects of the techniques in the foregoing, the fixed combination of CSM and HNBR not only requires the additional introduction of a layer of CSM shell on the surface of the cord, but also limits the use of the rubber matrix. At the same time, this also destroys the original interface components, which all increase the limitations. SUMMARY

[0014] Therefore, the present application provides a cord / rubber composite interface fatigue damage in-situ monitoring method. The method provided by the present application is efficient and convenient, and can intuitively and effectively monitor the interface fatigue damage of the cord / rubber composite.

[0015] The present application provides a cord / rubber composite interface fatigue damage in-situ monitoring method, comprising the following steps:

[0016] S1, preparing a conductive cord:

[0017] (S1a): adding carbon nanotubes to a solvent and performing ultrasonic dispersion treatment to obtain a carbon nanotube dispersion liquid;

[0018] (S1b): immersing the cord in the carbon nanotube dispersion liquid obtained in step (S1a) and performing ultrasonic swelling treatment to obtain a conductive cord;

[0019] The cord includes a cord body and an RFL coating layer combined on the surface of the cord body.

[0020] S2, preparing a cord / rubber composite sample:

[0021] An H extraction sample is prepared from the conductive cord obtained in step S1 and a rubber strip;

[0022] S3, resistance response in-situ monitoring test:

[0023] (S3a): fixing a monitoring circuit

[0024] The H extraction sample obtained in step S2 is fixed on an electronic fatigue testing machine, and the remaining conductive cords at both ends of the H extraction sample are connected to conductive wires, and then the two conductive wires connected are connected to a source table, so that a closed loop circuit is formed between the H extraction sample and the source table.

[0025] (S3b): performing fatigue test and measuring contact resistance

[0026] Opening the source table, loading voltage V, and recording real-time current changes under certain frequency conditions, obtaining real-time resistance R through the ratio of voltage V / current I; the above-mentioned resistance determination process is accompanied by a fatigue test; (S3c): resistance signal processing

[0027] Taking the initial stable resistance in (S3b) as the initial resistance R0, and taking the difference between the subsequent resistance and the initial resistance R0 divided by the initial resistance R0 as the resistance change rate ΔR / R0, which reflects the interface fatigue.

[0028] Preferably, in step (S1a), the carbon nanotubes are multi-walled carbon nanotubes; the length of the multi-walled carbon nanotubes is 0.5-50 μm, and the diameter is 4-50 nm.

[0029] Preferably, in step (S1a), the ultrasonic dispersion conditions are: power 500-3000 W, effective ultrasonic time 10-60 min, and pause every certain period of time.

[0030] Preferably, in step (S1b):

[0031] The ultrasonic swelling treatment conditions are: power 500-3000 W, effective ultrasonic time 10-60 min, and pause every certain period of time;

[0032] The cord body is a nylon cord, an aramid cord, or a polyester fiber cord.

[0033] Preferably, step (S2) comprises:

[0034] (S2a): placing the rubber strip and the conductive cord obtained in step S1 in a vulcanization mold;

[0035] (S2b): placing the vulcanization mold on a vulcanization machine for vulcanization to obtain an H-extraction sample.

[0036] Preferably, in step (S3a), the H-extraction sample obtained in step S2 is fixed on the upper and lower clamps of an electronic fatigue testing machine; the upper and lower clamps are pre-treated for insulation.

[0037] Preferably, in step (S3a):

[0038] The conductive metal wire is a copper wire;

[0039] The connection mode is winding;

[0040] The conductive glue is used to fix the connection between the conductive metal wire and the conductive cord.

[0041] Preferably, in step (S3b), the voltage is 1.0 V, and the certain frequency is 1-10 Hz.

[0042] Preferably, in step (S3b):

[0043] The fatigue parameters include: cyclic load, loading waveform and frequency;

[0044] The minimum load is 1N and the maximum load is 48~94N;

[0045] The loading waveform is a sine wave;

[0046] The frequency is preferably 0.05~10Hz.

[0047] Preferably, in step (S1a):

[0048] The solvent is at least one of DMF, NMP, acetone and toluene;

[0049] In the ultrasonic dispersion treatment, it is paused for 5~10min every 3~5min;

[0050] The concentration of carbon nanotubes in the obtained carbon nanotube dispersion is 0.05~5g / L;

[0051] In step (S1b):

[0052] The thickness of the RFL coating is 10~100μm;

[0053] In the ultrasonic swelling treatment, it is paused for 5~10min every 3~5min;

[0054] After the ultrasonic swelling treatment, it is also washed and dried.

[0055] In the prior art, the monitoring scheme of the interface area damage in-situ monitoring quantification and excellent adhesion performance of the cord / rubber composite material fatigue evolution cannot be compatible. In view of this, the present application provides a cord / rubber composite material interface fatigue damage in-situ monitoring method, which is a high-efficiency and convenient nondestructive testing method. The cord coated with RFL coating is subjected to ultrasonic swelling treatment by using carbon nanotube dispersion liquid, and then the H extraction sample is made with rubber. Then the circuit is connected, the obtained H extraction sample is fixed on the electronic fatigue testing machine, and the H extraction sample and the source table form a closed loop circuit, the fatigue test and the contact resistance are measured, and the resistance signal processing is carried out to obtain the resistance change rate ΔR / R0. In one aspect, the conductive network is constructed in the RFL impregnated layer of the interface between the cord and the rubber, which is changed into a simple resistance response sensor, which can not only solve the problem of limited actual monitoring site of the external photoelectric sensor, but also solve the problem of fatigue signal transmission distortion, and the electrical signal is directly related to the fatigue condition of the interface. On the other hand, the conductive particles are introduced into the RFL layer by ultrasonic swelling process, which not only has simple process and low cost, but also can greatly retain the adhesion strength of the two. In summary, the RFL coating in the cord and rubber composite material is taken as the target area, CNT is introduced into the interface layer which plays the role of adhesion to form a conductive network. The electrical signal under this response can not only directly associate with the stress change of the interface area, but also can reflect the damage condition. The above-mentioned means can not only effectively overcome the problem that CNT is difficult to anchor and disperse in the interface area, but also does not change the composition of the original macroscopic interface layer, and at the same time ensures the original composite material combination, so that the introduced conductive network penetrates into the RFL layer, which greatly reduces the loss of adhesion performance. BRIEF DESCRIPTION OF DRAWINGS

[0056] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the following will briefly introduce the drawings needed to be used in the embodiments or the prior art description. Obviously, the drawings in the following description are only embodiments of the present application, and for those skilled in the art, other drawings can also be obtained without creative labor on the basis of the provided drawings.

