Inverted ultrasensitive resistive flexible pressure sensor based on negative Poisson's ratio structure

By using a negative Poisson's ratio structure and composite material design, the problems of high sensitivity, wide operating range and stability of flexible resistive pressure sensors have been solved, and resistance stability and temperature adaptability have been achieved during repeated deformation processes.

CN122360745BActive Publication Date: 2026-11-17HEFEI UNIV OF TECH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202610519662.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-04-20
Publication Date
2026-11-17
Estimated Expiration
2046-04-20

AI Technical Summary

Technical Problem

Existing flexible resistive pressure sensors based on crack structures struggle to simultaneously achieve high sensitivity, wide operating range, and high stability. Furthermore, these sensors are prone to issues such as interface peeling, uneven dispersion of conductive materials, and high temperature sensitivity during repeated deformation.

Method used

The stacked design employs a negative Poisson's ratio structure, including upper and lower encapsulation layers and a middle high-conductivity layer. The encapsulation layer has concave hexagonal holes, and the high-conductivity layer has through cracks. The conductive path conversion and structural stability are ensured by using a composite material of silicone rubber, polylactic acid, hydroxylated graphene, and nano-carbon black particles, combined with laser etching directional crack technology.

Benefits of technology

This technology achieves high sensitivity and stability of the sensor over a wide pressure range, avoids interface delamination, improves the uniformity and temperature stability of conductive materials, and enhances the durability and consistency of the sensor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122360745B_ABST
    Figure CN122360745B_ABST
Patent Text Reader

Abstract

This invention discloses a flip-chip ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure, comprising, from top to bottom, an upper encapsulation layer, a low-conductivity layer, a high-conductivity layer, and a lower encapsulation layer. The upper, low-conductivity, and lower encapsulation layers all employ a pore structure composed of concave hexagonal holes, giving them a negative Poisson's ratio characteristic. Under pressure, they undergo lateral contraction, significantly increasing the opening and closing degree of cracks in the high-conductivity layer and effectively improving the sensor's sensitivity. The high-conductivity layer contains linear, regular cracks penetrating its thickness. The lower encapsulation layer contains two through-holes, each containing a signal electrode, the upper end of which is connected to the high-conductivity layer. The flexible pressure sensor provided by this invention possesses characteristics such as high sensitivity, high stability, and a wide operating range, making it well-suited for applications in wearable devices, industrial robots, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of sensor technology, specifically relating to an inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure. Background Technology

[0002] With the development of technologies such as the Internet of Things, intelligent robots, and health monitoring, wearable flexible electronic devices have broad application prospects due to their lightweight and high flexibility. Compared with traditional strain electronic sensors, flexible pressure sensors overcome the drawback of brittleness and have significant advantages in terms of flexibility and tensile strength. Flexible pressure sensors play a vital role in fields such as electronic skin, industrial robots, and health monitoring.

[0003] Crack-based resistive flexible pressure sensors have attracted much attention due to their simple fabrication, high sensitivity, and fast response. However, they struggle to simultaneously achieve both high sensitivity and a wide operating range, and the randomness and difficulty in controlling the number and location of cracks affect their stability. Therefore, designing a highly stable resistive flexible pressure sensor that combines high sensitivity, a wide operating range, and adjustable cracks is of great significance.

[0004] In recent years, much work has been done on the research of resistive flexible pressure sensors based on crack structures: The academic paper "Flexible and Highly Sensitive Pressure Sensors Based on Bionic Hierarchical Structures" (Muqiang Jian, Kailun Xia, Qi Wang, Huanhuan Xie, Mingchao Zhang, Yingying Zhang, Adv. Funct. Mater. 2017, 27, 1606066.) proposes a simple method for fabricating high-performance pressure sensors. This method involves coating a highly conductive ACNT / G thin film directly grown by chemical vapor deposition onto a hierarchically raised m-PDMS thin film, resulting in a sensor with high sensitivity and a low detection limit. However, since the bonding between the ACNT / G thin film and m-PDMS mainly relies on van der Waals forces, the interface is prone to delamination during long-term cyclic pressure loading, leading to poor sensor stability.

[0005] The academic paper "A stretchable strain sensor based on a metal nanoparticle-thin film for human motion detection" (J. Lee, S. Kim, J. Lee, D. Yang, BCPark, S. Ryu, I. Park Nanoscale 2014, 6, 11932.) proposes a novel stretchable strain sensor. It amplifies crack propagation under pressure by constructing a bridge-like stress-sensitive unit between two PDMS substrates, thus enabling the sensor to exhibit high sensitivity to both tensile and compressive strains. However, this structure requires a robust interfacial bond and is prone to breakage in practical applications.

