Method for optimizing tab slot center coating process
By screening key parameters through single-factor comparative experiments and optimizing the coating process in the tab slot, the problems of slot cleanliness and edge thickness fluctuations were solved, thereby improving battery performance and safety.
Patent Information
- Application Number
- CN202511948112.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-22
- Publication Date
- 2026-03-31
AI Technical Summary
In the existing electrode tray center coating process, the scraping and suction effect is affected by a variety of factors, resulting in poor cleanliness of the tray and fluctuations in edge thickness, which affects battery performance and safety. Furthermore, traditional methods make it difficult to quickly determine the optimal process window.
By selecting battery slurries of different viscosities and setting combinations of coating process parameters, single-factor comparative experiments were conducted to screen out key parameters affecting the cleanliness of the tank and the consistency of edge thickness. The pressure of the scraper, the scraper angle, and the viscosity of the slurry were optimized to formulate a process optimization plan.
Quickly determine the optimal process window, improve the cleanliness and edge thickness consistency of the tab slots, reduce production costs, improve production efficiency, and ensure battery performance and safety.
Smart Images

Figure CN121765949A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating process technology, and in particular to a method for optimizing coating process with tabs placed in the groove. Background Technology
[0002] In recent years, the centrally located tab structure of lithium batteries has become the dominant tab structure in the lithium battery field due to its advantages such as reducing internal resistance, improving rate performance, reducing temperature rise, increasing charging speed and enhancing battery consistency.
[0003] Currently, there are three main methods for preparing the electrode center structure: The first method is laser cleaning, which can precisely remove powder from the coated or rolled electrode sheets. However, it is energy-intensive, costly, and prone to dust splashing. The second method is foaming adhesive process, which involves applying foaming adhesive to the current collector before coating. During baking, the foaming adhesive expands and lifts up the coating. Afterward, the waste is removed. However, this process increases the production steps and has low precision. The third method is scraping process, which involves slitting the coated electrode sheets and scraping out the grooves required for electrode tab welding with a scraping machine. However, this process has problems such as difficulty in removing powder, low yield, and low production efficiency.
[0004] For the coating process, one existing method for fabricating a centrally located tab structure involves precisely creating the tab grooves during the coating process by scraping with a scraper head and using negative pressure suction from a vacuum pump. This method eliminates the need to remove the coating from the substrate surface using lasers or other methods after applying the slurry, thus effectively improving electrode production efficiency and yield, and reducing production costs. However, in this method (or coating process), many factors can affect the scraping effect. Changes in any of these factors can lead to poor cleanliness of the tab grooves and fluctuations in the thickness of the head / tail edges.
[0005] Poor cleanliness of the tab slots can lead to incomplete soldering or sparking during soldering. Incomplete soldering results in unreliable connections, significantly increasing the battery's internal resistance, which in turn exacerbates battery heating and reduces energy efficiency. Large fluctuations in the thickness of the slot edges can cause uneven current distribution, accelerate local aging, affect rate performance and energy efficiency, and cause lithium plating, which in severe cases can lead to short circuits and fires.
[0006] To address these issues, traditional trial-and-error methods or models relying on engineers' experience are insufficient for quickly and scientifically determining the optimal process window, resulting in wasted time and production resources. Therefore, given the current state of the process, there is an urgent need in this field for a highly efficient method to optimize the tab-center coating process, thereby promoting the engineering development of tab-center coating technology. Summary of the Invention
[0007] The purpose of this invention is to provide a method for optimizing the coating process in the tab groove, so as to solve or at least partially solve the technical problems mentioned in the background art.
[0008] To achieve this objective, the present invention adopts the following technical solution: This invention provides a method for optimizing the coating process in the tab groove, comprising: Several battery slurries with different viscosities were selected as test slurries, and a set of stable coating process parameter combinations was set for each test slurry as a control group; wherein, the coating process parameter combination includes several key parameters that affect or potentially affect the quality of the tank, including coating surface density, doctor blade material, doctor blade angle, negative pressure suction, doctor blade downward pressure and foil conveyor tension; Based on the control groups of each experimental slurry, corresponding single-factor control experimental groups were established; among them, the established single-factor control experimental groups covered all changes in key parameters. For each test slurry, the coating process parameter combination of its corresponding single-factor control test group was used to conduct the electrode groove center coating process test. Based on the experimental data, key parameters affecting the cleanliness of the tank and key parameters affecting the consistency of the thickness at the tank edge were selected.