[0057] Fig. 1 is a schematic view of the vulcanizing mold in the present application, wherein, Figure 1a is a structural schematic view of the bottom mold, Figure 1b is a structural schematic view of the middle mold, Figure 1c is a structural schematic view of the top mold;

[0058] Figure 2 is a structural schematic view of the H extraction sample prepared in the present application;

[0059] Figure 3 is a schematic view of the clamp of the electronic fatigue testing machine; wherein, Figure 3 (a) is a left view,Figure 3 (b) is a plan view, Figure 3 (c) is a front view;

[0060] Figure 4 is a schematic diagram of the connection between the H-extraction sample and the source table in the present application;

[0061] Figure 5 is a test effect diagram of the resistance response in-situ monitoring of Example 1 of the present application; wherein, Figure 5 (a)-(d) are the result diagrams under the conditions of frequencies 1 Hz, 2 Hz, 0.05 Hz and 0.1 Hz, respectively;

[0062] Figure 6 is a test effect diagram of the resistance response in-situ monitoring of Example 2 of the present application; wherein, Figure 6 (a) is a result diagram of 640 cycles under the conditions of 1 Hz and 1-94 N, Figure 6 (b) is a result diagram of 200-220 cycles in (a), Figure 6 (a) is a result diagram of 200-220 cycles in (a), Figure 6 (c) is a result diagram of 14800 cycles under the conditions of 1 Hz and 1-48 N, Figure 6 (d) is a result diagram of 5000-5014 cycles in (c), Figure 6 (c) is a result diagram of 5000-5014 cycles in (c);

[0063] Figure 7 is a test effect diagram of the resistance response in-situ monitoring of Example 3 of the present application; wherein, Figure 7 (a) is a result diagram under the conditions of 1 Hz and 1-80 N, Figure 7 (b) is a result diagram under the conditions of 1 Hz and 1-84 N;

[0064] Fig. 8(a)-(f) are effect comparison diagrams of the prior art and the present application; wherein, Fig. 8(a) is a cycle tensile resistance response effect diagram of a single glass fiber and an epoxy resin composite material after introducing a CNT layer by a deposition method; Fig. 8(b) is a cycle tensile test effect diagram of a carbon fiber reinforced epoxy resin; Fig. 8(c-d) are a carbon nanotube woven yarn and a polydimethylsiloxane composite material sample diagram and a tensile test effect diagram; Fig. 8(e) is a dynamic and static test response effect diagram of a chlorosulfonated polyethylene (CSM) layer introduced with CNT outside a glass fiber and a hydrogenated nitrile rubber (HNBR) composite material, wherein, Fig. 8(e1)-(e2) are displacement control response diagrams of pulse waveforms, and Fig. 8(e3) is an electrical response diagram of static extraction; Fig. 8(f) is a part of the test effect diagram of the present application. DETAILED DESCRIPTION

[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used in the description herein is for describing particular embodiments only and is not intended to be limiting of the application.

[0066] In the description herein, the technical features described in an open way include both the closed technical solution consisting of the listed features and the open technical solution comprising the listed features.

[0067] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0068] In the description herein, with respect to a numerical interval, unless otherwise specified, the numerical interval is considered to be continuous and includes the minimum value and the maximum value of the range and every value between such minimum value and maximum value. Further, when the range refers to integers, every integer between the minimum value and the maximum value of the range is included. In addition, when multiple ranges are provided to describe a feature or a characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein are to be understood as including any and all sub-ranges subsumed therein.

[0069] In the description herein, with respect to a data range, if only the unit is provided after the right end point, it means that the units of the left end point and the right end point are the same. For example, 500~3000W means that the units of the left end point "500" and the right end point "3000" are both W.

[0070] The application provides a method for monitoring fatigue damage in situ at a cord / rubber composite material interface, comprising the following steps:

[0071] S1, preparing a conductive cord:

[0072] (S1a): adding carbon nanotubes to a solvent and performing ultrasonic dispersion treatment to obtain a carbon nanotube dispersion liquid;

[0073] (S1b): immersing the cord in the carbon nanotube dispersion liquid obtained in step (S1a) and performing ultrasonic swelling treatment to obtain a conductive cord;

[0074] The cord comprises a cord body and an RFL coating layer combined on the surface of the cord body.

[0075] S2, preparing a cord / rubber composite material sample:

[0076] An H extraction sample is prepared from the rubber strip and the conductive cord obtained in step S1;

[0077] S3, resistance response in-situ monitoring test:

[0078] (S3a): Fixed monitoring circuit

[0079] The H-extraction sample obtained in step S2 is fixed on the electronic fatigue testing machine, and the remaining conductive cords at both ends of the H-extraction sample are connected to conductive metal wires respectively. Then, the two connected conductive metal wires are connected to the source meter to form a closed loop circuit between the H-extraction sample and the source meter.

[0080] (S3b): Perform fatigue testing and measure contact resistance.

[0081] Open the source meter, apply voltage V, and record the real-time current change under certain frequency conditions. Obtain the real-time resistance R by the ratio of voltage V / current I; fatigue testing is carried out during the above resistance measurement process; (S3c): Resistance signal processing

[0082] Using the initial stable resistance in (S3b) as the initial resistance R0, the difference between the subsequent resistance and the initial resistance R0 is divided by the ratio of the initial resistance R0 to obtain the resistance change rate ΔR / R0, thereby reflecting interface fatigue.

[0083] The method provided by this invention uses a simple immersion and swelling process to introduce carbon nanotubes (CNTs) into the RFL interface layer of a rubber / cord composite material. This forms a continuous conductive network in the interface region that can be used for fatigue response without damaging the interfacial adhesion. This invention transforms the interface itself into a "self-inductive" resistance response sensor, enabling in-situ monitoring of the entire fatigue cycle evolution signal without adding extra components, ensuring portability while maintaining monitoring accuracy and user experience. In other words, this invention introduces a conductive network at the adhesive interface between the cord and rubber, directly converting fatigue damage into a readily monitorable electrical signal. Therefore, by introducing a self-inductive conductive network into the interface region, it provides a means to achieve in-situ monitoring of damage in the cord / rubber interface region during fatigue loading.

[0084] Regarding step S1 :

[0085] In this invention, step S1 includes two steps, S1a and S1b, as follows:

[0086] Regarding step (S1a):

[0087] (S1a): Carbon nanotubes are added to the solvent and ultrasonically dispersed to obtain a carbon nanotube dispersion.

[0088] In this invention, the carbon nanotubes are preferably multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes is preferably 0.5~50 μm, and the diameter is preferably 4~50 nm. In some embodiments of this invention, the diameter of the multi-walled carbon nanotubes is 4~6 nm, and the length is 0.5~2 μm.

[0089] In this invention, the solvent is preferably at least one of DMF, NMP, acetone and toluene. Using the above solvents to match the solubility parameters of carbon nanotubes is beneficial to the dispersion of carbon nanotubes.

