Method for selectively extracting lithium from waste lithium iron phosphate batteries and high-value utilization of residues

By combining a selective leaching system with a Fenton-like catalyst, the problems of low Li purity and complex residue treatment in waste lithium iron phosphate batteries have been solved, achieving efficient and low-energy resource recycling and pollutant degradation, thus promoting sustainable development.

CN121225625BActive Publication Date: 2026-11-10SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511373182.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-09-24
Publication Date
2026-11-10
Estimated Expiration
2045-09-24

AI Technical Summary

Technical Problem

Existing technologies for the resource recycling of waste lithium iron phosphate batteries suffer from problems such as low purity of Li products, complex and energy-intensive treatment of phosphorus iron residue, and high cost of treating high-salt wastewater.

Method used

Taking advantage of the significant difference in solubility between Li2SO4 and (NH4)2SO4, a selective leaching system is constructed by combining acid and (NH4)2S2O8. Through selective leaching within a specific pH range, efficient extraction and purification of Li are achieved. Furthermore, the phosphorus and iron residue is used to construct a Fenton-like system using a heterogeneous catalyst to degrade organic pollutants in water.

Benefits of technology

This has enabled the resource recovery of high-purity Li products, reduced energy consumption and high-salt wastewater discharge, increased the utilization value of phosphorus iron residue, and achieved the sustainable development goal of "treating waste with waste".

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121225625B_ABST
    Figure CN121225625B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of waste old lithium iron phosphate battery selective lithium extraction and residue high-value utilization method.The present application utilizes the characteristics of the large difference in solubility of Li2SO4 and (NH4)2SO4, forms selective leaching system with acid and (NH4)2S2O8, avoids the problem of low purity of Li recovery product caused by similar chemical properties of Na or K and Li in traditional process, realizes the recycling of high-purity Li product.And, by using the selective leaching system of specific pH range, on the one hand, the leaching rate and selectivity of Li can be improved, on the other hand, the recycling of Li-containing solution can be realized, the effective enrichment of Li can be realized, and the discharge of high-salinity wastewater can also be effectively reduced.In addition, the carbon content of the phosphorus iron residue prepared by the present application is high, which is beneficial to improve the activity of phosphorus iron residue for fenton-like catalyst and enhance the degradation effect of organic pollutants in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of waste lithium battery resource utilization technology, and relates to a method for selective lithium extraction from waste lithium iron phosphate batteries and high-value utilization of residues. Background Technology

[0002] Driven by global "dual carbon" goals, the green and low-carbon transformation of energy is accelerating, and actively developing new energy sources and new energy storage technologies is an inevitable path. As a key carrier of new energy storage systems, lithium-ion batteries have become the most widely used energy storage devices due to their high energy density, small size, and good capacity retention. Among them, lithium iron phosphate batteries (LiFePO4 (LFP)) do not contain precious metals such as Co and Ni, have long cycle life, good stability, and high safety, and are continuously expanding their market share in the global battery market. Surveys show that LFP accounts for as much as 41% of the battery production market in China. Generally, the lifespan of LFPs in electric vehicles is 8-10 years. It is predicted that by 2030, the output of waste LFP batteries will reach 313,300 tons. The large-scale retirement of waste LFP batteries will pose severe environmental and resource challenges. Therefore, the resource recycling of LFP is necessary and urgent.

[0003] Besides lithium (Li), the cathode material of spent LFP batteries does not contain other high-value metal elements, making conventional resource recovery methods ineffective for cost-effective recycling. In recent years, selective Li recovery technology based on spent LFP batteries has attracted widespread attention due to its high Li recovery rate and low operating costs. However, currently used selective recovery technologies face three bottlenecks: 1. The addition of chemicals such as NaOH / Na2CO3 during the leaching and Li precipitation steps introduces impurity element Na. Since Li and Na are in the same group and have similar chemical properties, the separation process is lengthy and complex, leading to a decrease in the purity of the Li product. 2. The treatment and disposal of ferrophosphate residue is a problem. Currently, ferrophosphate residue is mostly disposed of through harmless landfill or purified for LFP synthesis. However, the purification and separation process for low-value ferrophosphate residue is complex and energy-intensive, significantly reducing its economic benefits. 3. The high-salinity wastewater generated during resource recovery requires further treatment, increasing the cost of resource recovery.