[0009] Optionally, the test data includes the residual slurry thickness T, the thickness difference H1 between the head edge and the normal head area of the tank, the thickness difference H2 between the tail edge and the normal tail area of the tank, the head edge range H3, and the tail edge range H4. The method for collecting the experimental data is as follows: Use a micrometer to measure the residual slurry thickness T in each tank area; For each slot area on the electrode, the coating areas on both sides of the slot are arranged sequentially from head to tail as follows: normal coating area at the head of the slot, data acquisition area at the edge of the head of the slot, uncontrolled area at the edge of the head of the slot, uncontrolled area at the edge of the tail of the slot, data acquisition area at the edge of the tail of the slot, and normal coating area at the tail of the slot. The head and tail sides of the uncontrolled area at the edge of the head of the slot are adjacent to the data acquisition area at the edge of the head of the slot and the slot area, respectively. The head and tail sides of the uncontrolled area at the edge of the tail of the slot are adjacent to the slot area and the data acquisition area at the edge of the tail of the slot, respectively. For the i-th slot region on the electrode, the slurry thickness at multiple first acquisition points is uniformly collected in the data acquisition area at the corresponding slot head edge. The maximum value of the slurry thickness at the multiple first acquisition points is denoted as A. imax The minimum value is A imin The mean is A iaveThe slurry thickness at multiple second sampling points is uniformly collected in the normal coating area at the corresponding tank head, and the average slurry thickness at the multiple second sampling points is recorded as B. iave The slurry thickness at multiple third acquisition points is uniformly collected in the data acquisition area at the tail edge of the corresponding tank position. The maximum value of the slurry thickness collected at the multiple third acquisition points is recorded as C. imax The minimum value is C imin The mean is C iave The slurry thickness at multiple fourth sampling points is uniformly collected at the tail end of the corresponding tank in the normal coating area, and the average slurry thickness at the multiple fourth sampling points is recorded as D. iave ; The formulas for calculating H1, H2, H3, and H4 are as follows: , , , ; Where n is the total number of slot regions 1 on the electrode.
[0010] Optionally, a corresponding single-factor control experimental group is established based on the control group of each test slurry, and the method is as follows: Each time a key parameter in the control group of the test slurry is changed individually, it is necessary to go through all the changes of key parameters to obtain multiple test groups; the test group is the combination of coating process parameters obtained after changing one key parameter in the control group individually. The control group and the experimental group of the test slurry were numbered and designated as the single-factor control experimental group.
[0011] Optionally, for each test slurry, the coating process parameter combination of its corresponding single-factor control test group is used to conduct the electrode groove center coating process test, specifically including: The test slurry was used to conduct coating process tests in the tab groove according to the coating process parameter combination corresponding to the single factor control test group. The equipment status and environmental conditions must be stable or consistent during each test. After each experiment, the average residual slurry thickness T in all slot areas on the electrode was measured and calculated. ave The values of H1, H2, H3, and H4 were recorded as experimental data.
[0012] Optionally, the step of screening key parameters affecting the cleanliness of the tank and key parameters affecting the consistency of the tank edge thickness based on experimental data specifically includes: Based on the average residual thickness T of multiple slurry values obtained from the single-factor control test group, avePlot the T-value, H1-value, H2-value, H3-value, and H4-value statistical charts respectively. The key parameters affecting the cleanliness of the tank were determined by plotting the T-value statistical chart; By drawing statistical charts of H1, H2, H3, and H4 values, the key parameters affecting the consistency of groove edge thickness were determined.
[0013] Optionally, after selecting several battery slurries of different viscosities as test slurries and setting a set of stable coating process parameter combinations for each test slurry as a control group, the method further includes: Set quality objectives for process optimization; these include quality objectives for tank cleanliness and quality objectives for uniform thickness at tank edges. The quality target for tank cleanliness is: the residual slurry thickness T in the tank is less than or equal to the predetermined thickness threshold; The quality target for the uniformity of the groove edge thickness is: H1 and H2 are both within the predetermined thickness difference range, H3 is less than or equal to the predetermined first range threshold, and H4 is less than or equal to the predetermined second range threshold.