[0090] In this invention, ultrasonic treatment is performed until no obvious clusters of particles are present in the solvent and no sedimentation occurs after a short period of settling. The preferred conditions for ultrasonic dispersion are: power 500-3000W, effective ultrasonic time 10-60 minutes, with pauses at intervals. Specifically, the power can be 500W, 1000W, 1500W, 2000W, 2500W, or 3000W. The effective ultrasonic time can be 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, or 60 minutes. The preferred intervals are 3-5 minutes, specifically 3 minutes, 4 minutes, or 5 minutes. The preferred pause times are 5-10 minutes, specifically 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, or 10 minutes. During the ultrasonic dispersion process, the process is paused periodically for heat dissipation to prevent excessive temperature and rapid solvent evaporation. The effective ultrasonic time is the actual ultrasonic time minus the pause times.

[0091] In this invention, the concentration of carbon nanotubes in the obtained carbon nanotube dispersion is preferably 0.05~5 g / L, specifically 0.05 g / L, 0.1 g / L, 0.5 g / L, 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L, or 5 g / L.

[0092] Regarding step (S1b):

[0093] (S1b): The cord is immersed in the carbon nanotube dispersion obtained in step (S1a) and subjected to ultrasonic swelling treatment to obtain conductive cord.

[0094] In this invention, the cord comprises a cord body and an RFL coating laminated to the surface of the cord body. The source of the cord is not particularly limited; it can be a commercially available product. The thickness of the RFL coating is preferably 10-100 μm, specifically 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm, more preferably 20 μm. In this invention, the cord body is preferably nylon cord, aramid cord, or polyester fiber cord.

[0095] In this invention, the preferred conditions for the ultrasonic swelling treatment are: power 500~3000W, effective ultrasonic time 5~60min, with pauses at intervals. Specifically, the power can be 500W, 1000W, 1500W, 2000W, 2500W, or 3000W. The effective ultrasonic time can be 5min, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min, or 60min. The preferred intervals are 3~5min, specifically 3min, 4min, or 5min. The preferred pause times are 5~10min, specifically 5min, 6min, 7min, 8min, 9min, or 10min. During the ultrasonic dispersion treatment, the process is paused periodically for heat dissipation to prevent excessive temperature and rapid solvent evaporation. Similarly, the effective ultrasonic time is the actual ultrasonic time minus the pause times.

[0096] In this invention, after the above-mentioned ultrasonic swelling treatment, it is preferable to further perform cleaning and drying. The cleaning includes immersing the ultrasonically swollen cord in an organic solvent for ultrasonic cleaning. The organic solvent is preferably at least one of anhydrous ethanol and acetone. The ultrasonic cleaning is performed using an ultrasonic disperser. The preferred conditions for the ultrasonic cleaning are: power 150~400W, time 20~60s. Specifically, the power can be 150W, 200W, 250W, 300W, 350W, or 400W. The specific time can be 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, or 60s. After the ultrasonic cleaning, drying is performed. The preferred drying temperature is 50~100℃, specifically 50℃, 60℃, 70℃, 80℃, 90℃, or 100℃. The drying time is preferably 10-48 hours, specifically 10 hours, 14 hours, 18 hours, 22 hours, 26 hours, 30 hours, 34 hours, 38 hours, 42 hours, 46 hours, or 48 hours. After drying, conductive cord is obtained.

[0097] Regarding step S2 :

[0098] S2. Preparation of cord / rubber composite material sample: The rubber strip and the conductive cord obtained in step S1 are used to make H-extraction sample.

[0099] In this invention, the rubber strip can be prepared by the following method: the raw material is mixed, milled, cut, thinned and sheeted to obtain a mixed rubber; the mixed rubber is cut to obtain a rubber strip.

[0100] In this invention, the raw material formulation of the rubber strip is not particularly limited, and this invention can be used to test rubber compounds with various formulations. In this invention, the rubber matrix of the rubber strip is preferably isoprene rubber. In some embodiments of this invention, the raw materials for preparing the rubber strip include: 100 parts isoprene rubber, 50 parts precipitated silica, 3.0 parts nano zinc oxide, 2.0 parts stearic acid, 1.0 part antioxidant, 2.5 parts sulfur, 1.0 part vulcanization accelerator, and 0.2 parts co-vulcanizing agent.

[0101] In this invention, the preparation of an H-pull sample from the rubber strip and the conductive cord obtained in step S1 refers to the preparation of a specimen for the H-pull test from the rubber strip and the conductive cord obtained in step S1. The H-pull test originates from GB / T 2942-2009 "Determination of Static Adhesion Strength of Vulcanized Rubber and Fiber Cord - H-Pull Method". This national standard specifies the method for determining the shear force value at the cord-rubber interface. The sample prepared by the method described in the standard resembles the letter "H", hence the name H-pull test. In this invention, the rubber strip and the conductive cord are used to prepare the specimen structure for the aforementioned H-pull test.

[0102] In this invention, the H extraction sample can be obtained by the following method: (S2a): placing the rubber strip and the conductive cord obtained in step S1 in a vulcanization mold; (S2b): placing the vulcanization mold on a vulcanizing machine for vulcanization to obtain the H extraction sample.

[0103] Regarding step (S2a):

[0104] The vulcanizing mold is a specially made vulcanizing mold, specifically a vulcanizing mold matched to the specimen used in the H extraction test. The structure of the specially made vulcanizing mold is shown in Figure 1, wherein... Figure 1a This is a structural diagram of the bottom mold (where 1 is the rubber groove, 2 is the intended position for the cord placement, 7 is the cord groove, 4 is the cord fixing buckle, 5 is the mold handle, and 6 is the threaded screw hole). Figure 1b This is a structural diagram of the middle mold (where 1 is a hollow screw groove without threads, 2 is a rubber groove, and the middle mold is fixed to the bottom mold by three screws). Figure 1c This is a schematic diagram of the top mold structure (the round hole is a hollow screw riser, and the top mold is directly attached to the middle mold).

[0105] The process of placing the rubber strips and the conductive cords obtained in step S1 into the vulcanizing mold includes: taking four rubber strips and stacking them in pairs in the bottom mold cavity of the vulcanizing mold; laying eight conductive cords on the rubber strips; passing one end of each conductive cord through a wire groove and fixing it with a bolt, and passing the other end through the wire groove and suspending a weight; placing the middle mold on the bottom mold and fixing it with bolts; then placing two more rubber strips in the middle mold cavity; and finally placing the top mold on the middle mold. At this point, the raw materials are assembled in the mold. The number of rubber strips and the number of cords can be adjusted accordingly.

