Continuous and pulse coaxial double-beam welding method for sheet titanium alloy corner joint process

By employing a coaxial dual-beam welding method combining continuous laser and pulsed laser, precise control of heat input for corner joint welding of thin-plate titanium alloys was achieved, solving the problems of welding deformation and residual stress control, and obtaining high-quality welded joints.

CN122033439APending Publication Date: 2026-05-15DALIAN UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202610448138.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-07
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

Existing technologies make it difficult to precisely and flexibly control the heat input in the corner joint welding of thin-plate titanium alloys, resulting in difficulty in controlling welding deformation and residual stress.

Method used

A coaxial dual-beam welding method using continuous lasers and pulsed lasers with similar wavelengths that completely overlap in space is employed. By adjusting the energy ratio and defocus ratio, the distribution gradient of the welding heat input can be actively controlled.

Benefits of technology

It effectively reduces residual stress and deformation during welding, ensuring the mechanical properties of the welded joint and meeting engineering application requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122033439A_ABST
    Figure CN122033439A_ABST
Patent Text Reader

Abstract

The invention provides a continuous and pulse coaxial double-beam welding method for a sheet titanium alloy corner joint process, and belongs to the technical field of laser welding. According to the method, continuous laser and pulse laser are adopted, coincidence arrangement of the two laser beams in space is achieved through a coaxial composite optical system to form a composite laser beam, the composite laser beam acts on a sheet titanium alloy corner joint assembled and fixed through a corner joint clamp, and the welding process is completed. The two laser beams are similar in wavelength, optical compatibility is good, and an optical system is stable. The coaxial composite heat source has the characteristics that the energy distribution gradient can be regulated and controlled, and the heat input is accurately controlled, so that the welding heat input can be effectively reduced while the mechanical property of the joint is ensured, and the residual stress is reduced to control the welding deformation. The sheet titanium alloy corner joint obtained through the method has the advantages of being uniform in welding seam forming, little in splashing, small in deformation and the like, and the technological requirements of the aerospace field for high-quality thin-wall titanium alloy structural parts are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal laser welding methods, and more particularly to a continuous and pulsed coaxial dual-beam welding method for corner jointing of thin titanium alloy plates. Background Technology

[0002] Titanium alloys are widely used in aerospace, shipbuilding, and chemical equipment industries due to their excellent specific strength, corrosion resistance, and high-temperature performance. Among these applications, the corner joint welding of thin-plate titanium alloy structural components is a critical technical step in the manufacturing process. However, thin-plate titanium alloys are extremely sensitive to welding heat input: insufficient heat input easily leads to defects such as incomplete penetration and poor fusion; excessive heat input causes a large temperature gradient and thermal stress concentration, resulting in significant residual stress and welding deformation in the joint area, severely affecting the dimensional accuracy and service performance of the structural components.

[0003] Laser welding, as a high-energy-density welding method, achieves rapid melting and solidification of materials by concentrating energy and applying it instantaneously to the weld area. It boasts advantages such as a narrow heat-affected zone, high welding speed, and minimal deformation, and is considered an effective way to solve the aforementioned problems. To further improve welding quality and process adaptability, dual-beam laser welding technology has gradually developed.

[0004] Chinese patent CN114669873A discloses a high-power fiber laser dual-gun symmetrical welding method for medium-thick plate titanium alloy T-joints. This method uses a high-power fiber laser with two guns to symmetrically weld medium-thick plate marine titanium alloy T-joints, achieving double-sided one-time penetration welding of marine titanium alloy T-joints with thicknesses ranging from 6mm to 20mm. However, this invention is still limited in the welding process of thin-plate titanium alloys. Chinese patent CN113182689A discloses a welding method for titanium alloy corner joints based on a dual-beam laser. This technical solution uses two beams distributed front-to-back along the welding path: the front laser beam uses high power for deep penetration welding to ensure root penetration, while the rear laser beam uses lower power pulse output for heat conduction welding to melt the welding wire, meeting the weld leg size requirements. Although it achieves one-time welding of the corner joint, the separate heat source layout causes the two laser beams to act on the molten pool at different times and in different areas, making synchronous energy control of the same molten pool area impossible. This limits the control effect on residual stress and deformation of thin-plate structures under thermal cycling.