[0014] Optionally, the scraper pressure and scraper angle are key parameters affecting the cleanliness of the tank; the viscosity of the slurry is a key parameter affecting the uniformity of the thickness at the head edge of the tank; and the negative pressure suction and scraper angle are key parameters affecting the uniformity of the thickness at the tail edge of the tank. After identifying the key parameters affecting the cleanliness of the tank and the key parameters affecting the consistency of the tank edge thickness based on experimental data, the process also includes: When the cleanliness of the electrode slot after completing the electrode tab center coating process does not meet the set quality target, the coating process can be optimized by increasing the doctor blade pressure / doctor blade angle; and / or, When the thickness uniformity at the edge of the electrode head after the electrode tab center coating process fails to meet the set quality target, the coating process is optimized by increasing the viscosity of the battery slurry; and / or, When the thickness consistency at the tail edge of the electrode after the electrode tab center coating process does not meet the set quality target, the coating process can be optimized by increasing the scraper angle and / or reducing the negative pressure suction within the predetermined negative pressure suction range.
[0015] Optionally, the distance between the normal coating area at the head of the tank and the data acquisition area at the edge of the head of the tank, and the distance between the data acquisition area at the edge of the tail of the tank and the normal coating area at the tail of the tank, are both greater than 10 mm. The width of the uncontrolled area at the head edge and the width of the uncontrolled area at the tail edge of the slot are both 2mm, and the width of the data acquisition area at the head edge and the width of the data acquisition area at the tail edge of the slot are both greater than or equal to 5mm.
[0016] Optionally, the thickness threshold is 1 μm, the first range threshold is 3 μm, and the second range threshold is 10 μm; The thickness difference of the negative electrode slurry ranges from -3μm to 7μm, and the thickness difference of the positive electrode slurry ranges from -7μm to 3μm.
[0017] Optionally, the selected test slurries include multiple positive electrode slurries of different viscosities and multiple negative electrode slurries of different viscosities.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention screens out key parameters affecting tank cleanliness and tank edge thickness consistency through single-factor control experiments, providing a scientific basis for process optimization, facilitating rapid determination of the optimal process window, and promoting the engineering application and development of tab-centered coating. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 A flowchart illustrating a method for optimizing the coating process in the tab groove, as provided in an embodiment of the present invention.
[0021] Figure 2 This is a schematic diagram of the structure of an electrode sheet after the electrode tab groove center coating process is completed, as provided in an embodiment of the present invention.
[0022] Figure 3 A statistical chart of T-values for a single-factor controlled trial provided in an embodiment of the present invention.
[0023] Figure 4a A statistical chart of H1 values for a single-factor controlled trial provided in an embodiment of the present invention.
[0024] Figure 4b A statistical chart of H2 values for a single-factor controlled trial provided in an embodiment of the present invention.
[0025] Figure 5a A statistical chart of H3 values for a single-factor controlled trial provided in an embodiment of the present invention.
[0026] Figure 5b A statistical chart of H4 values for a single-factor controlled trial provided in an embodiment of the present invention.
[0027] In the picture: 1. Tank area; 2. Coating area; 21. Uncontrolled area at the head edge of the tank; 22. Data acquisition area at the head edge of the tank; 23. Normal coating area at the head of the tank; 24. Uncontrolled area at the tail edge of the tank; 25. Data acquisition area at the tail edge of the tank; 26. Normal coating area at the tail of the tank. Detailed Implementation
[0028] To make the objectives, features, and advantages of this invention more apparent and understandable, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the embodiments described below are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0029] Example 1: Please refer to Figure 1 , Figure 1 A flowchart illustrating a method for optimizing a coating process in a tab groove, as provided in this embodiment of the invention, is shown below. The method specifically includes: Step 100: Select several battery slurries with different viscosities as test slurries, and set a set of stable coating process parameters for each test slurry as a control group.
[0030] This step is a pre-set step. The selected test slurry must include multiple positive electrode slurries and multiple negative electrode slurries with different viscosities.
[0031] This embodiment will use two representative negative electrode slurries (the two negative electrode slurries have viscosities of 2500 mPa·s and 5000 mPa·s, respectively, and solid contents of 40% and 50%, respectively, and are named slurry 1 and slurry 2, respectively) as examples to illustrate the method in detail.