[0106] Regarding step (S2b):

[0107] After the raw materials and mold are assembled in step (S2a), they are placed on a vulcanizing machine for vulcanization. The vulcanizing agent is preferably a flat vulcanizing machine. The vulcanization conditions are not particularly limited and are selected based on the suitability of the rubber formulation. Preferably, the vulcanization conditions are as follows: vulcanization temperature 140~160℃, vulcanization pressure 45~50t, and vulcanization time 30~120min. The vulcanization temperature can specifically be 140℃, 141℃, 142℃, 143℃, 144℃, 145℃, 146℃, 147℃, 148℃, 149℃, or 150℃, more preferably 145℃; the vulcanization pressure can specifically be 45t, 46t, 47t, 48t, 49t, or 50t, more preferably 50t; the vulcanization time can specifically be 30min, 40min, 50min, 60min, 65min, 70min, 80min, 90min, 100min, 110min, or 120min, more preferably 65min.

[0108] After vulcanization, a corresponding number of H-type samples are cut based on the cord data. For example, if 8 cords are laid, a total of 8 H-type samples of a single cord / rubber composite material are cut. The structure of the resulting H-type sample is as follows: Figure 2 As shown, 1 is the cord and 2 is the rubber.

[0109] Regarding step S3 :

[0110] In this invention, step S3 includes steps S3a to S3d, as follows:

[0111] Regarding step (S3a):

[0112] (S3a) Fix the monitoring circuit: Fix the H-extraction sample obtained in step S2 on the electronic fatigue testing machine, and connect the remaining conductive cords at both ends of the H-extraction sample to conductive metal wires respectively. Then connect the two connected conductive metal wires to the source meter to form a closed loop circuit between the H-extraction sample and the source meter.

[0113] In this invention, the H-extraction sample obtained in step S2 is fixed on the electronic fatigue testing machine, specifically by fixing the H-extraction sample on the upper and lower clamps of the electronic fatigue testing machine. The structure of the clamps is as follows: Figure 3 As shown, where, Figure 3 (a) is the left view. Figure 3 (b) is a top view. Figure 3(c) Main view; where 1 is the cord groove, 2 is the flange ring screw hole, and 3 is the rubber clamping groove; wherein, the flange ring is the part connected to the electronic fatigue testing machine, and the upper end is a smooth metal groove with a single-sided hollow in the middle, which can clamp the rubber part of the composite material sample while exposing the cord part. In this invention, the upper and lower clamps of the electronic fatigue testing machine are preferably pre-insulated to prevent the formation of a conductive path between the sample extracted in step S2 and the electronic fatigue testing machine.

[0114] In this invention, the conductive strands remaining at both ends of the sample extracted from H are respectively connected to conductive metal wires, i.e., as shown in the figure. Figure 4 The H-shaped sample is shown, with each end of the remaining cord connected to a section of conductive metal wire. Preferably, the conductive metal wire is copper wire. The connection method is preferably winding. In this invention, preferably, conductive adhesive is used to fix the connection between the conductive metal wire and the conductive cord, i.e., the position of the metal wire is fixed by the conductive adhesive. The conductive adhesive is preferably conductive graphite adhesive or conductive silver adhesive. Then, the two connected sections of conductive metal wire are connected to the source meter, forming a closed-loop circuit between the H-shaped sample and the source meter. Figure 4 As shown, 1 is conductive adhesive, 2 is conductive metal wire, 3 is source surface, 4 is cord, and 5 is rubber.

[0115] There are no special restrictions on the order of fixing the H-extracted sample obtained in step S2 on the electronic fatigue testing machine, and connecting the remaining conductive cords at both ends of the H-extracted sample to the conductive metal wire and the source meter, respectively.

[0116] Regarding step (S3b):

[0117] (S3b) Perform fatigue testing and measure contact resistance: turn on the source meter, apply voltage V, and record the real-time current change under certain frequency conditions. Obtain the real-time resistance R by the ratio of voltage V / current I. The fatigue test is carried out during the above resistance measurement process.

[0118] In this invention, the applied voltage V is preferably set to 0.1~10V, specifically 0.1V, 0.2V, 0.3V, 0.4V, 0.5V, 0.6V, 0.7V, 0.8V, 0.9V, or 1.0V. The specified frequency is preferably 1~10Hz, specifically 1Hz, 2Hz, 3Hz, 4Hz, 5Hz, 6Hz, 7Hz, 8Hz, 9Hz, or 10Hz. By fixing the voltage and recording real-time current changes, the real-time resistance R can be obtained through the ratio of voltage V to current I, thus reflecting the resistance change of the cord / rubber composite material.

[0119] In this invention, fatigue testing is conducted concurrently with the aforementioned contact resistance testing process. That is, the recorded contact resistance is the contact resistance during the fatigue testing phase, thus illustrating the fatigue evolution characteristics. The fatigue testing process in this invention includes: turning on the electronic fatigue testing machine, setting fatigue parameters, and conducting the fatigue test.

[0120] The fatigue parameters preferably include: cyclic load, loading waveform, and frequency. The cyclic load includes a minimum load and a maximum load. The minimum load is preferably 1 N. The maximum load is preferably 45~100 N, specifically 45 N, 48 N, 50 N, 55 N, 60 N, 65 N, 70 N, 75 N, 80 N, 84 N, 90 N, 94 N, or 100 N. In some embodiments, the cyclic load is 1~48 N, 1~80 N, 1~84 N, or 1~94 N. In this invention, the loading waveform is preferably a sine wave. In this invention, the frequency is preferably 0.05~10 Hz, specifically 0.05 Hz, 1 Hz, 2 Hz, 3 Hz, 4 Hz, 5 Hz, 6 Hz, 7 Hz, 8 Hz, 9 Hz, or 10 Hz.

[0121] Regarding step (S3c):

[0122] (S3c) Resistance signal processing: The initial stable resistance in (S3b) is taken as the initial resistance R0. The difference between the subsequent resistance and the initial resistance R0 is divided by the ratio of the initial resistance R0 to the resistance change rate ΔR / R0, thereby reflecting the interface fatigue.

[0123] In rubber composites, the elasticity of the rubber component consists of three parts: general elasticity, viscoelasticity, and high elasticity. The latter two cause stress relaxation under stress, meaning that after deformation, it requires a long time to recover, and excessive deformation can even lead to irreversible deformation. This means that external forces on the sample will affect the interfacial conductive network and thus the resistance. During experimental operations, stress is inevitably applied to the rubber composite material; therefore, it needs to be allowed to stand for a sufficient period to reach a stress equilibrium state. Only the stable resistance value reflected at this point can be considered the initial resistance. Otherwise, the resistance curve will drift significantly, which is detrimental to resistance normalization, i.e., the calculation of ΔR / R0. For example, if the material is subjected to a maximum cyclic load of 75N, it will require approximately 20 hours or more for the resistance to stabilize near a certain value. Therefore, in this invention, the initial stable resistance refers to the resistance at the initial stabilization point, which is the resistance that stabilizes after a certain period of standing.

