Zinc oxide-silicon dioxide core-shell nanostructure composite material and preparation method thereof
By preparing zinc oxide-silica core-shell nanostructured composite materials, controlling the thickness of the silica layer, and utilizing Si-O-Zn bonds, the selectivity and stability issues of existing materials in generating singlet oxygen were solved, achieving efficient singlet oxygen generation.
Patent Information
- Application Number
- CN202511341580.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-19
- Publication Date
- 2026-01-23
AI Technical Summary
When existing materials generate singlet oxygen (1O2), they often generate other reactive oxygen species, such as H2O2 and ·OH, resulting in low reaction selectivity and low efficiency.
A zinc oxide-silica core-shell nanostructured composite material was prepared by controlling the thickness of the silica layer to 8-12 nm and utilizing Si-O-Zn bonds to suppress the migration of photogenerated carriers, resulting in the generation of only singlet oxygen.
It achieves the generation of only singlet oxygen under light conditions, improving reaction selectivity and chemical stability of materials, and avoiding the generation of other reactive oxygen species.
Smart Images

Figure CN121377100A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic functional materials technology, and in particular to a zinc oxide-silica core-shell nanostructured composite material and its preparation method. Background Technology
[0002] Singlet oxygen ( 1 O2 is a metastable electronically excited state of molecular oxygen. As an important reactive oxygen species (ROS), it has been widely studied and applied in many fields due to its unique reactivity and selectivity in various chemical and biological systems. In contrast, other common reactive oxygen species, such as hydrogen peroxide (H2O2), hydroxyl radicals (·OH), and superoxide anion radicals (O2), are less reactive. - These reactive oxygen species typically exhibit low selectivity and indiscriminate attack on a variety of substrates. Currently, most materials in existing technologies simultaneously generate multiple reactive oxygen species, which leads to low efficiency in applications such as photodynamic therapy or organic synthesis. Summary of the Invention
[0003] The purpose of this invention is to address the aforementioned shortcomings of the prior art by proposing a zinc oxide-silica core-shell nanostructured composite material and its preparation method.
[0004] The first objective of this invention is to provide a zinc oxide-silica core-shell nanostructured composite material, with nano zinc oxide particles as the core and a silica layer as the shell, wherein the thickness of the silica layer is 8nm-12nm; it specifically generates singlet oxygen.
[0005] Furthermore, the thickness of the silicon dioxide layer is 8 nm-8.6 nm.
[0006] Furthermore, the particle size of the nano zinc oxide is 30-100 nm.
[0007] The second objective of this invention is to provide a method for preparing the zinc oxide-silica core-shell nanostructured composite material as described above, characterized by comprising the following steps: (1) Disperse the nano zinc oxide powder in an ethanol aqueous solution and adjust the pH to 5-7 to obtain a zinc oxide dispersion system; (2) Add tetraethyl orthosilicate and octadecyltrimethoxysilane to ethanol and stir until homogeneous to obtain a tetraethyl orthosilicate solution; (3) Add the tetraethyl orthosilicate solution obtained in step (2) to the zinc oxide dispersion system, stir, centrifuge, collect the precipitate, wash, dry, and obtain the precursor; (4) The precursor obtained in step (3) is calcined in air to obtain zinc oxide-silica core-shell nanostructured composite material.
[0008] Further, in step (3), stirring is performed for 10-15 h.
[0009] Further, in step (4), the heating rate is 1.5-3 ℃ / min, and the calcination is performed at 580-700 ℃ for 1.5-3 h.
[0010] Further, in step (1), the ethanol aqueous solution is prepared according to a volume ratio of ethanol to deionized water of 3:0.5-1.5 mL, and the mass-volume ratio of the nano-zinc oxide to the ethanol aqueous solution is 1 g:3-5 mL. In step (2), the volume ratio of tetraethyl orthosilicate, octadecyltrimethoxysilane and ethanol is 0.15-0.28:0.035-0.06:2.
[0011] Further, the ratio of the nano-zinc oxide powder to tetraethyl orthosilicate is 1 g:0.42-0.9 mL.
[0012] Further, the preparation method of the nano-zinc oxide powder comprises the following steps: S1. Sodium hydroxide is added to an ethanol aqueous solution, and stirring is performed to heat to 80-90 ℃ to obtain a solution A; S2. Zinc acetate and cetyltrimethylammonium bromide are added to an ethanol aqueous solution, and stirring is performed to heat to 80-90 ℃ to obtain a solution B; S3. The solution B is quickly added to the solution A, and reaction is performed at 600-800 rpm for 5-20 min, and quick centrifugation is performed, and the precipitate is obtained by washing with deionized water for 3-4 times; S4. The precipitate is dispersed into deionized water, and spray drying is performed at 110-125 ℃ to obtain the nano-zinc oxide powder.