[0005] Another Chinese patent, CN111940905A, discloses a coaxial dual-focal-length laser wire-filling welding method for both sides of a thin-plate titanium alloy T-joint. This method utilizes a coaxial dual-focal-length lens to generate long and short focal-length lasers, respectively achieving deep penetration welding and heat-conducting welding modes. Although called coaxial, the two laser beams form two overlapping spots on the workpiece surface due to their different focal lengths, with energy distributed in a ring shape in space, failing to achieve true spatial overlap. This design primarily utilizes the large spot size of the short-focal-length laser to reduce the accuracy requirements of the wire feeding position, without addressing the active control of the molten pool's internal flowability and keyhole stability, and further without mentioning controlling the heat input distribution through energy ratio to reduce residual stress.

[0006] Furthermore, Chinese patent CN109604831A discloses a laser-TIG hybrid welding process, which employs an ultra-high frequency pulsed TIG welding torch in front and a laser behind, utilizing the electromagnetic stirring effect of the TIG arc to improve the undercut problem. However, this solution introduces an arc as a second heat source, significantly increasing the heat input. Moreover, the mechanisms of action of the arc and the laser are different, making it difficult to achieve precise heat input control, and thus unsuitable for thin-plate titanium alloy corner joint structures that are highly sensitive to heat input.

[0007] Therefore, there is an urgent need for a welding method that can precisely and flexibly control the welding heat input, so as to effectively reduce the residual stress and welding deformation generated by welding thin-plate titanium alloy corner joints while ensuring the mechanical properties of the joint. Summary of the Invention

[0008] In view of this, the purpose of the present invention is to provide a continuous and pulsed coaxial dual-beam welding method for corner joints of thin titanium alloy plates. By completely overlapping continuous lasers and pulsed lasers with similar wavelengths in space and coordinating their energy ratio and defocus ratio, the active control of the welding heat input distribution gradient is achieved, thereby solving the technical problem of difficult deformation and stress control in corner joint welding of thin titanium alloy plates.

[0009] The technical means employed in this invention are as follows:

[0010] A continuous and pulsed coaxial dual-beam welding method for corner jointing of thin titanium alloy sheets includes the following steps: A first laser beam and a second laser beam with similar wavelengths are coupled into a composite laser beam that is completely overlapped in space through a coaxial composite optical system. The laser irradiates the weld area of ​​the thin titanium alloy corner joint to be welded. After the material melts and forms a molten pool, the laser directly acts on the molten pool area. By adjusting the energy ratio of the first laser beam and the second laser beam, the distribution gradient of welding heat input in the molten pool is controlled, thereby reducing welding residual stress and deformation angle.

[0011] Furthermore, the first laser beam is a continuous laser, used to provide the basic heat input to maintain the stability of the molten pool; the second laser beam is a pulsed laser, which injects periodic energy into the molten pool through its high frequency and high peak power to induce forced convection and enhance the stability of the keyhole.

[0012] Furthermore, the coaxial composite optical system includes at least one dichroic mirror, which has high transmission for the first wavelength laser and high reflection for the second wavelength laser, or vice versa, so as to achieve optical path overlap of the two laser beams.

[0013] Furthermore, it also includes the steps of grinding the workpiece to be welded to remove surface oil and oxide layer before welding, and assembling and fixing the titanium alloy corner joint components to be welded using corner joint clamps.

[0014] Furthermore, the energy ratio is controlled by adjusting the ratio of the average power P1 of the continuous laser to the average power P2 of the pulsed laser, and the ratio satisfies: 3≤P1 / P2≤5.5.

[0015] Furthermore, it also includes adjusting the ratio of the defocusing amount Δf1 of the continuous laser to the defocusing amount Δf2 of the pulsed laser to control the energy distribution of the composite laser beam in the direction of the molten pool depth, and the ratio satisfies: 0.5≤Δf1 / Δf2≤2.

[0016] Furthermore, the pulse width τ and frequency f of the pulsed laser are adjustable to match different welding speeds v1 and wire feed speeds v2, thereby controlling the solidification process of the molten pool. Specifically, the pulsed laser frequency f is set to 20Hz~50Hz, the pulse width τ is set to 4ms~8ms, the welding speed v1 is 600mm / min~1400mm / min, and the wire feed speed v2 is 1500mm / min~2100mm / min.

[0017] Furthermore, the wavelength of the first laser beam is 1070 nm, and the wavelength of the second laser beam is 1064 nm.