[0124] This invention utilizes a carbon nanotube dispersion to ultrasonically swell RFL-coated cords, introducing CNTs onto the RFL surface and imparting electrical conductivity to the cords. During the composite material molding process, the interface consists of the RFL surface and a several-micrometer-thick layer of rubber connected to it. This invention introduces carbon nanotubes into this region, forming a conductive network. Due to the constraint of this solid-phase interface, the carbon nanotubes cannot move freely. Therefore, changes in the conductivity of this conductive network reflect the contact between the carbon nanotubes at the interface, thus providing effective information on interfacial fatigue. The most typical example is when the composite material is stretched; the interface is subjected to significant shear force, resulting in a noticeable increase in the detected electrical signal ΔR / R0.

[0125] by Figure 5 For example, the increase in the red displacement signal in the figure indicates that fatigue loading has begun (the fatigue testing machine automatically records the displacement changes of its actuator cylinder during fatigue testing; the actuator cylinder is directly connected to the fixture and sample via a flange ring). At this time, the electrical signal ΔR / R0 also shows a corresponding increase. This likely represents the decrease in carbon nanotube contact and the increase in resistance due to interfacial network strain. During the unloading phase after reaching the first cycle's peak, the loading force decreases rapidly, reducing the contact between carbon nanotubes that were originally "oriented" by interfacial shear force, returning them to their original disordered state, thus the resistance continues to increase. In the next loading phase, the orientation caused by interfacial shear force again increases carbon nanotube contact and decreases resistance. However, the fatigue damage caused by the tension strain of the cord has already stretched the macroscopic conductive network, resulting in a further weakening of carbon nanotube contact over a larger area; therefore, the overall resistance remains at an increasing level. Thus, a negative correlation between the electrical signal and the fatigue signal is established, reflecting the interfacial fatigue condition.

[0126] In existing technologies, monitoring schemes for fatigue evolution of cord / rubber composite materials cannot simultaneously achieve both in-situ quantitative monitoring of interface damage and excellent adhesive performance. To address this, this invention provides an in-situ monitoring method for interface fatigue damage in cord / rubber composite materials. This method utilizes a carbon nanotube dispersion to ultrasonically swell the RFL-coated cord, which is then combined with rubber to form an H-extraction sample. A circuit is then connected, and the resulting H-extraction sample is fixed on an electronic fatigue testing machine, forming a closed-loop circuit between the sample and the source surface. Fatigue testing and contact resistance measurement are performed, and the resistance signal is processed to obtain the resistance change rate ΔR / R0. On one hand, this invention directly constructs a conductive network within the RFL impregnation layer at the cord-rubber interface, transforming it into a simple resistance response sensor. This solves the problem of limited actual monitoring area in external photoelectric sensors and the problem of fatigue signal transmission distortion, directly linking the electrical signal to the fatigue condition of the interface. On the other hand, the ultrasonic swelling process introduces conductive particles into the RFL layer, which is not only simple and cost-effective but also greatly preserves the adhesive strength between the two materials. In summary, this invention targets the RFL coating in the cord-rubber composite material, introducing CNTs into the interface layer that enhances adhesion to form a conductive network. The resulting electrical signal can directly correlate with the stress changes in the interface area and reflect its damage. This method effectively overcomes the problem of CNTs being difficult to anchor and disperse in the interface area, without changing the original macroscopic composition of the interface layer, while ensuring fidelity to the original composite material composition. The introduced conductive network penetrates into the RFL layer, greatly reducing the loss of adhesive performance.

[0127] Compared with the prior art, the present invention has the following beneficial effects:

[0128] (1) The raw materials of this invention are inexpensive and the technical implementation is relatively simple. It only requires ultrasonic bath in a CNT dispersion in a commonly used solvent. It also has a very obvious cost advantage in actual production.

[0129] (2) The present invention has good portability. Only the RFL coating on the surface of the skeleton cord, which is necessary for the material, is made conductive, which will not bring additional device burden to the product.

[0130] (3) The present invention introduces CNTs into the RFL layer in an oriented manner, which ensures the accuracy of fatigue signal detection in the interface area without significantly affecting the adhesion performance.

[0131] To further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, and are not intended to limit the scope of the claims of the present invention.

[0132] Example 1

[0133] S1. Preparation of conductive cord:

[0134] (S1a): Take 0.2g of multi-walled carbon nanotubes (diameter 4-6nm, length 0.5~2μm) and add them to 400mL of DMF solvent. Place a vibrating amplitude rod with an ultrasonic generator into the solvent, select an ultrasonic power of 1500W, and use a sweep frequency mode to sonicate for 5min and pause for 10min to dissipate heat. The effective ultrasonic working time is 20min, and a uniformly mixed carbon nanotube dispersion (carbon nanotube concentration 0.5g / L) is obtained.

[0135] (S1b): Take several nylon 66 cords with a specification of 1400dtex / 2 (the cord surface has an RFL coating with a thickness of 20μm), cut them into lengths of about 30-50cm, and immerse them in the carbon nanotube dispersion obtained in step (S1a). At the same time, place the vibration amplitude rod connected to the ultrasonic generator into the dispersion. Select an ultrasonic power of 1500W and use the frequency sweep mode. After every 5 minutes of ultrasonication, pause for 10 minutes to dissipate heat. The effective ultrasonic working time is 30 minutes.

[0136] Then, the ultrasonically swollen cord was removed and placed in anhydrous ethanol for 20 seconds. The cord, along with the anhydrous ethanol, was then placed in a 150W ultrasonic cleaner for 20 seconds. The cord was then removed and dried in a 60°C oven for 20 hours to obtain the conductive cord.

[0137] S2. Preparation of cord / rubber composite material samples:

[0138] Take 100 parts of isoprene rubber, 50 parts of precipitated silica, 3.0 parts of nano zinc oxide, 2.0 parts of stearic acid, 1.0 part of antioxidant, 2.5 parts of sulfur, 1.0 part of vulcanization accelerator, and 0.2 parts of co-vulcanizing agent. Add the isoprene rubber to a mixer and mix for 2 minutes. Then add half of the silica to the mixer and mix for 2 minutes. Add the remaining silica, nano zinc oxide, stearic acid, and antioxidant to the mixer and mix for 4 minutes. After obtaining the masterbatch, transfer it to a two-roll mill, add the vulcanization accelerator, sulfur, co-vulcanizing agent, and anti-scorching agent. Cut it into thin sheets with a thickness of 3 mm to obtain the compound. Let the compound stand at room temperature for 16 hours and cut several 10×200 mm strips.

[0139] Using the vulcanizing mold shown in Figure 1, four rubber strips are stacked in pairs in the bottom mold cavity. Eight 400mm long conductive cords are laid on the rubber strips. One end of each conductive cord passes through a wire groove and is fixed with a bolt, while the other end passes through the wire groove and suspends a 50g weight. The middle mold is placed on the bottom mold and fixed with bolts. Then, two rubber strips are placed in the middle mold cavity. The top mold is placed on the middle mold.