[0004] Therefore, developing efficient and environmentally friendly new technologies for the resource recycling of waste lithium iron phosphate batteries is of great significance for promoting the sustainable development of the low-carbon and environmentally friendly industry. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a method for selective lithium extraction from spent lithium iron phosphate batteries and high-value utilization of the residue. This invention innovatively combines acid and (NH4)2S2O8 to form a selective leaching system, leveraging the significant difference in solubility between Li2SO4 and (NH4)2SO4. This avoids the problem of low purity in Li recovery products caused by the similar chemical properties of Na or K with Li in traditional processes, achieving resource recovery of high-purity Li products. Furthermore, this invention employs a selective leaching system within a specific pH range, which improves the leaching rate and selectivity of Li and allows for the recycling of Li-containing solutions, achieving effective Li enrichment. This significantly reduces the energy consumption required for concentration and enrichment in subsequent Li recovery processes, while also effectively reducing the discharge of high-salinity wastewater. In addition, the lithium iron phosphate residue prepared by this invention has a high carbon content and can be used as a heterogeneous catalyst to form a novel Fenton-like system with hydroxylamine and hydrogen peroxide for the efficient degradation of organic pollutants in water, achieving the sustainable development goal of "treating waste with waste."

[0006] The objective of this invention can be achieved through the following methods: In a first aspect, the present invention provides a method for selective lithium extraction from waste lithium iron phosphate batteries and high-value utilization of the residue, comprising the following steps: S1. Place the waste lithium iron phosphate battery black powder in a selective leaching system composed of acid and (NH4)2S2O8 to selectively leach Li elements. S2. Filter the leachate to obtain a Li-containing solution and phosphorus-iron residue, respectively. S3. Repeat steps S1 and S2 with the Li-containing solution to enrich Li; S4. The enriched Li solution is subjected to stepwise evaporation and crystallization to obtain Li2SO4 and crude (NH4)2SO4 products.

[0007] In one embodiment of the present invention, in step S1, the waste lithium iron phosphate battery black powder is pretreated waste lithium iron phosphate battery black powder, and the pretreatment includes: Step 1: Soak the used lithium iron phosphate batteries in a 10-200 g / L NaCl solution for 1-20 days; Step 2: Disassemble the soaked waste lithium iron phosphate batteries and separate the positive electrode plates; Step 3: Soak the positive electrode in deionized water for 1-10 hours, then peel it off to separate the aluminum foil; Step 4: Filter the stripped positive electrode sheet and dry it at 50-70 ℃ for 10-15 h, then grind it to obtain waste lithium iron phosphate battery black powder.

[0008] As one embodiment of the present invention, in step S1, the acid includes one or more of sulfuric acid, nitric acid, hydrochloric acid, citric acid, maleic acid, tartaric acid, and malic acid.

[0009] In one embodiment of the present invention, in step S1, the concentration of waste lithium iron phosphate battery black powder in the selective leaching system is 1~600 g / L, the concentration of acid is 0.1~10 mmol / L, and the pH is 1.5~3.4. Preferably, the concentration of acid is 2-8 mmol / L, and the pH is 1.88-2.45.

[0010] The reason for choosing the specific pH range mentioned above in this invention is that, under weakly acidic conditions, Li + Will with H + An ion exchange reaction occurs, causing Li to... + Extracted from the waste lithium iron phosphate lattice, forming soluble Li + And Fe 2+ / Fe 3+ and PO4 3- It remains in the solid phase, and then the ammonium persulfate in the system will remove the Fe from the solid phase. 2+ Further oxidized to Fe 3+ This makes the Fe in the solid phase 2+ / Fe 3+ and PO4 3- It is completely converted into FePO4 precipitate, which is sparingly soluble in water. Finally, selective lithium extraction is achieved through solid-liquid separation (selectivity of 99.3%), and the Fe recovery rate is as high as 99.9%.

[0011] As one embodiment of the present invention, in step S1, the molar ratio of (NH4)2S2O8 to Fe element in waste lithium iron phosphate battery black powder is 1:1 to 1.5:1.

[0012] In one embodiment of the present invention, in step S1, the reaction time for selective leaching is 10-120 min.