[0013] Further, in steps S1 and S2, the ethanol aqueous solution is prepared according to a volume ratio of ethanol to deionized water of 1:8-10; In the solution A, the concentration of sodium hydroxide is 0.8-1.2 mol / L, in the solution B, the concentration of zinc acetate is 0.4-0.6 mol / L, and the concentration of cetyltrimethylammonium bromide is 2-4 g / L; In step S3, the volume ratio of the solution A to the solution B is 1:1.
[0014] Compared with the prior art, the present application has the following beneficial effects: The present application provides a zinc oxide-silicon dioxide core-shell nanostructure composite material, limits the thickness of the silicon dioxide layer to 8-12 nm, effectively inhibits the migration of photo-generated carriers (photo-generated electrons or holes) to the surface, and maintains effective energy transfer, so that the composite material does not generate other active oxygen substances H2O2, ·OH and O2 under light conditions.- only generate singlet oxygen 1 O2, and the coated silicon dioxide and zinc oxide are connected through Si-O-Zn bonds, enhancing the chemical stability of the composite material.
[0015] The preparation method of the zinc oxide-silicon dioxide core-shell nanostructure composite material of the application can obtain the zinc oxide coated with silicon dioxide with uniform coating, high dispersibility and other advantages, and the coating thickness can be controlled, and zinc oxide with different silicon dioxide coating thicknesses can be obtained by adjusting the ratio; the coating layer of silicon dioxide and zinc oxide are connected through Zn-O-Si bonds, improving the interface bonding of silicon dioxide and zinc oxide, and improving the chemical stability of the composite material.
[0016] The preparation method of the zinc oxide-silicon dioxide core-shell nanostructure composite material of the application can obtain the zinc oxide-silicon dioxide core-shell nanostructure composite material with high dispersibility and stability by optimizing the preparation steps and parameters of zinc oxide.
[0017] The preparation method of the zinc oxide-silicon dioxide core-shell nanostructure composite material of the application is simple to operate, raw materials are easy to obtain, and is suitable for large-scale production. BRIEF DESCRIPTION OF DRAWINGS
[0018] Figure 1 The transmission electron microscope image (TEM image) of the nano zinc oxide powder prepared in Example 1 of the application; Figure 2 The transmission electron microscope image of the nano zinc oxide powder prepared in Comparative Example 1 of the application; Figure 3 The transmission electron microscope image of the nano zinc oxide powder prepared in Comparative Example 2 of the application; Figure 4 The transmission electron microscope image of the nano zinc oxide powder prepared in Comparative Example 3 of the application; Figure 5 The transmission electron microscope image of the nano zinc oxide powder prepared in Comparative Example 4 of the application; Figure 6 The transmission electron microscope image of the nano zinc oxide powder prepared in Comparative Example 5 of the application; Figure 7 The preparation process flow chart of the zinc oxide-silicon dioxide core-shell nanostructure composite material of the application; Figure 8 The XRD pattern of the zinc oxide-silicon dioxide core-shell nanostructure composite material prepared in Example 2, Comparative Examples 7 and 8 of the application: a is the XRD full pattern; a is the XRD local enlarged view; Figure 9TEM images of zinc oxide-silica core-shell nanostructure composite prepared for inventive example 2: a is FESEM image of zinc oxide; b is TEM image of inventive example 2 (ZS15); c is HRTEM image of inventive example 2 (ZS15); (d-h) are HAADF image and EDX image of inventive example 2; Figure 10 TEM images of zinc oxide-silica core-shell nanostructure composite prepared for inventive example 2: a is FESEM image of zinc oxide; b is TEM image of inventive example 2 (ZS15); c is HRTEM image of inventive example 2 (ZS15); (d-h) are HAADF image and EDX image of inventive example 2; Figure 11 TEM images of zinc oxide-silica core-shell nanostructure composite prepared for inventive example 2: a is FESEM image of zinc oxide; b is TEM image of inventive example 2 (ZS15); c is HRTEM image of inventive example 2 (ZS15); (d-h) are HAADF image and EDX image of inventive example 2; Figure 12 TEM images of zinc oxide-silica core-shell nanostructure composite prepared for inventive example 2: a is FESEM image of zinc oxide; b is TEM image of inventive example 2 (ZS15); c is HRTEM image of inventive example 2 (ZS15); (d-h) are HAADF image and EDX image of inventive example 2; Figure 13 XPS images of zinc oxide-silica core-shell nanostructure composite prepared for inventive example 2, comparative examples 7 and 8; Figure 14 Active oxygen species generated by ZnO and zinc oxide-silica core-shell nanostructure composite prepared for inventive example 2, comparative examples 7 and 8. DETAILED DESCRIPTION
[0019] The following are specific embodiments of the present application and further describe the technical solutions of the present application in conjunction with the accompanying drawings, but the present application is not limited to these embodiments.