[0032] Based on process principles and experience, N key parameters with significant potential impact on tank quality were selected, including but not limited to: slurry surface density, scraper material, scraper slot depth, contact angle between the scraper and the electrode (scraper angle) and downward pressure, negative pressure suction magnitude, foil conveying speed, and foil tension. Two engineering-significant levels (e.g., high level H and low level L) were determined for each factor to be investigated.
[0033] Step 110: Based on the control groups of each experimental slurry, corresponding single-factor control experimental groups are established.
[0034] The implementation method for step 110 is as follows: This embodiment uses the two test slurries mentioned above as a benchmark and sets up two series of studies, A (corresponding to slurry 1) and B (corresponding to slurry 2); Each time a key parameter in the control group of the test slurry (i.e., slurry 1 and slurry 2) is changed individually, it is necessary to go through all the changes of key parameters to obtain multiple test groups; the test group is the combination of coating process parameters obtained after changing one key parameter in the control group individually. The control and experimental groups of the test slurry were numbered separately and designated as single-factor control experimental groups.
[0035] like Figure 3 As shown, series A is numbered A1-A8, and series B is numbered B1-B9, where A1 and B1 are control groups. The established single-factor controlled experimental groups are shown in Table 1 and Table 2, respectively: Table 1 Table 2 Step 120: For each test slurry, the coating process parameter combination of its corresponding single-factor control test group was used to conduct the electrode groove center coating process test.
[0036] The specific implementation method of step 120 is as follows: The experimental slurry was used to conduct coating process tests in the tab groove according to the coating process parameter combination corresponding to the single factor control test group. The equipment status and environmental conditions must be stable or consistent during each test. After each experiment, the average thickness T of the residual slurry in all slot regions 1 on the electrode was measured and calculated. ave The values of H1, H2, H3, and H4 were recorded as experimental data; among them, T ave H1 is the average thickness T of the slurry residue in all slot areas 1 on electrode 1, H2 is the thickness difference between the head edge and the normal head area of the slot, H3 is the thickness difference between the tail edge and the normal tail area of the slot, and H4 is the thickness difference between the head edge and the tail edge.
[0037] It should be noted that since the 1-2mm range at the beginning / end edge of the slot can be covered with insulating adhesive during the subsequent tab manufacturing process and will not affect the overall quality of the battery, this area is designated as the uncontrolled area 21 at the beginning edge of the slot and the uncontrolled area 24 at the end edge of the slot. The optimization method in this embodiment mainly targets the thickness within the 3-7mm range at the beginning / end edge of the slot, that is, the data acquisition area 22 at the beginning edge of the slot and the data acquisition area 25 at the end edge of the slot.
[0038] It should be noted that in this embodiment, "head side" refers to... Figure 2 The upper side, "tail side" refers to Figure 2 The lower side.
[0039] Specifically, the experimental data collection method is as follows: like Figure 2 As shown, for each slot area 1 on the electrode, its corresponding coating area 2 is provided with the following from beginning to end: normal coating area 23 at the head of the slot, data acquisition area 22 at the edge of the head of the slot, uncontrolled area 21 at the edge of the head of the slot, uncontrolled area 24 at the edge of the tail of the slot, data acquisition area 25 at the edge of the tail of the slot, and normal coating area 26 at the tail of the slot. The head and tail sides of the uncontrolled area 21 at the head of the slot are adjacent to the data acquisition area 22 at the edge of the head of the slot and the slot area 1, respectively. The head and tail sides of the uncontrolled area 24 at the tail of the slot are adjacent to the slot area 1 and the data acquisition area 25 at the edge of the tail of the slot, respectively. For the i-th slot region 1 on the electrode, the slurry thickness of multiple first acquisition points (5 points are collected horizontally every 1 mm within a range of 3-7 mm from slot region 1, for a total of 25 points) are uniformly collected in the data acquisition area 22 at the edge of the corresponding slot head. The maximum value of the slurry thickness among the multiple first acquisition points is recorded as A. imax The minimum value is A imin The mean is A iave ; In the normal coating area 23 at the corresponding tank head, multiple second sampling points (within a range of 3-7 mm from tank area 1, 5 points are collected horizontally every 1 mm, for a total of 25 points) are evenly collected to measure the slurry thickness. The average slurry thickness of the multiple second sampling points is recorded as B. iave The slurry thickness is uniformly collected from multiple third collection points (10 points laterally) at the edge of the corresponding tank tail. The maximum value of the slurry thickness collected from the multiple third collection points is recorded as C. imax The minimum value is C imin The mean is C iave The slurry thickness at multiple fourth sampling points (10 points laterally) is uniformly collected at the normal coating area 26 at the tail of the corresponding tank. The average slurry thickness collected at the multiple fourth sampling points is recorded as D. iave ; The formulas for calculating H1, H2, H3, and H4 are as follows: , , , ; Where n is the total number of slot regions 1 on the electrode.