[0018] Compared with the prior art, the present invention has the following advantages: 1. This invention completely overlaps continuous laser and pulsed laser in space, allowing the energy of both laser beams to act on the molten pool simultaneously and at the same point. This is fundamentally different from the heat source layouts in existing technologies that are separated front and back or arranged inside and outside. Spatial overlap ensures the superposition effect of the two energies, laying the foundation for subsequent coordinated control. This allows stable heat sources and disturbed heat sources to function simultaneously in the same molten pool area, achieving flexible and adjustable heat sources.

[0019] 2. In this invention, continuous laser provides a stable and continuous base heat input, maintaining the stability of the keyhole and molten pool, and preventing spatter and collapse caused by drastic energy fluctuations; pulsed laser, through periodic injection of high frequency and high peak power, creates a strong convection stirring effect in the molten pool, significantly enhancing the fluidity of the liquid metal, which is beneficial for the escape of pores and the homogenization of composition, while refining grains. This linkage mechanism of stable base and active disturbance is key to solving the problem of porosity in titanium alloy thin plate welding and improving microstructure and properties.

[0020] 3. In this invention, the active control of the energy distribution of the composite heat source within the molten pool is achieved by adjusting the power ratio and defocus ratio of the continuous laser and pulsed laser. Specifically, the power ratio controls the total heat input and the proportion of pulsed energy, while the defocus ratio controls the energy distribution along the depth direction of the molten pool. This multi-dimensional synergistic control can precisely shape the temperature field of the molten pool according to different plate thicknesses and process requirements, reducing the temperature gradient at its source, thereby effectively reducing residual stress and welding deformation. No existing technology mentions this method of jointly controlling the power ratio and defocus ratio of coaxial dual beams.

[0021] In summary, this invention provides a complete low-stress, low-deformation welding solution for thin-plate titanium alloy corner joints through a coaxial, spatially overlapping dual-beam design, coordinated control of energy ratio and defocus ratio, and the integration of three-dimensional gas protection and precision fixtures. By adjusting the energy ratio of continuous and pulsed lasers, precise control of welding heat input and energy distribution gradient is achieved, thereby reducing residual welding stress and effectively controlling the deformation angle of the thin-plate structure. The coaxial composite dual-beam laser offers a wide range of adjustable parameters, including continuous laser power, pulsed laser power, frequency, pulse width, defocus amount, and welding speed, providing a broad process window and reducing the requirements for assembly precision in thin-plate titanium alloy corner joint structures. By optimizing the power ratio of continuous and pulsed lasers and the coaxial dual-beam welding speed, welded joints with good weld formation and low residual stress can be obtained under the premise of good gas protection, and the welded joints have good mechanical properties, meeting the requirements of engineering applications. Attached Figure Description

[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 This is a schematic diagram of the coaxial dual-beam composite laser optical system of the present invention.

[0024] Figure 2This is a schematic diagram of the coaxially coupled dual-beam laser corner joint of the present invention.

[0025] Figure 3 This is a schematic diagram of the corner clamp of the present invention.

[0026] Figure 4 This is a schematic diagram of the gas protection device of the present invention.

[0027] Figure 5 This is an appearance drawing of a fillet weld on a thin titanium alloy plate.

[0028] Figure 6 This is an appearance drawing of the fillet weld of a square tube made of titanium alloy.

[0029] In the diagram: 1. Continuous laser; 2. Pulsed laser; 3. Aspherical lens on the continuous laser side; 4. Aspherical lens on the pulsed laser side; 5. Reflector; 6. Dichroic mirror; 7. Focusing lens; 8. First upper pressure plate; 9. Second upper pressure plate; 10. Lower base plate; 11. First bolt; 12. Second bolt; 13. Third bolt; 14. Fourth bolt; 15. Support plate; 16. Angle adjustment frame; 17. Argon gas protective cover; 18. Copper gas pipe; 19. Back copper liner; 20. Gas delivery hose; 21. Argon gas cylinder. Detailed Implementation

[0030] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0031] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0033] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps described in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.

[0034] In the description of this invention, it should be understood that the orientation or positional relationship indicated by directional terms such as "front, back, up, down, left, right", "horizontal, vertical, horizontal" and "top, bottom" is generally based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing this invention and simplifying the description. Unless otherwise stated, these directional terms do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on the scope of protection of this invention. The directional terms "inner" and "outer" refer to the inner and outer contours relative to the outline of each component itself.