[0013] In one embodiment of the present invention, in step S3, the repetition is performed 20-45 times, preferably 30-45 times.

[0014] As one embodiment of the present invention, in step S4, the stepwise evaporation and crystallization process includes: evaporating the enriched Li solution to 30-50 mL to obtain precipitated Li2SO4, and then evaporating and crystallizing to obtain crude (NH4)2SO4 product.

[0015] In one embodiment of the present invention, in step S4, the crude (NH4)2SO4 product can be used as a nitrogen fertilizer raw material.

[0016] Secondly, the present invention provides a phosphorus-iron residue prepared by the method described above.

[0017] Thirdly, the present invention provides the application of the aforementioned phosphorus iron residue in the preparation of a Fenton-like catalyst for degrading organic pollutants in water.

[0018] In one embodiment of the present invention, the Fenton-like catalyst comprises ferric phosphorus residue, hydroxylamine, and hydrogen peroxide. The ferric phosphorus residue is used as a heterogeneous catalyst.

[0019] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention utilizes the significant difference in solubility between Li2SO4 and (NH4)2SO4 to innovatively combine acid and (NH4)2S2O8 into a selective leaching system, effectively avoiding the ion pollution problem caused by traditional sodium salt systems and achieving the directional separation and purification of Li. At the same time, the phosphorus-iron residue obtained after resource recovery can be used as a catalyst to construct a homogeneous-heterogeneous coupled Fenton catalytic system for the degradation of organic pollutants in water, achieving the goal of green and sustainable resource recovery through "waste treatment of waste".

[0020] 2. This invention employs a selective leaching system within a specific pH range. This improves both the leaching rate and selectivity of Li and allows for the recycling of Li-containing solutions, achieving effective Li enrichment. This significantly reduces the energy consumption required for concentration and enrichment during subsequent Li recovery processes, while also effectively reducing the discharge of high-salinity wastewater. Traditional recovery methods use acid leaching systems with excessively low pH levels. This not only results in low Li selectivity but also prevents the recycling of Li-containing solutions at this pH, causing the concentration to fall short of the minimum Li concentration required for product recovery. Instead, heating and concentration are necessary, significantly increasing energy consumption and generating evaporation wastewater.

[0021] 3. This invention unexpectedly discovered that carbon-containing substances are beneficial for improving the activity of ferrophosphate residue as a Fenton-like catalyst. Specifically, the presence of carbon facilitates electron transport in the Fenton-like process, promoting the activation of oxidants such as hydrogen peroxide, thereby generating more active free radicals for the degradation of organic pollutants in water. Based on this, this invention avoids the use of ultrasonic synergistic oxidation technology and the addition of hydrogen peroxide in traditional recovery methods. This not only simplifies the process, reduces energy consumption, and is suitable for large-scale industrial production, but also increases the carbon content in the ferrophosphate residue, thereby enhancing the degradation effect of the Fenton-like catalyst.

[0022] 4. Based on the two sustainable development concepts of recycling non-renewable resources and "treating waste with waste," this invention has developed a new environmentally friendly process for the efficient resource recycling of waste LFP batteries. The entire process achieves closed-loop reuse of (NH4)2SO4 through material recycling design, producing high-purity Li2SO4 products and using the surplus crude (NH4)2SO4 as a raw material for nitrogen fertilizer. The remaining phosphorus and iron residue can also be used as a Fenton-like catalyst to efficiently degrade organic pollutants in water. This provides a new paradigm with both scientific value and engineering practical significance for the full life cycle management of LFP batteries and the high-value utilization of the solid waste they generate. Attached Figure Description

[0023] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1 This is a flowchart of the recycling process of the present invention; Figure 2 The effects of different sulfuric acid concentrations on Li leaching rate and selectivity in Examples 1-4 and Comparative Example 1; Figure 3 The graphs show the degradation performance and degradation rate constants of organic pollutants by the phosphate iron residue in Example 2 and other different Fenton systems; wherein, (A) is the degradation performance of organic pollutants by the phosphate iron residue (FePO4-LIBs) in Example 2 and other different Fenton systems, and (B) is the degradation rate constant of organic pollutants by the phosphate iron residue (FePO4-LIBs) in Example 2 and other different Fenton systems. Figure 4 This is a graph showing the leaching rate and selective stability of the Li-containing solution reused in Example 2; Figure 5 This is a pH-potential diagram of lithium iron phosphate according to the present invention. Detailed Implementation

[0024] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, providing detailed implementation methods and specific operating procedures, which will help those skilled in the art to further understand the present invention. It should be noted that the scope of protection of the present invention is not limited to the following embodiments; any adjustments and improvements made under the concept of the present invention are all within the scope of protection of the present invention.