[0020] Example 1 A method for preparing a nano-zinc oxide powder, comprising the following steps: S1. 0.2 mol of sodium hydroxide was added to 200 mL of an ethanol aqueous solution, which was prepared by mixing 20 mL of ethanol with 180 mL of water, and heated to 90 ℃ under stirring to obtain solution A; S2. 0.1 mol of zinc acetate and 1 g of cetyltrimethylammonium bromide (CTAB) were added to 200 mL of an ethanol aqueous solution, which was prepared by mixing 20 mL of ethanol with 180 mL of water, and heated to 90 ℃ under stirring to obtain solution B; S3. Solution B was quickly added to solution A, and reacted for 10 min under 800 rpm, and then quickly centrifuged, and washed with deionized water for 3 times to obtain a precipitate; S4. The precipitate was dispersed into 200 mL deionized water and spray dried at 120 ℃, with an inlet temperature of 120 ℃, a fan frequency of 35 Hz, and a peristaltic speed of 13 RPM, to obtain the nano-zinc oxide powder.
[0021] The nano-zinc oxide powder prepared in this example 1 was dispersed in ethanol and then photographed by transmission electron microscope, and the transmission electron microscope image (TEM) is shown in Figure 1 From the TEM image, it can be seen that the nano-zinc oxide powder prepared in this example has good dispersibility. Figure 1
[0022] Comparative Example 1 The difference between this comparative example and example 1 is that in step S3, the reaction time is 1 h, and other steps and parameters are the same as in example 1. The transmission electron microscope image of the nano-zinc oxide prepared in this comparative example is shown in Figure 2 The zinc oxide is agglomerated and has poor dispersibility.
[0023] Comparative Example 2 The difference between this comparative example and example 1 is that in step S2, only CTAB is added, and the solution does not contain ethanol, and other steps and parameters are the same as in example 1. The transmission electron microscope image of the nano-zinc oxide prepared in this comparative example is shown in Figure 3 The zinc oxide is agglomerated and has poor dispersibility.
[0024] Comparative Example 3 The difference between this comparative example and example 1 is that in steps S1 and S2, the ethanol in the ethanol aqueous solution is 40 mL, and other steps and parameters are the same as in example 1. The transmission electron microscope image of the nano-zinc oxide prepared in this comparative example is shown in Figure 4 The zinc oxide is agglomerated and has poor dispersibility.
[0025] Comparative Example 4 The difference between this comparative example and example 1 is that in step S2, zinc sulfate is used instead of zinc acetate, and other steps and parameters are the same as in example 1. The transmission electron microscope image of the nano-zinc oxide prepared in this comparative example is shown in Figure 5 The zinc oxide is agglomerated and has poor dispersibility.
[0026] Comparative Example 5 The difference between this comparative example and example 1 is that in step S2, zinc chloride is used instead of zinc acetate, and other steps and parameters are the same as in example 1. The transmission electron microscope image of the nano-zinc oxide prepared in this comparative example is shown in Figure 6 The zinc oxide is agglomerated and has poor dispersibility.
[0027] The nano-zinc oxide powder prepared in example 1 was used in the following preparation of zinc oxide-silicon dioxide core-shell nanostructure composite material.
[0028] Example 2 A method for preparing a zinc oxide-silicon dioxide core-shell nanostructure composite material for specifically generating singlet oxygen is shown in Figure 7 and comprises the following steps: (1) 1 g of nano zinc oxide powder is dispersed in 4 mL of an ethanol aqueous solution, the ethanol aqueous solution is prepared by mixing 3 mL of ethanol and 1 mL of deionized water, and diluted hydrochloric acid is used to adjust the pH to 6 to obtain a zinc oxide dispersion system; (2) 0.6 mL of tetraethyl orthosilicate and 0.05 mL of octadecyl trimethoxysilane are added to 1 mL of ethanol, and stirred uniformly to obtain a tetraethyl orthosilicate solution; (3) The tetraethyl orthosilicate solution obtained in step (2) is added to the zinc oxide dispersion system, stirred at room temperature for 12 h, centrifuged, the precipitate is collected, washed, and dried at 80°C for 12 h to obtain a precursor; (4) The precursor obtained in step (3) is calcined in an air atmosphere at a temperature increasing rate of 2°C / min to 600°C for 2 h to obtain a zinc oxide-silicon dioxide core-shell nanostructure composite material, which is named ZS15.