[0035] For ease of description, spatial relative terms such as "above," "over," "on the upper surface of," "above," etc., are used herein to describe the spatial positional relationship of a device or feature as shown in the figures to other devices or features. It should be understood that spatial relative terms are intended to encompass different orientations in use or operation besides the orientation of the device as described in the figures. For example, if the device in the figures is inverted, a device described as "above" or "above" other devices or structures would subsequently be positioned as "below" or "under" other devices or structures. Thus, the exemplary term "above" can include both "above" and "below." The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used herein will be interpreted accordingly.

[0036] Furthermore, it should be noted that the use of terms such as "first" and "second" to define components is merely for the purpose of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore should not be construed as limiting the scope of protection of this invention.

[0037] like Figure 1 , Figure 2 As shown, this invention discloses a method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints, comprising the following steps: A first laser beam and a second laser beam with similar wavelengths are coupled into a composite laser beam that is completely overlapped in space through a coaxial composite optical system, and directly acted on the molten pool area of ​​the thin titanium alloy corner joint to be welded. By adjusting the energy ratio of the first laser beam and the second laser beam, the distribution gradient of welding heat input in the molten pool is actively controlled, thereby reducing welding residual stress and deformation angle.

[0038] Specifically, by adjusting the energy ratio and welding speed of the continuous and pulsed coaxial dual-beam laser flexible heat source, the energy distribution gradient of the composite heat source can be precisely controlled, reducing heat input, stress concentration, and effectively controlling the welding deformation of thin-plate titanium alloy corner joints.

[0039] Furthermore, the first laser beam is a continuous laser 1, used to provide the basic heat input to maintain the stability of the molten pool; the second laser beam is a pulsed laser 2, used to induce forced convection in the molten pool through periodic energy injection with its high frequency and high peak power, and to enhance the stability of the keyhole. The optical system specifically includes a continuous laser-side aspherical lens 3, a pulsed laser-side aspherical lens 4, a reflector 5, a dichroic mirror 6, and a focusing lens 7.

[0040] Furthermore, the coaxial composite optical system includes at least one dichroic mirror, which has high transmission for the first wavelength laser and high reflection for the second wavelength laser, or vice versa, so as to achieve optical path overlap of the two laser beams.

[0041] Continuous laser 1 is emitted by the first laser and has a wavelength of 1070 nm. Continuous laser 1 first enters the aspherical lens 3 on the continuous laser side, and then continues to propagate along the optical path, entering the dichroic mirror 6. The dichroic mirror 6 is a beam splitter with high transmission for 1070 nm wavelength laser and high reflection for 1064 nm wavelength laser. It is mounted on the optical system base, and its angle with the optical axis is adjusted by a precision adjustment bracket.

[0042] Pulsed laser 2 is emitted by the second laser and has a wavelength of 1064 nm. Pulsed laser 2 first enters the aspherical lens 4 on the pulse laser side, which is used to collimate the pulse laser 2. The collimated pulse laser 2 continues to propagate along the optical path and enters the reflecting mirror 5. The reflecting mirror 5 is a total reflection mirror, and its surface is coated with a dielectric film that is highly reflective to 1064 nm wavelength laser light. It is used to change the optical path direction of the pulse laser 2 so that the reflected pulse laser 2 is coaxial with the optical path of the continuous laser 1.

[0043] The pulsed laser 2, reflected by mirror 5, is incident on dichroic mirror 6. Because dichroic mirror 6 has high reflectivity for 1064nm wavelength laser light, the pulsed laser 2 is reflected by dichroic mirror 6, and its reflected light path completely coincides with the light path of the continuous laser 1 transmitted through dichroic mirror 6. After the two laser beams are coaxially coupled in space, they are jointly incident on focusing mirror 7.

[0044] Focusing lens 7 is a biconvex spherical lens used to focus the coaxially coupled composite laser beam onto the surface of the workpiece to be welded. Focusing lens 7 is mounted at the output end of the optical system via a threaded connection or a flange connection, and its mounting position can be finely adjusted along the optical axis to regulate the defocusing amount.

[0045] Through the synergistic effect of the aforementioned optical elements, continuous laser 1 and pulsed laser 2 achieve complete spatial overlap, forming a coaxial composite laser beam. The energy density distribution of this composite laser beam is determined by the power ratio and defocus ratio of the two laser beams.

[0046] Furthermore, it also includes the steps of grinding the workpiece to be welded to remove surface oil and oxide layer before welding, and assembling and fixing the titanium alloy corner joint components to be welded using corner joint clamps.