[0040] In this embodiment, the distance between the normal coating area 23 at the head of the slot and the data acquisition area 22 at the edge of the head of the slot, as well as the distance between the data acquisition area 25 at the edge of the tail of the slot and the normal coating area 26 at the tail of the slot, are all greater than 10mm. The width of the uncontrolled area 21 at the head edge of the slot and the width of the uncontrolled area 24 at the tail edge of the slot are both 2mm, and the width of the data acquisition area 22 at the head edge of the slot and the width of the data acquisition area 25 at the tail edge of the slot are both greater than or equal to 5mm.
[0041] The cleanliness of the tank is determined by the absence of obvious slurry residue visible to the naked eye, and the thickness of the slurry residue in the tank is used as the core indicator, with a residue thickness T≤1μm.
[0042] Specifically, preliminary visual inspection revealed no obvious slurry residue in the tanks of each group. A micrometer was used to measure the slurry residue thickness in area 1 of each group, and statistical analysis was performed to obtain the final thickness. Figure 3 .
[0043] Step 130: Based on the experimental data, screen out the key parameters that affect the cleanliness of the tank and the key parameters that affect the consistency of the thickness at the edge of the tank.
[0044] Specifically, step 130 includes: The mean T values of multiple slurry residual thicknesses obtained from the single-factor control experimental group were... ave Plot T-value statistics for H1, H2, H3, and H4 values respectively (e.g., Figure 3 As shown), H1 value statistics chart (as shown) Figure 4a As shown), H2 value statistics chart (as shown) Figure 4b As shown), H3 value statistics chart (as shown) Figure 5a (as shown) and H4 value statistics chart (as shown) Figure 5b (as shown) The key parameters affecting the cleanliness of the tank were determined by plotting the T-value statistical chart; By drawing statistical charts of H1, H2, H3, and H4 values, the key parameters affecting the consistency of groove edge thickness were determined.
[0045] from Figure 3 As can be seen, the residual slurry thickness in tank area 1 of each group is less than 1μm, indicating that the provided electrode-center coating process can achieve relatively clean scraping and suction in the tank. However, it can be clearly seen that the residual slurry thickness in tank area 1 of groups A4, A6, A7, B6, B7 and B9 is significantly lower than that of other groups. These groups correspond to increasing the downward pressure of the scraper and increasing the scraper angle. Therefore, the verification shows that the greater downward pressure and the larger scraper angle are the key to further improving the cleaning effect of scraping and suction.
[0046] From Figure 4, we can deduce four conclusions: (1) such as Figure 4a As shown, the values of groups B1 to B9 are significantly lower than those of groups A1 to A8, and group B corresponds to high viscosity slurry; it can be seen that high viscosity is the key to the stability of the edge of the tank head.
[0047] (2) Figure 4b In the study, both groups A3 and B3 reduced the negative pressure suction, and the results were low. This indicates that moderately reducing the suction can stabilize the thickness at the tail edge. The reason should be that it reduces the "suction disturbance" during scraping, because excessive suction will interfere with the normal separation of slurry at the boundary and cause thickness fluctuations.
[0048] (3) Figure 4b Among them, the values of groups A6, A7, B6, B7, and B9 are significantly lower than those of the other groups, corresponding to an increase in the scraper angle. Increasing the angle changes the contact between the scraper and the coating from "vertical impact" to "sliding shearing", reducing "squeezing and accumulation" at the front end. The slurry is smoothly guided away from the scraping area, avoiding accumulation or stringing at the end position due to poor flow, resulting in a more stable thickness.