[0025] The waste lithium iron phosphate battery black powder in the embodiments and comparative examples of this invention is waste lithium iron phosphate battery black powder after pretreatment. The pretreatment includes: 1) soaking in 100g / L NaCl solution for 10 days to complete the discharge treatment of waste lithium iron phosphate batteries to ensure safe disassembly; 2) physically disassembling waste lithium iron phosphate batteries in a fume hood using tools such as knives and scissors to effectively separate each part of the waste lithium battery; 3) soaking the positive electrode sheet in deionized water for 5 hours and then manually peeling it off to separate the aluminum foil; 4) filtering the remaining positive electrode lithium iron phosphate material and drying it at 60 ℃ for 12 hours, and then grinding it with a mortar and pestle to obtain waste lithium iron phosphate battery black powder.

[0026] Example 1 This embodiment provides a method for selective lithium extraction from spent lithium iron phosphate batteries and high-value utilization of the residue. The process is as follows: Figure 1 This includes the following steps: (1) Under room temperature (25℃) conditions, the waste lithium iron phosphate battery black powder obtained after pretreatment was placed in a selective leaching system composed of (NH4)2S2O8 and sulfuric acid to selectively leach Li elements. The concentration of waste lithium iron phosphate battery black powder was 20 g / L, the molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder was 1:1, the concentration of sulfuric acid was 2 mmol / L, the pH was 2.45, and the reaction time was 30 min. The equation for this reaction is: 2LiFePO4 + (NH4)2S2O8 → Li2SO4 + 2FePO4↓ + (NH4)2SO4; (2) After the reaction is complete, the system obtained in (1) is filtered to obtain a Li-containing solution and a phosphorus-iron residue. (3) The Li-containing solution obtained in (2) is reused in steps (1) and (2) for 20 times to achieve Li enrichment; (4) The enriched Li solution is subjected to simple stepwise evaporation and crystallization to obtain high-purity Li2SO4 product and crude (NH4)2SO4 product, wherein the crude (NH4)2SO4 product can be used as nitrogen fertilizer raw material; wherein the stepwise evaporation and crystallization step is as follows: 100 mL is used to evaporate the enriched Li solution to 30~50 mL to obtain precipitated Li2SO4, and then the crude (NH4)2SO4 product is obtained by evaporation and crystallization.

[0027] (5) Phosphorus iron residue is used as a heterogeneous catalyst to form a novel Fenton-like system with hydroxylamine and hydrogen peroxide for the efficient degradation of organic pollutants in water.

[0028] (6) The concentration of metal elements in the Li-containing solution obtained in (2) was detected by inductively coupled plasma optical emission spectrometry (ICP-OES). It was found that the Li leaching rate reached 96.4% and the selectivity reached 99.7% within 30 min. The concentration of metal elements in the enriched Li solution obtained in (3) was detected. It was found that the Li leaching rate reached 94.4% and the selectivity reached 97.7% within 30 min.

[0029] (7) The catalytic performance of potassium persulfate (PMS) degrading bisphenol A (BPA) was evaluated by activating potassium persulfate (PMS) with phosphorus iron residue catalyst. The specific operation steps are as follows: First, add 50 mL of 5 mg / L BPA solution to a 100 mL beaker, and add phosphorus iron residue catalyst at a ratio of 0.1 g / L. Place the reaction vessel in a constant temperature water circulation device, set the temperature to 25 ℃, and stir with a magnetic stirrer for 15 min until the adsorption-desorption equilibrium between BPA molecules and the catalyst is reached. Then, add 1 mM NH2OH·HCl and 5 mM H2O2 to the solution to start the removal reaction. After reacting for 12 min, take 1.0 mL of water sample from the reaction solution every 2 min, and immediately add 1.0 mL of methanol to quench the active substances and terminate the reaction. After quenching, filter the mixture using a 0.22 μm polytetrafluoroethylene filter membrane, and then detect the concentration of BPA in the filtrate by high performance liquid chromatography. It was found that the BPA degradation rate reached 93.2% after the system reacted for 12 minutes.