[0047] like Figure 3 As shown, the corner joint fixture used in this embodiment of the invention is used to precisely assemble and fix the thin-plate titanium alloy corner joint components to be welded. The corner joint fixture includes a lower base plate 10, a first upper pressure plate 8, a second upper pressure plate 9, a first bolt 11, a second bolt 12, a third bolt 13, a fourth bolt 14, a support plate 15, and an angle adjustment bracket 16.

[0048] The lower base plate 10 is a rectangular flat plate structure. Multiple threaded holes are formed on the upper surface of the lower base plate 10 for mounting the first upper pressure plate 8 and the second upper pressure plate 9. The angle adjustment bracket 16 is an adjustable angle support structure, which is fixedly connected to the lower base plate 10. The tilt angle of the angle adjustment bracket 16 can be adjusted by changing the height of the support plate 15 to accommodate the assembly requirements of corner joints with different bevel angles. Both the first upper pressure plate 8 and the second upper pressure plate 9 are rectangular pressure block structures. The first upper pressure plate 8 is connected to the lower base plate 10 by the first bolt 11 and the second bolt 12; the second upper pressure plate 9 is connected to the lower base plate 10 by the third bolt 13 and the fourth bolt 14.

[0049] Specifically, the titanium alloy corner joint components to be welded undergo surface pretreatment, with mechanical grinding to remove the surface oxide layer, followed by wiping with anhydrous ethanol to remove impurities and oil stains; the treated components are then placed... Figure 3 In the dedicated corner joint fixture, precise assembly and positioning are ensured, and the laser incident angle can be adjusted by adjusting the height of the support plate; Adjust the continuous and pulsed coaxial dual-beam laser head, and the coaxial protective nozzle. Figure 4The relative position between the argon protective shroud and the titanium alloy fillet weld in the gas protection device is determined by placing the argon protective shroud behind the laser head and providing back protection through a copper backing tube. The protective gas pipe is connected to the inlet of the shroud and the back copper tube directly behind the laser head, forming an argon protective atmosphere. This gas protection device includes an argon protective shroud 17, a copper gas pipe 18, a back copper backing tube 19, a gas delivery hose 20, and an argon cylinder 21. The argon protective shroud 17 is a semi-enclosed shroud made of thin stainless steel sheet, with the copper gas pipe 18 connected inside. This pipe blows the incoming argon gas obliquely upwards from the outlet of the pipe, avoiding direct blowing onto the weld and distributing it evenly throughout the weld area. The back copper backing tube 19 is a hollow copper tube with uniformly spaced outlet holes at its top. The back copper backing tube 19 is installed in a groove on the lower substrate, facing the back of the fillet weld joint to be welded. The air inlet of the copper liner 19 on the back is connected to the argon gas cylinder 21 via the gas delivery hose 20, and its outlet faces the back of the weld to provide back protective gas.

[0050] Adjust the original parameters of the dual-beam composite laser: average power P1 and defocusing amount Δf1 of the continuous laser; average power P2, defocusing amount Δf2, pulse frequency f, and pulse width τ of the pulsed laser; welding speed v1 and wire feed speed v2. After the program is set up, turn on the laser, start the control system, and execute the welding process according to the preset program to complete the welding of the titanium alloy corner joint; In the process, the flow rate of the protective gas for the laser nozzle is 15~25L / min, and the flow rate of the argon protective shroud and the copper backing tube is 30~50L / min.

[0051] Furthermore, the energy ratio is controlled by adjusting the ratio of the average power P1 of the continuous laser to the average power P2 of the pulsed laser, and the ratio satisfies: 3 ≤ P1 / P2 ≤ 5.5. The average output power P1 of the continuous laser is 1200W~1800W; the average output power P2 of the pulsed laser is 200W~400W.

[0052] Furthermore, the method also includes adjusting the ratio of the defocusing amount Δf1 of the continuous laser to the defocusing amount Δf2 of the pulsed laser to control the energy distribution of the composite laser beam in the direction of the molten pool depth, wherein the ratio satisfies: 0.5 ≤ Δf1 / Δf2 ≤ 2. The defocusing amount Δf1 of the continuous laser is +2mm to +10mm, and the defocusing amount Δf2 of the pulsed laser is 0mm to +12mm.