[0049] (4) Comparison Figure 4b In groups B1 and B2: B2, due to its higher areal density, exhibited poorer consistency in the thickness of its tail edge, resulting in a greater thickness difference compared to the normal area; B9, by simply increasing the scraper angle, yielded significantly better results than B2. This verifies that the instability in the thickness of the head and tail edges caused by areal density can be effectively corrected by adjusting the scraper angle.
[0050] The results obtained in Figure 5 are consistent with the analysis results in Figure 4, as follows: Depend on Figure 5a Similarly, it can be seen that the thickness range of the tank head edge is smaller in groups B1 to B9, which once again verifies that high viscosity slurry can stabilize the thickness of the tank head edge, reduce its range, and slow down the fluctuation. Figure 5b The tail edge thickness range of groups A3, A6, A7, B3, B6, B7, and B9 was also significantly lower than other values, further confirming that appropriately reducing the negative pressure suction and increasing the scraper angle can make the tail edge thickness more stable and greatly reduce the fluctuation. This is consistent with... Figure 4b The results are consistent.
[0051] Through the above experiments, it was determined that the factors with the greatest impact on the cleanliness of the tank were the scraper pressure and the scraper angle. When there is a lot of slurry residue, increasing the scraper pressure and raising the scraper angle can further reduce the thickness of the slurry residue in the tank.
[0052] High slurry viscosity is key to the stability and consistency of the thickness at the head edge of the tank. Increasing the slurry viscosity helps to reduce fluctuations in the head edge area. Appropriately reducing the negative pressure suction or increasing the scraper angle can stabilize the thickness at the tail edge of the tank and optimize consistency.
[0053] Furthermore, the method for optimizing the coating process in the tab groove also includes: Step 140: Set quality objectives for process optimization.
[0054] Among them, the quality objectives of process optimization include the quality objective of tank cleanliness and the quality objective of uniform thickness at the tank edge; The quality target for tank cleanliness is: the residual slurry thickness T in the tank is less than or equal to the predetermined thickness threshold; The quality target for the uniformity of the groove edge thickness is: H1 and H2 are both within the predetermined thickness difference range, H3 is less than or equal to the predetermined first range threshold, and H4 is less than or equal to the predetermined second range threshold.
[0055] Specifically, in this embodiment, the thickness threshold is 1 μm, the first range threshold is 3 μm, and the second range threshold is 10 μm; The thickness difference of the negative electrode slurry ranges from -3μm to 7μm, and the thickness difference of the positive electrode slurry ranges from -7μm to 3μm.
[0056] After step 140, the following also includes: Step 150: Determine whether the quality of the electrode sheet after completing the coating process in the tab groove meets the set quality target; if yes, determine that the quality of the electrode sheet is qualified; if not, proceed to step 151.
[0057] Step 151: Adjust the key parameters that affect the cleanliness of the tank and / or the key parameters that affect the thickness consistency of the tank edge to ensure that the quality of the electrode sheet meets the set quality target.
[0058] Step 151 specifically includes: Step 1511: When the cleanliness of the electrode slot after completing the electrode tab center coating process does not meet the set quality target, optimize the coating process by increasing the doctor blade pressure / doctor blade angle; and / or, Step 1512: When the thickness consistency of the electrode head edge after completing the electrode tab center coating process does not meet the set quality target, the coating process is optimized by increasing the viscosity of the battery slurry; and / or, Step 1513: When the thickness consistency of the tail edge of the electrode after the electrode tab center coating process is not met, the coating process is optimized by increasing the scraper angle and / or reducing the negative pressure suction within the predetermined negative pressure suction range.
[0059] It should be noted that the execution order of some steps in the method for optimizing the coating process in the tab groove provided in this embodiment can be changed according to actual needs. For example, step 140 can be executed after step 130 or before step 100. Both can achieve the method for optimizing the coating process in the tab groove provided in this embodiment.