[0030] Example 2 (1) Under room temperature (25℃) conditions, the waste lithium iron phosphate battery black powder obtained after pretreatment was placed in a selective leaching system composed of (NH4)2S2O8 and sulfuric acid to selectively leach Li elements. The concentration of waste lithium iron phosphate battery black powder was 20 g / L, the molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder was 1:1, the concentration of sulfuric acid was 4 mmol / L, the pH was 2.18, and the reaction time was 30 min. (2) After the reaction is complete, the system obtained in (1) is filtered to obtain a Li-containing solution and a phosphorus-iron residue. (3) The Li-containing solution obtained in (2) is reused in steps (1) and (2) for 20 times to achieve Li enrichment; (4) The enriched Li solution is subjected to simple stepwise evaporation and crystallization to obtain high-purity Li2SO4 product and crude (NH4)2SO4 product, wherein the crude (NH4)2SO4 product can be used as a nitrogen fertilizer raw material; (5) Phosphorus iron residue is used as a heterogeneous catalyst to form a novel Fenton-like system with hydroxylamine and hydrogen peroxide for the efficient degradation of organic pollutants in water.

[0031] (6) The concentration of metal elements in the Li-containing solution obtained in (2) was detected by ICP-OES. It was found that the Li leaching rate reached 100% and the selectivity reached 99.3% within 30 min. The concentration of metal elements in the enriched Li solution obtained in (3) was detected. It was found that the Li leaching rate reached 99.3% and the selectivity reached 98.7% within 30 min.

[0032] Example 3 (1) Under room temperature (25℃) conditions, the waste lithium iron phosphate battery black powder obtained after pretreatment was placed in a selective leaching system composed of (NH4)2S2O8 and sulfuric acid to selectively leach Li elements. The concentration of waste lithium iron phosphate battery black powder was 20 g / L, the molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder was 1:1, the concentration of sulfuric acid was 6 mmol / L, the pH was 1.99, and the reaction time was 30 min. (2) After the reaction is complete, the system obtained in (1) is filtered to obtain a Li-containing solution and a phosphorus-iron residue. (3) The Li-containing solution obtained in (2) is reused in steps (1) and (2) for 20 times to achieve Li enrichment; (4) The enriched Li solution is subjected to simple stepwise evaporation and crystallization to obtain high-purity Li2SO4 product and crude (NH4)2SO4 product, wherein the crude (NH4)2SO4 product can be used as a nitrogen fertilizer raw material; (5) Phosphorus iron residue is used as a heterogeneous catalyst to form a novel Fenton-like system with hydroxylamine and hydrogen peroxide for the efficient degradation of organic pollutants in water.

[0033] (6) The concentration of metal elements in the Li-containing solution obtained in (2) was detected by ICP-OES. It was found that the Li leaching rate reached 99.9% and the selectivity reached 98.8% within 30 min. The concentration of metal elements in the enriched Li solution obtained in (3) was detected. It was found that the Li leaching rate reached 98.9% and the selectivity reached 96.4% within 30 min.

[0034] Example 4 (1) Under room temperature (25℃) conditions, the waste lithium iron phosphate battery black powder obtained after pretreatment was placed in a selective leaching system composed of (NH4)2S2O8 and acid to selectively leach Li elements. The concentration of waste lithium iron phosphate battery black powder was 20 g / L, the molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder was 1:1, the concentration of sulfuric acid was 8 mmol / L, the pH was 1.88, and the reaction time was 30 min. (2) After the reaction is complete, the system obtained in (1) is filtered to obtain a Li-containing solution and a phosphorus-iron residue. (3) The Li-containing solution obtained in (2) is reused in steps (1) and (2) for 20 times to achieve Li enrichment; (4) The enriched Li solution is subjected to simple stepwise evaporation and crystallization to obtain high-purity Li2SO4 product and crude (NH4)2SO4 product, wherein the crude (NH4)2SO4 product can be used as a nitrogen fertilizer raw material; (5) Phosphorus iron residue is used as a heterogeneous catalyst to form a novel Fenton-like system with hydroxylamine and hydrogen peroxide for the efficient degradation of organic pollutants in water.