[0053] Furthermore, the pulse width τ and frequency f of the pulsed laser are adjustable to match different welding speeds v1 and wire feed speeds v2, thereby controlling the solidification process of the molten pool. Specifically, the pulsed laser frequency f is set to 20Hz~50Hz, the pulse width τ is set to 4ms~8ms, the welding speed v1 is 600mm / min~1400mm / min, and the wire feed speed v2 is 1500mm / min~2100mm / min.

[0054] Furthermore, the wavelength of the first laser beam is 1070 nm, and the wavelength of the second laser beam is 1064 nm.

[0055] This invention combines a continuous laser with a wavelength of 1070nm and a pulsed laser with a wavelength of 1064nm. The coaxial dual-beam composite laser of continuous and pulsed lasers combines the advantages of continuous lasers (stable heat input and high welding efficiency) and pulsed lasers (high instantaneous peak power and deep penetration) with the advantages of composite flexible heat sources (precise control of heat input, regulation of energy distribution gradient, and expansion of process window), providing a new welding method for corner joint structures of titanium alloy thin plates.

[0056] Example 1 A continuous and pulsed coaxial dual-beam welding method for thin-plate titanium alloy corner joints was used to weld Ti-6Al-4V titanium alloy corner joints. The fabrication process is as follows: (1) Select TC4 thin plate titanium alloy with thicknesses of 1.5mm and 2mm respectively as the wing plate and rib plate of the corner joint structure, and perform pretreatment. Use sandpaper to mechanically grind the surface of the titanium alloy to remove the surface oxide film. Use anhydrous ethanol to clean the workpiece after grinding to remove surface impurities and oil stains, and use a special welding fixture to assemble and fix the workpiece. (2) Adjust the relative angle and position between the coaxial dual-beam laser head, coaxial protective nozzle, argon protective shroud and titanium alloy fillet weld, and connect the protective gas pipe and the inlet of the back copper pipe. The continuous and pulsed coaxial dual beams include a continuous laser with a wavelength of 1070nm and a pulsed laser with a wavelength of 1064nm, which are coupled into a composite laser beam through the coaxial optical system; adjust the height of the laser head to the fillet weld so that the defocusing amount of both the continuous laser beam and the pulsed laser beam is set to Δf=+6mm; before welding, introduce high-purity argon gas (purity 99.99%) for 120 seconds in advance to fully remove the air in the protective area. Set the gas flow rate of the coaxial protective nozzle to 20L / min to fully remove the air in the protective gas shroud and the back copper pipe, and ensure that the welding area is in an inert gas atmosphere to prevent titanium alloy oxidation. After welding, continue to introduce argon gas for 120s to maintain the protective atmosphere until the weld cools down; (3) Set the initial experimental parameters for continuous laser with wavelength of 1070nm and pulsed laser with wavelength of 1064nm: average output power of continuous laser P1=1600W, average output power of pulsed laser P2=300W, pulsed laser frequency f=45Hz, pulsed laser pulse width τ=6ms; welding speed ν1=1000mm / min, wire feeding speed ν2=1800mm / min; (4) After the program is set, turn on the laser, start the control system, and execute the welding process according to the preset program. Turn on the continuous laser and the pulsed laser in sequence, and start the control system. The robotic arm carries the laser welding head, argon gas protective cover and wire feeder, and moves along the fillet weld direction at the set welding speed according to the pre-taught trajectory. During the welding process, the coaxially overlapping composite laser beam acts on the weld area of ​​the thin plate titanium alloy fillet joint. After the material melts to form a molten pool, the laser directly acts on the molten pool area. Under the guidance of the wire feeder, the welding wire is accurately fed into the energy action area of ​​the composite laser beam. The molten welding wire enters the molten pool in a liquid bridge transition mode, forming a weld with good forming quality. The entire welding process is carried out stably under the three-dimensional protection of argon gas. The welding of the titanium alloy fillet joint is completed; The weld appearance of the Ti-6Al-4V titanium alloy corner joint obtained by this method is as follows: Figure 5 As shown, the weld surface is silvery-white, well-formed, and free of obvious oxidation and spatter. Mechanical property tests of the joint indicate that its maximum tensile strength reaches 19.5 kN, meeting the requirements of relevant engineering applications.