[0140] The assembled vulcanizing mold was placed on a flat vulcanizing machine for vulcanization at a temperature of 145℃, a pressure of 50t, and a time of 65min. After vulcanization, eight single cord / rubber composite H-type samples with rubber dimensions of 10×10×25mm were cut.

[0141] S3. In-situ resistance response monitoring test:

[0142] (S3a) Fixed monitoring circuit:

[0143] Wrap copper wire around the excess conductive cord at both ends of the H-shaped cord / rubber composite sample, and apply conductive graphite adhesive to the connection between the copper wire and the conductive cord for fixation. Figure 3 The fixture shown (pre-insulated) is connected to the electronic fatigue testing machine. A 5mm thick plastic gasket is added between the enamel rings of the two fixtures, and they are fixed with special plastic screws. The H-extraction specimen is fixed on the upper and lower fixtures of the electronic fatigue testing machine, and the copper wires at both ends of the H-extraction specimen are connected to the source meter.

[0144] (S3b) Perform fatigue testing and measure contact resistance:

[0145] Contact resistance measurement: Turn on the source meter, fix the voltage at 1.0V, record the real-time current change at a frequency of 10Hz, and obtain the real-time resistance R by the ratio of voltage V / current I.

[0146] Fatigue test: Turn on the electronic fatigue testing machine, maintain a load of 1N for 2 minutes, and then set the loading parameters at frequencies of 0.05Hz, 0.1Hz, 1Hz and 2Hz respectively, with a range of 1-94N. The loading waveform is a sine wave.

[0147] The above-mentioned contact resistance test is accompanied by a fatigue test, in which the contact resistance during the fatigue test stage is recorded to illustrate the fatigue evolution characteristics.

[0148] (S3c) Resistance signal processing:

[0149] Using the initial stable resistance in (S3b) as the initial resistance R0, the difference between the subsequent resistance and the initial resistance R0 is divided by the ratio of the initial resistance R0 to obtain the resistance change rate ΔR / R0, thereby reflecting interface fatigue.

[0150] Collected data processing and organization, such as Figure 5 As shown, where, Figure 5Figures (a) to (d) show the results under frequencies of 1 Hz, 2 Hz, 0.05 Hz, and 0.1 Hz, respectively. It can be seen that regardless of the loading frequency, the applied sinusoidal displacement signal, starting from the second cycle, consistently produces a sinusoidal feedback with a 90° phase difference in the electrical signal response. This indicates that the resistance of the carbon nanotube conductive network reflects the changes in the macroscopic interface during each cycle.

[0151] Adhesion performance test: Using the H-type test obtained in step S2 as the test sample, the test was conducted according to GB / T 2942-2009 "Determination of Static Adhesion Strength between Vulcanized Rubber and Fiber Cord - H Extraction Method". The results showed that the pull-out force of the untreated cord was 186.26 ± 8.78 N, while the pull-out force of the cord treated with carbon nanotube dispersion in step S1 was 175.31 ± 7.89 N. It can be seen that the pull-out force of the cord did not change much before and after treatment with carbon nanotube dispersion, proving that the method of the present invention can reduce the loss of adhesion performance.

[0152] Example 2

[0153] S1. Preparation of conductive cord:

[0154] (S1a): Take 0.2g of multi-walled carbon nanotubes (diameter 4-6nm, length 0.5~2μm) and add them to 400mL of DMF solvent. Place a vibrating amplitude rod with an ultrasonic generator into the solvent, select an ultrasonic power of 1500W, and use a sweep frequency mode to sonicate for 4min and pause for 5min to dissipate heat. The effective ultrasonic working time is 20min, and a uniformly mixed carbon nanotube dispersion (carbon nanotube concentration 0.5g / L) is obtained.

[0155] (S1b): Take several nylon 66 cords with a specification of 1400dtex / 2 (the cord surface has an RFL coating with a thickness of 20μm), cut them into lengths of about 30-50cm, and immerse them in the carbon nanotube dispersion obtained in step (S1a). At the same time, place the vibration amplitude rod connected to the ultrasonic generator into the dispersion. Select an ultrasonic power of 1500W and use the frequency sweep mode. After every 4 minutes of ultrasonication, pause for 5 minutes to dissipate heat. The effective ultrasonic working time is 30 minutes.

[0156] Then, the ultrasonically swollen cord was removed and placed in anhydrous ethanol for 20 seconds. The cord, along with the anhydrous ethanol, was then placed in a 150W ultrasonic cleaner for 20 seconds. The cord was then removed and dried in a 60°C oven for 20 hours to obtain the conductive cord.

[0157] S2. Preparation of cord / rubber composite material samples:

[0158] Take 100 parts of isoprene rubber, 50 parts of precipitated silica, 3.0 parts of nano zinc oxide, 2.0 parts of stearic acid, 1.0 part of antioxidant, 2.5 parts of sulfur, 1.0 part of vulcanization accelerator, and 0.2 parts of co-vulcanizing agent. Add the isoprene rubber to a mixer and mix for 2 minutes. Then add half of the silica to the mixer and mix for 2 minutes. Add the remaining silica, nano zinc oxide, stearic acid, and antioxidant to the mixer and mix for 4 minutes. After obtaining the masterbatch, transfer it to a two-roll mill, add the vulcanization accelerator, sulfur, co-vulcanizing agent, and anti-scorching agent. Cut it into thin sheets with a thickness of 3 mm to obtain the compound. Let the compound stand at room temperature for 16 hours and cut several 10×200 mm strips.

[0159] Using the vulcanizing mold shown in Figure 1, four rubber strips are stacked in pairs in the bottom mold cavity. Eight 400mm long conductive cords are laid on the rubber strips. One end of each conductive cord passes through a wire groove and is fixed with a bolt, while the other end passes through the wire groove and suspends a 50g weight. The middle mold is placed on the bottom mold and fixed with bolts. Then, two rubber strips are placed in the middle mold cavity. The top mold is placed on the middle mold.

[0160] The assembled vulcanizing mold was placed on a flat vulcanizing machine for vulcanization at a temperature of 145℃, a pressure of 50t, and a time of 65min. After vulcanization, eight single cord / rubber composite H-type samples with rubber dimensions of 10×10×25mm were cut.

[0161] S3. In-situ resistance response monitoring test:

[0162] (S3a) Fixed monitoring circuit:

[0163] Wrap copper wire around the excess conductive cord at both ends of the H-shaped cord / rubber composite sample, and apply conductive graphite adhesive to the connection between the copper wire and the conductive cord for fixation. Figure 3 The fixture shown (pre-insulated) is connected to the electronic fatigue testing machine. A 5mm thick plastic gasket is added between the enamel rings of the two fixtures, and they are fixed with special plastic screws. The H-extraction specimen is fixed on the upper and lower fixtures of the electronic fatigue testing machine, and the copper wires at both ends of the H-extraction specimen are connected to the source meter.