[0035] (6) The concentration of metal elements in the Li-containing solution obtained in (2) was detected by ICP-OES. It was found that the Li leaching rate reached 100% and the selectivity reached 98.1% within 30 min. The concentration of metal elements in the enriched Li solution obtained in (3) was detected. It was found that the Li leaching rate reached 99.4% and the selectivity reached 95.4% within 30 min.

[0036] Comparative Example 1 (1) Under room temperature (25℃) conditions, the waste lithium iron phosphate battery black powder obtained after pretreatment was placed in a selective leaching system composed of (NH4)2S2O8 and acid to selectively leach Li elements. The concentration of waste lithium iron phosphate battery black powder was 20 g / L, the molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder was 1:1, the concentration of sulfuric acid was 0 mmol / L, the pH was 3.43, and the reaction time was 30 min. (2) After the reaction is complete, the system obtained in (1) is filtered to obtain a Li-containing solution and a phosphorus-iron residue. (3) The Li-containing solution obtained in (2) is reused in steps (1) and (2) for 20 times to achieve Li enrichment; (4) The enriched Li solution is subjected to simple stepwise evaporation and crystallization to obtain high-purity Li2SO4 product and crude (NH4)2SO4 product, wherein the crude (NH4)2SO4 product can be used as a nitrogen fertilizer raw material; (5) Phosphorus iron residue is used as a heterogeneous catalyst to form a novel Fenton-like system with hydroxylamine and hydrogen peroxide for the efficient degradation of organic pollutants in water.

[0037] (6) The concentration of metal elements in the Li-containing solution obtained in (2) was detected by ICP-OES. It was found that the Li leaching rate reached 88.5% and the selectivity reached 100% within 30 min. The concentration of metal elements in the enriched Li solution obtained in (3) was detected. It was found that the Li leaching rate reached 82.7% and the selectivity reached 97.8% within 30 min.

[0038] Figure 2 Examples 1-4 and Comparative Example 1 show the effects of different sulfuric acid concentrations on Li leaching rate and selectivity. It can be seen that if the pH of the selective leaching system is too high, the Li leaching rate will decrease significantly, thus affecting Li recovery.

[0039] Figure 3 (A) is a graph showing the degradation performance of FePO4-LIBs and other Fenton systems in Example 2 on organic pollutants. (B) is a graph showing the degradation rate constants of FePO4-LIBs and other Fenton systems in Example 2 on organic pollutants. It can be seen that the FePO4-LIBs prepared in this invention has higher degradation performance and rate on organic pollutants.

[0040] Figure 4 The figure shows the leaching rate and selectivity stability of the Li-containing solution in Example 2. It can be seen that the Li-containing solution maintains a relatively stable Li leaching rate and selectivity in multiple recycling cycles.

[0041] Figure 5 The pH-potential diagram for lithium iron phosphate shows that the pH range of 1.88-2.45 is conducive to the efficient recovery of Li.

[0042] Comparative Example 2 The method of this comparative example is basically the same as that of Example 1. The only difference is that the sulfuric acid concentration in step (1) is replaced with 0.2 mol / L, and its pH is 0.70. At this pH, the reuse operation in step (3) cannot be performed.

[0043] The concentration of metal elements in the Li-containing solution obtained in (2) was detected by ICP-OES. It was found that the Li leaching rate reached 100% and the selectivity reached 55.4% within 30 min.

[0044] Comparative Example 3 The method used in this comparative example is basically the same as that in Example 1, except that ultrasonic treatment is added in step (1), as follows: (1) Under room temperature (25℃) conditions, the waste lithium iron phosphate battery black powder obtained after pretreatment was placed in a selective leaching system composed of (NH4)2S2O8 and sulfuric acid, and the selective leaching of Li element was carried out under ultrasonic treatment of 200W. The concentration of waste lithium iron phosphate battery black powder was 20 g / L, the molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder was 1:1, the concentration of sulfuric acid was 2 mmol / L, the pH was 2.45, and the reaction time was 30 min.

[0045] The phosphorus iron residue in step (2) was subjected to Fenton-like performance tests, and the results are as follows: the degradation rate of BPA at 12 min was only 75.4%, which is 17.8% lower than the 93.2% in Example 1.