[0057] Example 2 A continuous and pulsed coaxial dual-beam welding method for welding square tube Ti-6Al-4V titanium alloy corner joints was adopted. The preparation process is as follows: (1) Select a 1.5mm thick TC4 titanium alloy sheet and a 3mm thick TC4 titanium alloy square tube as the base plate and side plate of the corner joint structure, respectively. Pre-treat the base plate and side plate, use sandpaper to mechanically grind the titanium alloy surface to remove the surface oxide film, and clean the workpiece after grinding with anhydrous ethanol to remove surface impurities and oil stains. Then, use a special welding fixture to assemble and fix the workpiece. (2) Adjust the relative angle and position between the coaxial dual-beam laser head, coaxial protective nozzle, argon protective shield and titanium alloy fillet weld, and connect the protective gas pipe and the inlet of the back copper pipe. The continuous + pulsed coaxial dual beam includes a continuous laser with a wavelength of 1070nm and a pulsed laser with a wavelength of 1064nm, which are coupled into a composite laser beam through a coaxial optical system; adjust the height of the laser head to the fillet weld so that the defocusing amount of the continuous laser beam is set to Δf=+10mm and the defocusing amount of the pulsed laser beam is set to +5mm; before welding, argon gas is introduced for 120s in advance to fully remove the air in the protective gas shield and the back copper pipe, ensuring that the welding area is in an inert gas atmosphere to prevent titanium alloy oxidation. After welding, continue to introduce argon gas for 120s to maintain the protective atmosphere until the weld cools down; (3) Set the initial experimental parameters for continuous laser with wavelength of 1070nm and pulsed laser with wavelength of 1064nm: average output power of continuous laser P1=1800W, average output power of pulsed laser P2=330W, pulsed laser frequency f=50Hz, pulsed laser pulse width τ=8ms; welding speed ν1=600mm / min, wire feeding speed ν2=2100mm / min; (4) After the program is set, turn on the laser, start the control system, and execute the welding process according to the preset program to complete the welding of the titanium alloy corner joint; The weld appearance of the titanium alloy square tube corner joint obtained using this method is as follows: Figure 6 As shown, the weld surface is well formed and basically without deformation.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints, characterized in that, Includes the following steps: A first laser beam and a second laser beam with similar wavelengths are coupled into a composite laser beam that is completely overlapped in space through a coaxial composite optical system. The laser irradiates the weld area of ​​the thin titanium alloy corner joint to be welded. After the material melts and forms a molten pool, the laser directly acts on the molten pool area. By adjusting the energy ratio of the first laser beam and the second laser beam, the distribution gradient of welding heat input in the molten pool is controlled, thereby reducing welding residual stress and deformation angle. The first laser beam is a continuous laser, used to provide the basic heat input to maintain the stability of the molten pool; The second laser beam is a pulsed laser, which injects its high-frequency, high-peak-power periodic energy into the molten pool to induce forced convection and enhance the stability of the keyhole.

2. The method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints according to claim 1, characterized in that, The coaxial composite optical system includes at least one dichroic mirror, which has high transmission for the first wavelength laser and high reflection for the second wavelength laser, or vice versa, so as to achieve optical path overlap of the two laser beams.

3. The method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints according to claim 1, characterized in that, It also includes the steps of grinding the workpiece to be welded to remove surface oil and oxide layer before welding, and assembling and fixing the titanium alloy corner joint components to be welded using corner joint fixtures.

4. The method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints according to claim 1, characterized in that, The energy ratio is controlled by adjusting the ratio of the average power P1 of the continuous laser to the average power P2 of the pulsed laser, and the ratio satisfies: 3≤P1 / P2≤5.

5.

5. The method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints according to claim 1, characterized in that, It also includes adjusting the ratio of the defocusing amount Δf1 of the continuous laser to the defocusing amount Δf2 of the pulsed laser to control the energy distribution of the composite laser beam in the direction of the molten pool depth, and the ratio satisfies: 0.5≤Δf1 / Δf2≤2.

6. The method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints according to claim 1, characterized in that, The pulse width τ and frequency f of the pulsed laser are adjustable to match different welding speeds v1 and wire feed speeds v2, thereby controlling the solidification process of the molten pool. Specifically, the pulsed laser frequency f is set to 20Hz~50Hz, the pulse width τ is set to 4ms~8ms, the welding speed v1 is 600mm / min~1400mm / min, and the wire feed speed v2 is 1500mm / min~2100mm / min.

7. The method for continuous and pulsed coaxial dual-beam welding of thin-plate titanium alloy corner joints according to claim 1, characterized in that, The wavelength of the first laser beam is 1070 nm, and the wavelength of the second laser beam is 1064 nm.