[0006] The academic paper "Hollow-porous fiber-shaped strain sensor with multiple wrinkle-crack microstructure for strain visualization and wind monitoring" (Zhao XX, Guo H, Ding P, et al. Nano Energy, 2023(108):108197.) developed a fiber-shaped strain sensor with a hollow, porous, wrinkled, and cracked structure through wet spinning and two pre-stretching / release processes. The fabricated sensor has a wide sensing range (530%) and high sensitivity (GF≈57.2). However, the conductive layer of this sensor is obtained by immersing and drying in carbon nanotube ink. Repeated processes can easily lead to the expansion of the number and depth of cracks, and the stability and repeatability of the sensor cannot be guaranteed.

[0007] The academic paper "A Flexible Strain Sensor Based on the Porous Structure of a Carbon Black / Carbon Nanotube Conducting Network for Human Motion Detection" (Zhang P, Chen Y, Li Y, et al. Sensors. 2020, 20(4): 1154.) employs a simple and low-cost porous polydimethylsiloxane surface spraying method. By constructing a synergistic conductive network on carbon black and multi-walled carbon nanotubes, the synergistic effect of carbon black and multi-walled carbon nanotubes, combined with the advantages of its porous polydimethylsiloxane structure, improves the sensor's performance. However, this sensor only uses carbon-based materials for conductivity, and the non-uniform dispersion of the filler leads to poor electrical stability and consistency of the sensor.

[0008] Patent application CN105783697A employs a method of pre-setting microcrack structures in the conductive layer, resulting in high sensor sensitivity. Furthermore, an encapsulation layer is added outside the conductive coating to protect the internal crack structures, significantly extending the lifespan of the crack strain sensor and enhancing its stability. However, this pre-set microcrack structure is prone to fatigue under long-term cyclic strain, as the microcracks propagate and recover, leading to a gradual decrease in sensitivity with increasing usage. Additionally, if the flexibility of the encapsulation layer and the conductive layer is poorly matched, the encapsulation layer can easily peel off from the conductive layer under high strain conditions, resulting in poor sensor stability.

[0009] The flexible pressure sensor in patent application CN113340484A has a multi-layer structure, consisting of a lower encapsulation layer, a flexible substrate layer, a first conductive electrode, a composite sponge layer, a second conductive electrode, and an upper encapsulation layer from bottom to top. This invention enhances pressure testing sensitivity by ensuring full contact between the electrode's nanofiber structure and its porous structure. It also combines a flexible sponge framework with conductive materials to achieve pressure sensitivity switching across different pressure ranges, expanding the pressure detection range and maintaining good linear response over a wide range. However, under long-term pressure, interlayer delamination is prone to occur, leading to a decrease in sensor performance. Furthermore, when the composite sponge layer is impregnated using a solution impregnation method, the uniformity of the conductive material distribution within the sponge is poor, easily causing large individual differences in the sensors and resulting in poor sensor consistency.

[0010] Patent application CN109655180A describes a method of creating a crack array structure and its inverse on a PDMS surface using a flip-flop technique. Two flexible substrates, one with a regular crack array structure and the other with its inverse, are positioned opposite each other. The sensor's resistance is altered by the change in the contact area between the crack array structure and its inverse on the flexible substrate surface under external pressure, thereby improving the sensor's sensitivity. However, this design, relying on the contact between the crack array and its inverse, is prone to wear at the crack edges under long-term cyclic pressure or strain. This leads to unstable changes in the contact resistance, affecting the sensor's stability and repeatability.

[0011] Despite significant progress in the research of flexible resistive sensors based on crack structures, the following shortcomings still exist: 1. Flexible strain sensors based on single-strain layer crack structures struggle to simultaneously achieve both high sensitivity and a wide operating strain range. Early designs, with network-like crack structures in the strain layer, exhibited randomly distributed crack directions and short lengths. Due to reduced crack propagation efficiency, these flexible strain sensors offered a wide operating range but low sensitivity. Conversely, when the strain layer possessed a fully channeled crack structure, the conductive paths within the strain layer were rapidly severed under small deformations, resulting in high sensitivity but a narrower operating range.