[0164] (S3b) Perform fatigue testing and measure contact resistance:

[0165] Contact resistance measurement: Turn on the source meter, fix the voltage at 1.0V, record the real-time current change at a frequency of 10Hz, and obtain the real-time resistance R by the ratio of voltage V / current I.

[0166] Fatigue test: Turn on the electronic fatigue testing machine, maintain a load of 1N for 2 minutes, and then set the loading parameters at a frequency of 1Hz with a range of 1-94N and 1-48N. The loading waveform is a sine wave.

[0167] The above-mentioned contact resistance test is accompanied by a fatigue test, in which the contact resistance during the fatigue test stage is recorded to illustrate the fatigue evolution characteristics.

[0168] (S3c) Resistance signal processing:

[0169] Using the initial stable resistance in (S3b) as the initial resistance R0, the difference between the subsequent resistance and the initial resistance R0 is divided by the ratio of the initial resistance R0 to obtain the resistance change rate ΔR / R0, thereby reflecting interface fatigue.

[0170] Collected data processing and organization, such as Figure 6 As shown, where, Figure 6 (a) is a graph showing the results of 640 cycles under 1Hz and 1-94N conditions. Figure 6 (b) is Figure 6 (a) shows the results of loops 200-220. Figure 6 (c) shows the results of 14800 cycles under 1Hz and 1-48N conditions. Figure 6 (d) is Figure 6 (c) shows the results of loops 5000-5014. It can be seen that... Figure 6 In the trends of the force and displacement signals in (a) and (c), the cyclic maximum / minimum values ​​initially experienced a rapid increase, followed by a steady increase, and finally a rapid increase to a relatively high value just before fatigue failure. These three characteristics can all be clearly found in the red displacement curve signal, indicating that the black electrical signal curve has a clear correspondence with the load signal. It can effectively reflect the interfacial mechanical evolution throughout the fatigue stage. Figure 6 (b)(d) are the corresponding ones. Figure 6 The local stages in (a) and (c) illustrate Figure 5 The phenomenon of a 90° phase difference between the sinusoidal waves of the force-electric signals was found to still exist in local phases of the complete fatigue cycle test.

[0171] Adhesion performance test: The method is the same as in Example 1. The results show that the average pull force of the cord decreased by only 5.88% before and after treatment with carbon nanotube dispersion, which is not a significant change.

[0172] Example 3

[0173] S1. Preparation of conductive cord:

[0174] (S1a): Take 0.2g of multi-walled carbon nanotubes (diameter 4-6nm, length 0.5~2μm) and add them to 400mL of DMF solvent. Place a vibrating amplitude rod with an ultrasonic generator into the solvent, select an ultrasonic power of 1500W, and use a sweep frequency mode to sonicate for 4min and pause for 5min to dissipate heat. The effective ultrasonic working time is 20min, and a uniformly mixed carbon nanotube dispersion (carbon nanotube concentration 0.5g / L) is obtained.

[0175] (S1b): Take several nylon 66 cords with a specification of 1400dtex / 2 (the cord surface has an RFL coating with a thickness of 20μm), cut them into lengths of about 30-50cm, and immerse them in the carbon nanotube dispersion obtained in step (S1a). At the same time, place the vibration amplitude rod connected to the ultrasonic generator into the dispersion. Select an ultrasonic power of 1500W and use the frequency sweep mode. After every 4 minutes of ultrasonication, pause for 5 minutes to dissipate heat. The effective ultrasonic working time is 30 minutes.

[0176] Then, the ultrasonically swollen cord was removed and placed in anhydrous ethanol for 20 seconds. The cord, along with the anhydrous ethanol, was then placed in a 150W ultrasonic cleaner for 20 seconds. The cord was then removed and dried in a 60°C oven for 20 hours to obtain the conductive cord.

[0177] S2. Preparation of cord / rubber composite material samples:

[0178] Take 100 parts of isoprene rubber, 50 parts of precipitated silica, 3.0 parts of nano zinc oxide, 2.0 parts of stearic acid, 1.0 part of antioxidant, 2.5 parts of sulfur, 1.0 part of vulcanization accelerator, and 0.2 parts of co-vulcanizing agent. Add the isoprene rubber to a mixer and mix for 2 minutes. Then add half of the silica to the mixer and mix for 2 minutes. Add the remaining silica, nano zinc oxide, stearic acid, and antioxidant to the mixer and mix for 4 minutes. After obtaining the masterbatch, transfer it to a two-roll mill, add the vulcanization accelerator, sulfur, co-vulcanizing agent, and anti-scorching agent. Cut it into thin sheets with a thickness of 3 mm to obtain the compound. Let the compound stand at room temperature for 16 hours and cut several 10×200 mm strips.

[0179] Using the vulcanizing mold shown in Figure 1, four rubber strips are stacked in pairs in the bottom mold cavity. Eight 400mm long conductive cords are laid on the rubber strips. One end of each conductive cord passes through a wire groove and is fixed with a bolt, while the other end passes through the wire groove and suspends a 50g weight. The middle mold is placed on the bottom mold and fixed with bolts. Then, two rubber strips are placed in the middle mold cavity. The top mold is placed on the middle mold.

[0180] The assembled vulcanizing mold was placed on a flat vulcanizing machine for vulcanization at a temperature of 145℃, a pressure of 50t, and a time of 65min. After vulcanization, eight single cord / rubber composite H-type samples with rubber dimensions of 10×10×25mm were cut.

[0181] S3. In-situ resistance response monitoring test:

[0182] (S3a) Fixed monitoring circuit:

[0183] Wrap copper wire around the excess conductive cord at both ends of the H-shaped cord / rubber composite sample, and apply conductive graphite adhesive to the connection between the copper wire and the conductive cord for fixation. Figure 3 The fixture shown (pre-insulated) is connected to the electronic fatigue testing machine. A 5mm thick plastic gasket is added between the enamel rings of the two fixtures, and they are fixed with special plastic screws. The H-extraction specimen is fixed on the upper and lower fixtures of the electronic fatigue testing machine, and the copper wires at both ends of the H-extraction specimen are connected to the source meter.

[0184] (S3b) Perform fatigue testing and measure contact resistance:

[0185] Contact resistance measurement: Turn on the source meter, fix the voltage at 1.0V, record the real-time current change at a frequency of 10Hz, and obtain the real-time resistance R by the ratio of voltage V / current I.

[0186] Fatigue test: Turn on the electronic fatigue testing machine, maintain a load of 1N for 2 minutes, and then set the loading parameters at a frequency of 1Hz with a range of 1-80N and 1-84N. The loading waveform is a sine wave.

[0187] The above-mentioned contact resistance test is accompanied by a fatigue test, in which the contact resistance during the fatigue test stage is recorded to illustrate the fatigue evolution characteristics.