[0029] Comparative Example 6 This comparative example is different from Example 2 in that no octadecyl trimethoxysilane is added in step (2), and the other steps and parameters are the same as those in Example 2. The transmission electron microscope image of the zinc oxide-silicon dioxide composite material prepared in this comparative example is shown in Figure 11 , and the uniformity of the zinc oxide surface coating is poor.
[0030] Under the same conditions, omit ZnO, and directly use the pure TEOS hydrolysis method to prepare amorphous SiO2 powder, see Figure 12 .
[0031] Comparative Example 7 A method for preparing a zinc oxide-silicon dioxide core-shell nanostructure composite material is shown in Figure 7 and comprises the following steps: (1) 1 g of nano zinc oxide powder is dispersed in 4 mL of an ethanol aqueous solution, the ethanol aqueous solution is prepared by mixing 3 mL of ethanol and 1 mL of deionized water, and diluted hydrochloric acid is used to adjust the pH to 6 to obtain a zinc oxide dispersion system; (2) 0.2 mL of tetraethyl orthosilicate and 0.05 mL of octadecyl trimethoxysilane are added to 1 mL of ethanol, and stirred uniformly to obtain a tetraethyl orthosilicate solution; (3) The tetraethyl orthosilicate solution obtained in step (2) is added to the zinc oxide dispersion system, stirred at 800 rpm at room temperature for 12 h, centrifuged, the precipitate is collected, washed, and dried at 80°C for 12 h to obtain a precursor; (4) The precursor obtained in step (3) is calcined in an air atmosphere at a temperature- increasing rate of 2 ℃ / min to 600 ℃ for 2 h to obtain a zinc oxide-silicon dioxide core-shell nanostructure composite material, which is named ZS5.
[0032] Comparative Example 8 A preparation method of a zinc oxide-silicon dioxide core-shell nanostructure composite material is shown in Figure 7 and includes the following steps: (1) 1 g of nano zinc oxide powder is dispersed in 4 mL of an ethanol aqueous solution, the ethanol aqueous solution is prepared by mixing 3 mL of ethanol and 1 mL of deionized water, and the pH is adjusted to 6 to obtain a zinc oxide dispersion system; (2) 0.4 mL of tetraethyl orthosilicate and 0.05 mL of octadecyl trimethoxysilane are added to 1 mL of ethanol, and stirred uniformly to obtain a tetraethyl orthosilicate solution; (3) The tetraethyl orthosilicate solution obtained in step (2) is added to the zinc oxide dispersion system, stirred at room temperature for 12 h, centrifuged, the precipitate is collected, washed, and dried at 80 ℃ for 12 h to obtain a precursor; (4) The precursor obtained in step (3) is calcined in an air atmosphere at a temperature- increasing rate of 2 ℃ / min to 600 ℃ for 2 h to obtain a zinc oxide-silicon dioxide core-shell nanostructure composite material, which is named ZS1.
[0033] The XRD pattern of the zinc oxide-silicon dioxide core-shell nanostructure composite material prepared in Example 2, Comparative Examples 7 and 8 is shown in Figure 8 , and the TEM image is shown in Figures 9-10 As can be seen from the figures, the zinc oxide surface is uniformly coated with silicon dioxide, and as the amount of tetraethyl orthosilicate increases, the thickness of the coating layer increases, and by adjusting the ratio, zinc oxide with different SiO2 coating thicknesses can be obtained.
[0034] Figure 13 The XPS diagram of the zinc oxide-silicon dioxide core-shell nanostructure composite material prepared in Example 2, Comparative Examples 7 and 8 is shown in Figures a and b. The additional new peaks of the zinc oxide-silicon dioxide core-shell nanostructure composite material indicate that a Zn-O-Si bond is formed between the ZnO and the silicon dioxide shell layer, the interface bonding is strong, and the stability is high.