[0046] Traditional recovery processes use excessively high-concentration acid solutions, resulting in excessively low pH levels. This leads to the following consequences: 1. Significant dissolution and loss of Fe and P. When the pH is below 1.5, ferric phosphate (FePO4) dissolves in large quantities, increasing the concentration of Fe and P impurities in the Li-containing solution. This increases the difficulty of impurity removal during subsequent Li product recovery, reducing the FePO4 recovery rate to only around 90% at its optimal level. 2. Fe and P impurities dissolved at excessively low pH levels enter the washing liquid, increasing wastewater treatment costs (e.g., P removal, as P is a key element causing eutrophication). 3. Significantly reduced process economics. Increased acid consumption necessitates substantial alkali neutralization, increasing reagent costs; Fe and P loss leads to decreased resource recovery rates and overall process efficiency reduction. Furthermore, traditional recovery processes add hydrogen peroxide to the leaching system, creating a strong oxidizing effect that increases the mineralization of carbonaceous substances, thereby reducing the carbon content in the ferric phosphate residue and consequently lowering its Fenton-like activity. In addition, traditional recycling processes also use ultrasonic synergistic oxidation technology, but the industrial application of ultrasound has the following problems: 1. Severe noise pollution; 2. Low energy transfer efficiency, with most of the electrical energy lost as heat, resulting in high energy consumption; 3. Sound wave reflection, interference, and attenuation in large industrial reactors, resulting in the coexistence of "hot spots" and "cold spots," which reduces reaction efficiency; 4. High-power ultrasonic systems are expensive and require a matching cooling system to prevent overheating, further increasing their cost.

[0047] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for selective lithium extraction from waste lithium iron phosphate batteries and high-value utilization of the residue, characterized in that, Includes the following steps: S1. Place the waste lithium iron phosphate battery black powder in a selective leaching system composed of acid and (NH4)2S2O8 to selectively leach Li elements. In the selective leaching system, the acid concentration is 0.1~10 mmol / L, and the pH is 1.5~3.4; The molar ratio of (NH4)2S2O8 to Fe in waste lithium iron phosphate battery black powder is 1:1 to 1.5:1; S2. Filter the leachate to obtain a Li-containing solution and phosphorus-iron residue, respectively. The phosphorus-iron residue is used to prepare a Fenton-like catalyst for degrading organic pollutants in water; the Fenton-like catalyst includes phosphorus-iron residue, hydroxylamine, and hydrogen peroxide; S3. Repeat steps S1 and S2 with the Li-containing solution to enrich Li; The number of repetitions is 20-45 times; S4. The enriched Li solution is subjected to stepwise evaporation and crystallization to obtain Li2SO4 and crude (NH4)2SO4 products.

2. The method according to claim 1, characterized in that, In step S1, the waste lithium iron phosphate battery black powder is pretreated waste lithium iron phosphate battery black powder, and the pretreatment includes: Step 1: Soak the used lithium iron phosphate batteries in a 10-200 g / L NaCl solution for 1-20 days; Step 2: Disassemble the soaked waste lithium iron phosphate batteries and separate the positive electrode plates; Step 3: Soak the positive electrode in deionized water for 1-10 hours, then peel it off to separate the aluminum foil; Step 4: Filter the stripped positive electrode sheet and dry it at 50-70 ℃ for 10-15 h, then grind it to obtain waste lithium iron phosphate battery black powder.

3. The method according to claim 1, characterized in that, In step S1, the concentration of waste lithium iron phosphate battery black powder in the selective leaching system is 1~600 g / L.

4. The method according to claim 3, characterized in that, The acid includes one or more of sulfuric acid, nitric acid, hydrochloric acid, citric acid, maleic acid, tartaric acid, and malic acid; in the selective leaching system, the concentration of the acid is 2-8 mmol / L and the pH is 1.88-2.

45.

5. The method according to claim 1, characterized in that, In step S1, the reaction time for selective leaching is 10-120 min.

6. A phosphorus-iron residue prepared by the method according to any one of claims 1-5.

Citation Information

Patent Citations

  • Method for water treatment through Fenton oxidation coupled with sludge biochar-ferric phosphate catalyst

    CN113244937A

  • Lithium iron phosphate (LFP) battery recovery

    CN117795736A