[0060] In summary, this embodiment provides a method for optimizing the electrode tray center coating process of lithium-ion batteries based on the single-factor comparison method. The aim is to systematically evaluate the independent impact of each process parameter on the tray quality (cleanliness, edge thickness consistency) with minimal number of experiments, quickly identify key parameters and their reasonable ranges, solve the problem of low parameter optimization efficiency in existing technologies, and screen out the main factors affecting the quality of the tray edge. This facilitates the rapid determination of the optimal process window and promotes the engineering application and development of the electrode tray center coating process.
[0061] Those skilled in the art will understand that all or part of the steps of the above embodiments can be implemented by hardware, or by a program instructing related hardware. The program can be stored in a computer-readable storage medium, such as a read-only memory, a disk, or an optical disk. Based on this understanding, the technical solution of the present invention, or the part that contributes to the prior art, or all or part of the technical solution, can be embodied in the form of a software product. This computer software product is stored in a storage medium and includes several instructions to cause a computer device (which may be a personal computer, a server, or a network device, etc.) to execute all or part of the steps of the methods described in the various embodiments of the present invention. The aforementioned storage medium includes various media capable of storing program code, such as a USB flash drive, a portable hard drive, a read-only memory (ROM), a random access memory (RAM), a magnetic disk, or an optical disk.
[0062] The above-described embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for optimizing the coating process in the tab groove, characterized in that, include: Several battery slurries with different viscosities were selected as test slurries, and a set of stable coating process parameter combinations was set for each test slurry as a control group; wherein, the coating process parameter combination includes several key parameters that affect or potentially affect the quality of the tank, including coating surface density, doctor blade material, doctor blade angle, negative pressure suction, doctor blade downward pressure and foil conveyor tension; Based on the control groups of each experimental slurry, corresponding single-factor control experimental groups were established; among them, the established single-factor control experimental groups covered all changes in key parameters. For each test slurry, the coating process parameter combination of its corresponding single-factor control test group was used to conduct the electrode groove center coating process test. Based on the experimental data, key parameters affecting the cleanliness of the tank and key parameters affecting the consistency of the thickness at the tank edge were selected.
2. The method for optimizing the coating process in the tab groove according to claim 1, characterized in that, The test data include the residual slurry thickness T, the thickness difference H1 between the head edge and the normal head area of the tank, the thickness difference H2 between the tail edge and the normal tail area of the tank, the head edge range H3, and the tail edge range H4. The method for collecting the experimental data is as follows: Use a micrometer to measure the residual slurry thickness T in each tank area; For each slot area on the electrode, the coating areas on both sides of the slot are arranged sequentially from head to tail as follows: normal coating area at the head of the slot, data acquisition area at the edge of the head of the slot, uncontrolled area at the edge of the head of the slot, uncontrolled area at the edge of the tail of the slot, data acquisition area at the edge of the tail of the slot, and normal coating area at the tail of the slot. The head and tail sides of the uncontrolled area at the edge of the head of the slot are adjacent to the data acquisition area at the edge of the head of the slot and the slot area, respectively. The head and tail sides of the uncontrolled area at the edge of the tail of the slot are adjacent to the slot area and the data acquisition area at the edge of the tail of the slot, respectively. For the i-th slot region on the electrode, the slurry thickness at multiple first acquisition points is uniformly collected in the data acquisition area at the corresponding slot head edge. The maximum value of the slurry thickness at the multiple first acquisition points is denoted as A. imax The minimum value is A imin The mean is A iave The slurry thickness at multiple second sampling points is uniformly collected in the normal coating area at the corresponding tank head, and the average slurry thickness at the multiple second sampling points is recorded as B. iave The slurry thickness at multiple third acquisition points is uniformly collected in the data acquisition area at the tail edge of the corresponding tank position. The maximum value of the slurry thickness collected at the multiple third acquisition points is recorded as C. imax The minimum value is C imin The mean is C iave The slurry thickness at multiple fourth sampling points is uniformly collected at the tail end of the corresponding tank in the normal coating area, and the average slurry thickness at the multiple fourth sampling points is recorded as D. iave ; The formulas for calculating H1, H2, H3, and H4 are as follows: , , , ; Where n is the total number of slot regions 1 on the electrode.
3. The method for optimizing the coating process in the tab groove according to claim 2, characterized in that, The control groups for each experimental slurry were respectively established into corresponding single-factor control experimental groups, and the method was as follows: Each time a key parameter in the control group of the test slurry is changed individually, it is necessary to go through all the changes of key parameters to obtain multiple test groups; the test group is the combination of coating process parameters obtained after changing one key parameter in the control group individually. The control group and the experimental group of the test slurry were numbered and designated as the single-factor control experimental group.