[0035] Figure 14 The active oxygen species generated by ZnO and the zinc oxide-silicon dioxide core-shell nanostructure composite material prepared in Example 2, Comparative Examples 7 and 8 are shown in Figure 14 As can be seen from the figures, in addition to the composite material prepared in Example 4 generating only singlet oxygen, the composite materials prepared in Comparative Examples 7 and 8 generate other active oxygen. 1O2 can be generated through two distinct pathways. In the first pathway, the photosensitizer in the excited triplet state undergoes photoinduced electron transfer, thereby generating a radical intermediate, such as the superoxide anion radical (·O2). - These free radical intermediates can react with photogenerated holes to ultimately generate... 1 O2. In the second pathway, the semiconductor surface excites a triplet state ( 3 Σ g - The energy of ) will be transferred to ground-state molecular oxygen ( 3 O2). This energy transfer mechanism itself is more selective because it primarily promotes... 1 The formation of O2 occurs without the simultaneous generation of other reactive oxygen species. Therefore, when SiO2 is coated to a certain thickness, the migration of photogenerated carriers (photogenerated electrons or holes) to the surface is effectively suppressed, while maintaining effective energy transfer. This results in ZnO no longer producing H2O2, ·OH, and O2. - Only produces 1 O2.
[0036] For any points not covered above, existing technologies shall apply.
[0037] Although specific embodiments of the present invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art can make various modifications or additions to the described specific embodiments or use similar methods to replace them, without departing from the direction of the invention or exceeding the scope defined by the appended claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc., made to the above embodiments based on the technical essence of the present invention should be included within the protection scope of the present invention.
Claims
1. A zinc oxide-silicon dioxide core-shell nanostructure composite material, characterized in that, The nano zinc oxide particle is taken as a core and a silica layer is taken as a shell, and the thickness of the silica layer is 8-12 nm; and the single state oxygen is generated.
2. The zinc oxide-silicon dioxide core-shell nanostructure composite of claim 1, wherein, The thickness of the silica layer is 8-8.6 nm.
3. The zinc oxide-silicon dioxide core-shell nanostructure composite of claim 1, wherein, The particle size of the nano zinc oxide is 30-100 nm.
4. A method of preparing the zinc oxide-silicon dioxide core-shell nanostructure composite of any one of claims 1-3, characterized by: The method comprises the following steps, (1) dispersing the nano zinc oxide powder in an ethanol aqueous solution, adjusting the pH to 5-7, and obtaining a zinc oxide dispersion system; (2) adding tetraethyl orthosilicate and octadecyl trimethoxysilane into ethanol, stirring uniformly, and obtaining a tetraethyl orthosilicate solution; (3) adding the tetraethyl orthosilicate solution obtained in step (2) into the zinc oxide dispersion system, stirring, centrifuging, collecting the precipitate, washing, and drying, and obtaining a precursor; (4) calcining the precursor obtained in step (3) in air, and obtaining a zinc oxide-silica core-shell nano structure composite material.
5. The production method according to claim 4, characterized by, In step (3), the stirring is performed for 10-15 h.
6. The production method according to claim 4, wherein In step (4), the heating rate is 1.5-3 ℃ / min, and the calcination is performed at 580-700 ℃ for 1.5-3 h.
7. The production method according to claim 4, wherein In step (1), the ethanol aqueous solution is prepared according to a volume ratio of ethanol to deionized water of 3:0.5-1.5 mL, and the mass-volume ratio of the nano zinc oxide to the ethanol aqueous solution is 1 g:3-5 mL; In step (2), the volume ratio of the tetraethyl orthosilicate, the octadecyl trimethoxysilane and the ethanol is 0.15-0.28:0.035-0.06:
2.
8. The production method according to claim 4, characterized by, The ratio of the nano zinc oxide powder to the tetraethyl orthosilicate is 1 g:0.42-0.9 mL.
9. The production method according to claim 4, wherein The preparation method of the nano zinc oxide powder comprises the following steps: S1. adding sodium hydroxide into an ethanol aqueous solution, stirring, and heating to 80-90 ℃ to obtain a solution A; S2. adding zinc acetate and cetyltrimethylammonium bromide into an ethanol aqueous solution, stirring, and heating to 80-90 ℃ to obtain a solution B; S3. quickly adding the solution B into the solution A, reacting at 600-800 rpm for 5-20 min, and quickly centrifuging, and washing with deionized water for 3-4 times to obtain a precipitate; S4. dispersing the precipitate into deionized water, and performing spray drying at 110-125 ℃ to obtain the nano zinc oxide powder.
10. The production method according to claim 9, wherein In steps S1 and S2, the ethanol aqueous solution is prepared according to a volume ratio of ethanol to deionized water of 1:8-10; In the solution A, the concentration of sodium hydroxide is 0.8-1.2 mol / L, in the solution B, the concentration of zinc acetate is 0.4-0.6 mol / L, and the concentration of cetyltrimethylammonium bromide is 2-4 g / L; In step S3, the volume ratio of the solution A to the solution B is 1:1.