[0012] 2. Flexible strain sensors are mostly suitable for operation under tension. To convert the strain element into a pressure working mechanism, elastic sensitive elements, such as cantilever beams or diaphragms, are generally used. However, using such elastic sensitive elements will significantly reduce the flexibility and interface compatibility of the sensor, and may cause interface delamination under repeated bending and stretching cycles. In addition, the introduction of additional elastic sensitive elements will result in a larger overall sensor size, which is not conducive to miniaturization and integration, thus limiting the application range of the sensor. Designing a flexible pressure sensor with a cracked structure without using elastic sensitive elements is a major challenge.

[0013] 3. Resistive flexible pressure sensors often employ conductive fillers incorporated into polymers or stress-sensitive elements fabricated using intrinsically conductive polymers to achieve conductivity. However, conductive fillers such as metal fillers and carbon-based fillers are unevenly dispersed within the polymer, leading to poor sensor stability. Stress-sensitive elements fabricated using intrinsically conductive polymers, such as PEDOT:PSS, exhibit excellent electrochemical performance and stability; however, PEDOT:PSS has poor tensile strength and low intrinsic conductivity, making it difficult to meet the high sensitivity requirements of sensors.

[0014] 4. Resistive flexible pressure sensors based on crack structures often employ solution evaporation or pre-strain methods to generate cracks. Solution evaporation induces cracks through the shrinkage stress generated during solvent evaporation, but its location and number are easily affected by factors such as evaporation rate and humidity. Pre-strain methods induce cracks through pre-stretching and then releasing; however, due to uneven stress distribution, the number and location of cracks are also prone to be random, affecting the sensor's sensitivity and stability.

[0015] 5. Resistive flexible pressure sensors based on crack structures often use a single polymer material for the encapsulation layer, which typically has high thermal conductivity. This makes it difficult to effectively isolate the sensor from the influence of external environmental temperature changes, easily leading to interlayer thermal stress and non-stressful opening and closing of cracks, causing resistance signal drift. In addition, the conductive material used in the sensor's sensitive layer is usually highly sensitive to temperature, making the sensor prone to large resistance signal fluctuations in a wide temperature range.

[0016] 6. The conductive layer and encapsulation layer of resistive flexible pressure sensors often have significantly different mechanical moduli between them, as well as between different strain layers. The adhesion between the layers is purely based on van der Waals forces, resulting in weak interfacial adhesion and poor compatibility. Since flexible pressure sensors need to be repeatedly deformed during operation, this may lead to peeling, detachment, or displacement between the layers, resulting in poor sensor stability and durability. Furthermore, existing negative Poisson's ratio materials are mostly prepared by converting positive Poisson's ratio materials with honeycomb cell structures. Under repeated pressure loads, they are prone to pore collapse and irreversible deformation, which seriously affects the stability and durability of the sensor. Summary of the Invention

[0017] The purpose of this invention is to overcome the shortcomings of the prior art and provide an inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure and its fabrication method. This effectively improves the problem that flexible pressure sensors are difficult to achieve simultaneously with high sensitivity, high stability and wide operating range, and can be widely used in wearable electronics, industrial robots and electronic skin.

[0018] To solve the above problems, the present invention adopts the following solution: The flip-chip ultrasensitive resistive flexible pressure sensor based on the negative Poisson ratio structure is characterized in that: the flexible pressure sensor has a stacked structure, which consists of an upper encapsulation layer with negative Poisson bit characteristics, a low conductivity layer with negative Poisson bit characteristics, a high conductivity layer with positive Poisson ratio characteristics, and a lower encapsulation layer with negative Poisson bit characteristics from top to bottom. The upper encapsulation layer, low conductivity layer, and lower encapsulation layer all employ a porous structure composed of concave hexagonal holes, giving them a negative Poisson's ratio characteristic. The high conductivity layer contains linear, regular cracks that penetrate its thickness, dividing it into multiple discontinuous square blocks. The lower encapsulation layer contains two through-holes, each containing a signal electrode. The upper end of the signal electrode is electrically connected to the high conductivity layer, and the lower end protrudes 100-500 μm from the bottom of the lower encapsulation layer.

[0019] Furthermore, the low-conductivity layer is prepared by mixing silicone rubber, polylactic acid, hydroxylated graphene, and nano-carbon black particles, and the elastic modulus of the low-conductivity layer is 1.2-1.8 MPa; the angle α of the concave hexagonal holes is 60°-75°, the length is 400-600 μm, the width is 300-400 μm, and the spacing between two adjacent concave hexagonal holes is 700-1000 μm. Even further, the composite matrix formed by silicone rubber and polylactic acid possesses both flexibility and structural stability, and the combination of hydroxylated graphene and nano-carbon black particles as conductive fillers can construct continuous conductive pathways, enabling the low-conductivity layer to maintain both flexibility and basic conductivity. The angles and dimensions of the concave hexagonal pores are structurally optimized. The α angle of 60°-75° can endow the material with stable negative Poisson's ratio characteristics. The combination of a length of 400-600μm and a width of 300-400μm, along with an adjacent spacing of 700-1000μm, not only ensures the directional deformation capability of the pore structure, but also suppresses irreversible structural damage after large deformation through the support of the pore walls. This allows the low conductivity layer to achieve excellent shape recovery and structural stability of the composite foam while also possessing conductivity.