[0188] (S3c) Resistance signal processing:

[0189] Using the initial stable resistance in (S3b) as the initial resistance R0, the difference between the subsequent resistance and the initial resistance R0 is divided by the ratio of the initial resistance R0 to obtain the resistance change rate ΔR / R0, thereby reflecting interface fatigue.

[0190] Collected data processing and organization, such as Figure 7 As shown, where, Figure 7 (a) shows the results under the conditions of 1Hz and 1-80N. Figure 7 (b) shows the results under the conditions of 1Hz and 1-84N. It can be seen that... Figure 6The force-electric curves of the two have a good correspondence. In the last few hundred cycles before fatigue failure, it can be clearly seen that the rate of increase of the maximum / minimum value of the electrical signal is much greater than that of the previous stage, which also indicates that fatigue failure is about to occur.

[0191] Adhesion performance test: The method is the same as in Example 1. The results show that the average pull force of the cord decreased by only 10N before and after treatment with carbon nanotube dispersion, which is not a significant change.

[0192] Effect comparison :

[0193] The test results of the prior art are compared with those of the present invention, as shown in Figures 8(a)-(f). Figure 8(a) shows the cyclic tensile resistance response of a single glass fiber and epoxy resin composite material after the CNT layer is introduced by deposition; Figure 8(b) shows the cyclic tensile test results of carbon fiber reinforced epoxy resin; Figure 8(cd) shows the sample image and tensile test results of carbon nanotube braided yarn and polydimethylsiloxane composite material; Figure 8(e) shows the dynamic and static test response of a composite material with hydrogenated nitrile butadiene rubber (HNBR) after CNTs are introduced into the chlorosulfonated polyethylene (CSM) layer outside the glass fiber, where Figures 8(e1)-(e2) are displacement control response diagrams of the pulse waveform, and Figure 8(e3) is the static extraction electrical response diagram; Figure 8(f) shows some test results of the present invention.

[0194] The above comparison of monitoring results shows that the time scale of observation in this invention is far superior to that of fibers treated by similar technical solutions. Furthermore, as... Figures 6-7 As shown, another advantage of this invention is that it can effectively respond to the entire fatigue life cycle of a product, and has considerable application potential for both the study of evolution mechanisms and the monitoring of practical applications.

[0195] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The descriptions of these embodiments are merely to aid in understanding the method and core ideas of the present invention, including the best mode, and to enable any person skilled in the art to practice the present invention, including manufacturing and using any device or system, and implementing any combined method. It should be noted that those skilled in the art can make various improvements and modifications to the present invention without departing from its principles, and these improvements and modifications also fall within the scope of protection of the claims. The scope of protection of this patent is defined by the claims and may include other embodiments that can be conceived by those skilled in the art. If these other embodiments have structural elements similar to those expressed in the claims, or if they include equivalent structural elements that are not substantially different from those expressed in the claims, then these other embodiments should also be included within the scope of the claims.

Claims

1. A method for in-situ monitoring of fatigue damage at the cord / rubber composite interface, characterized in that, The method comprises the following steps: S1, preparing a conductive cord: (S1a): adding carbon nanotubes into a solvent and performing ultrasonic dispersion treatment to obtain a carbon nanotube dispersion liquid; (S1b): immersing the cord into the carbon nanotube dispersion liquid obtained in step (S1a) and performing ultrasonic swelling treatment to obtain a conductive cord; The cord comprises a cord body and an RFL coating layer combined on the surface of the cord body. S2, preparing a cord / rubber composite material sample: An H-extraction sample is prepared from the conductive cord obtained in step S1 and a rubber strip; S3, in-situ monitoring test of resistance response: (S3a): fixing a monitoring circuit The H-extraction sample obtained in step S2 is fixed on an electronic fatigue testing machine, and the conductive cords left at both ends of the H-extraction sample are connected to conductive wires, respectively. Then, the two conductive wires are connected to a source table, so that a closed loop circuit is formed between the H-extraction sample and the source table; (S3b): performing a fatigue test and measuring a contact resistance The source table is opened, a voltage V is loaded, and real-time current changes are recorded under certain frequency conditions. The real-time resistance R is obtained by the ratio of voltage V / current I. The process of measuring the resistance is accompanied by the fatigue test; (S3c): resistance signal processing 2. The method of claim 1, wherein, The initial stable resistance in (S3b) is taken as an initial resistance R0, and the difference between the subsequent resistance and the initial resistance R0 is divided by the initial resistance R0 to obtain a resistance change rate ΔR / R0, which reflects the interface fatigue.

3. The method of claim 1, wherein, In step (S1a), the carbon nanotubes are multi-walled carbon nanotubes; the length of the multi-walled carbon nanotubes is 0.5-50 μm, and the diameter is 4-50 nm.

4. The method of claim 1, wherein, In step (S1a), the ultrasonic dispersion conditions are as follows: power 500-3000 W, effective ultrasonic time 10-60 min, and pause every certain time. In step (S1b): The ultrasonic swelling treatment conditions are as follows: power 500-3000 W, effective ultrasonic time 10-60 min, and pause every certain time; 5. The method of claim 1, wherein, The cord body is a nylon cord, an aramid cord or a polyester fiber cord. Step (S2) comprises: (S2a): placing the rubber strip and the conductive cord obtained in step S1 in a vulcanization mold; 6. The method of claim 1, wherein, (S2b): vulcanizing the vulcanization mold on a vulcanization machine to obtain an H-extraction sample.

7. The method of claim 1, wherein, In step (S3a), the H-extraction sample obtained in step S2 is fixed on the upper and lower clamps of the electronic fatigue testing machine; the upper and lower clamps are pre-treated for insulation. In step (S3a): The conductive wire is a copper wire; The connection mode is winding; 8. The method of claim 1, wherein, The conductive glue is used to fix the connection between the conductive wire and the conductive cord.

9. The method of claim 1, wherein, In step (S3b), the voltage is 1.0 V, and the certain frequency is 1-10 Hz. In step (S3b): The fatigue parameters include: cyclic load, loading waveform and frequency; The minimum load is 1 N, and the maximum load is 48-94 N; The loading waveform is a sine wave; 10. The method of claim 1, wherein, The frequency is preferably 0.05-10 Hz. In step (S1a): The solvent is at least one of DMF, NMP, acetone and toluene; The ultrasonic dispersion treatment is interrupted every 3-5 minutes for 5-10 minutes; The concentration of the carbon nanotubes in the obtained carbon nanotube dispersion is 0.05-5 g / L; In step (S1b): The thickness of the RFL coating is 10-100 μm; The ultrasonic swelling treatment is interrupted every 3-5 minutes for 5-10 minutes; After the ultrasonic swelling treatment, cleaning and drying are further performed.

Citation Information

Cited By

  • Interface bonding failure test method and system, storage medium and program product

    CN121954820A