4. The method for optimizing the coating process in the tab groove according to claim 3, characterized in that, For each test slurry, the coating process parameter combination of its corresponding single-factor control test group was used to conduct the electrode groove center coating process test, specifically including: The test slurry was used to conduct coating process tests in the tab groove according to the coating process parameter combination corresponding to the single factor control test group. The equipment status and environmental conditions must be stable or consistent during each test. After each experiment, the average residual slurry thickness T in all slot areas on the electrode was measured and calculated. ave The values of H1, H2, H3, and H4 were recorded as experimental data.
5. The method for optimizing the coating process in the tab groove according to claim 4, characterized in that, The key parameters affecting the cleanliness of the tank and the key parameters affecting the consistency of the tank edge thickness were selected based on experimental data, specifically including: Based on the average residual thickness T of multiple slurry values obtained from the single-factor control test group, ave Plot the T-value, H1-value, H2-value, H3-value, and H4-value statistical charts respectively. The key parameters affecting the cleanliness of the tank were determined by plotting the T-value statistical chart; By drawing statistical charts of H1, H2, H3, and H4 values, the key parameters affecting the consistency of groove edge thickness were determined.
6. The method for optimizing the coating process in the tab groove according to claim 5, characterized in that, After selecting several battery slurries of different viscosities as test slurries, and setting a set of stable coating process parameter combinations for each test slurry as a control group, the process further includes: Set quality objectives for process optimization; these include quality objectives for tank cleanliness and quality objectives for uniform thickness at tank edges. The quality target for tank cleanliness is: the residual slurry thickness T in the tank is less than or equal to the predetermined thickness threshold; The quality target for the uniformity of the groove edge thickness is: H1 and H2 are both within the predetermined thickness difference range, H3 is less than or equal to the predetermined first range threshold, and H4 is less than or equal to the predetermined second range threshold.
7. The method for optimizing the coating process in the tab groove according to claim 6, characterized in that, The downward pressure and angle of the scraper are key parameters affecting the cleanliness of the tank; the viscosity of the slurry is a key parameter affecting the consistency of the thickness at the head edge of the tank; the negative pressure suction and the scraper angle are key parameters affecting the consistency of the thickness at the tail edge of the tank. After identifying the key parameters affecting the cleanliness of the tank and the key parameters affecting the consistency of the tank edge thickness based on experimental data, the process also includes: When the cleanliness of the electrode slot after completing the electrode tab center coating process does not meet the set quality target, the coating process can be optimized by increasing the doctor blade pressure / doctor blade angle; and / or, When the thickness uniformity at the edge of the electrode head after the electrode tab center coating process fails to meet the set quality target, the coating process is optimized by increasing the viscosity of the battery slurry; and / or, When the thickness consistency at the tail edge of the electrode after the electrode tab center coating process does not meet the set quality target, the coating process can be optimized by increasing the scraper angle and / or reducing the negative pressure suction within the predetermined negative pressure suction range.
8. The method for optimizing the coating process in the tab groove according to claim 7, characterized in that, The distance between the normal coating area at the head of the tank and the data acquisition area at the edge of the head of the tank, as well as the distance between the data acquisition area at the edge of the tail of the tank and the normal coating area at the tail of the tank, are all greater than 10mm. The width of the uncontrolled area at the head edge and the width of the uncontrolled area at the tail edge of the slot are both 2mm, and the width of the data acquisition area at the head edge and the width of the data acquisition area at the tail edge of the slot are both greater than or equal to 5mm.
9. The method for optimizing the coating process in the tab groove according to claim 8, characterized in that, The thickness threshold is 1 μm, the first range threshold is 3 μm, and the second range threshold is 10 μm; The thickness difference of the negative electrode slurry ranges from -3μm to 7μm, and the thickness difference of the positive electrode slurry ranges from -7μm to 3μm.
10. The method for optimizing the coating process in the tab groove according to claim 1, characterized in that, The selected test slurries included multiple positive electrode slurries of different viscosities and multiple negative electrode slurries of different viscosities.