[0020] Furthermore, both the upper and lower encapsulation layers are silicone rubber composite materials, composed of silicone rubber, polyimide micro / nano hollow fibers, and silane coupling agent KH-550. The elastic modulus of both the upper and lower encapsulation layers is 1.0-1.6 MPa. Based on the total mass of silicone rubber, polyimide micro / nano hollow fibers, and silane coupling agent KH-550 as 100%, the polyimide micro / nano hollow fibers account for 6%-12%, the silane coupling agent KH-550 accounts for 0.1%-0.3%, and the balance is silicone rubber. Silicone rubber, as the substrate of the encapsulation layer, with a sufficient mass fraction, ensures that the encapsulation layer has excellent flexibility and resistance to high and low temperatures, adapting to the overall flexibility requirements of the sensor; 6%-12% of polyimide micro / nano hollow fibers, as lightweight thermal insulation fillers, can significantly reduce the thermal conductivity of the encapsulation layer. Combined with its three-dimensional continuous network structure, it further improves the overall thermal insulation performance of the sensor, achieving temperature stability of the internal structure when the external temperature changes; 0.1%-0.3% of silane coupling agent KH-550 can improve the compatibility between the components, strengthen the bonding force between the polyimide micro / nano hollow fibers and the silicone rubber matrix, and prevent component delamination.

[0021] Furthermore, the highly conductive layer is prepared by mixing PVA, PEDOT:PSS, hydroxylated graphene, and nano-carbon black particles, with an elastic modulus of 0.8-1.3 MPa. The hydroxylated graphene and nano-carbon black particles serve as composite conductive fillers, synergistically interacting with PVA and PEDOT:PSS. In the highly conductive layer, the hydroxylated graphene interweaves with the conductive chains of PEDOT:PSS through a two-dimensional sheet structure to form a three-dimensional conductive network, enhancing the conductivity of the composite layer. Furthermore, the surface hydroxyl groups form hydrogen bonds with the sulfonic acid groups on the PEDOT:PSS molecular chains, improving the dispersion of graphene in the PEDOT:PSS matrix and preventing aggregation. The π-π interaction between PEDOT:PSS and graphene results in a highly ordered arrangement of the PEDOT conjugated chains, enabling effective charge transfer between PEDOT and graphene. This transforms the PEDOT chain from a benzene structure to a quinone structure, improving the conductivity and electrical stability of the highly conductive layer, thereby further enhancing the sensitivity and stability of the sensor.

[0022] Furthermore, the thickness of the highly conductive layer is 10-300 μm, and the conductivity is not less than 3000 S / cm; the thickness of the low-conductivity layer is 0.5-2 mm, and the conductivity is not higher than 15 S / cm. The sensitivity of a resistive pressure sensor is defined as the ratio of the change in sensor resistance to the initial resistance under a unit pressure intensity. Different conductivity levels in the highly conductive and low-conductivity layers result in different overall sensor performance. Higher conductivity in the highly conductive layer leads to a smaller initial resistance in the sensor's conductive path, allowing minute resistance changes to be detected and improving sensitivity to minute pressures. Conversely, lower conductivity in the low-conductivity layer results in a larger resistance change after the sensor cracks under pressure, thus increasing the sensor's sensitivity.

[0023] Furthermore, the regular cracks within the highly conductive layer have a width of 10-20 μm, with a spacing of 60-120 μm between adjacent cracks, and their extension direction is parallel to the sensor's force direction. The 10-20 μm crack width provides sufficient physical space for the high-conductivity layer's contraction deformation under pressure, preventing premature crack closure due to insufficient contraction under low pressure. The 60-120 μm spacing between adjacent cracks primarily controls the density of the crack network: too large a spacing results in a sparse crack distribution, leading to a smaller change in the conductive path under pressure and insufficient sensor sensitivity; too small a spacing results in a dense crack distribution, easily causing excessive concentration of conductive paths under pressure, which not only leads to sensor signal fluctuations but may also cause localized breakage of conductive paths due to excessive crack density, affecting sensor stability. The design of its extension direction being parallel to the sensor's force direction allows the highly conductive layer to contract synchronously with the sensor's force, ensuring a precise correspondence between crack opening and closing states and pressure changes, further guaranteeing the stability and consistency of the sensor signal, and achieving a linear correspondence between pressure and resistance changes.

[0024] Furthermore, the pressure sensor adopts an inverted structure, with the signal electrodes arranged at the bottom layer of the sensor. The electrode lead-out direction is perpendicular to the force direction. Compared with the traditional electrode lead structure, this avoids the pressure acting directly on the electrodes and leads, significantly improving the reliability of electrical connection and cycle stability. Moreover, the electrodes do not occupy the upper effective sensing area, allowing the negative Poisson's ratio contraction of the low conductivity layer to be completely transmitted to the crack area of ​​the high conductivity layer, further improving the sensor sensitivity. At the same time, the upper end of the electrode is tightly connected to the high conductivity layer, ensuring the continuity of the conductive path.

[0025] The method for fabricating the resistive flexible pressure sensor of the present invention includes the following steps: Step 1: Prepare the upper and lower encapsulation layers. Silicone rubber is added to anhydrous ethanol and continuously stirred in a constant temperature water bath at 80-90℃ until dissolved. Then, an ethanol solution of silane coupling agent KH-550 with a concentration of 15-25 mg / mL is added and stirred for 3-10 minutes until completely dissolved. While stirring, polyimide micro / nano hollow fibers are slowly added and ultrasonically mixed evenly. Then, mechanical stirring is performed for 20-40 minutes, and the mixture is allowed to stand for 10-20 minutes to remove bubbles, resulting in a silicone rubber composite slurry. Edible salt is then added at 2-5 times the total mass of the composite slurry and stirred until evenly mixed to obtain a mixed liquid slurry. Based on the total mass of silicone rubber, polyimide micro / nano hollow fibers, and silane coupling agent KH-550 as 100%, polyimide micro / nano hollow fibers account for 6%-12%, silane coupling agent KH-550 accounts for 0.1%-0.3%, and the remainder is silicone rubber. The mixed liquid slurry was slowly poured into the 3D-printed concave hexagonal array mold and pre-cured in an oven at 55-65℃ for 2-4 hours. Then, the sample was immersed in deionized water at 35-45℃ for 10-14 hours to fully dissolve and remove edible salt particles using a salt immersion method. The sample was then removed, dried and cured at 75-85℃ for 1.5-4.5 hours, and allowed to cool naturally to room temperature to obtain the initial blanks of the upper and lower encapsulation layers. The upper encapsulation layer preform is placed in a plasma cleaner and O2 plasma treatment is used to activate the surface hydroxyl groups. Two through holes penetrating the thickness of the lower encapsulation layer preform are made using laser drilling. The through holes correspond to the electrode connection area of ​​the high conductivity layer. The inner wall of the through holes is activated by O2 plasma treatment. Conductive silver paste is poured into the through holes and cured at 55-65℃ for 1-3 hours to form the signal electrode. The O2 plasma treatment parameters are 40-60W and 15-25s. The lower end of the signal electrode protrudes 100-500μm from the bottom of the lower encapsulation layer. Step 2: Prepare a highly conductive layer Polyvinyl alcohol (PVA) is added to deionized water and stirred in a constant temperature water bath at 85-95℃ until completely dissolved. After cooling to room temperature, a PEDOT:PSS solution with a solid content of 1-3%, hydroxylated graphene, and nano-carbon black particles are added. The mixture is stirred for 5-15 minutes, ultrasonically mixed until homogeneous, and allowed to stand for 5-15 minutes to remove bubbles, thus obtaining a highly conductive slurry. Based on the total mass of PVA, PEDOT:PSS, hydroxylated graphene, and nano-carbon black particles as 100%, PVA accounts for 20%-30%, hydroxylated graphene accounts for 1.2%-3%, nano-carbon black particles account for 1.8%-4.2%, and the remainder is PEDOT:PSS. The highly conductive paste is applied to the lower encapsulation layer using screen printing and then dried in an oven at 75-85℃ for 20-40 minutes to cure. The coating speed is 3-5 mm / s and the coating pressure is 0.1-0.2 MPa. A 532nm wavelength laser was used to etch crack guide grooves on the surface of a highly conductive layer at a power of 10-20 mW and a scanning speed of 100-200 μm / s. The crack guide grooves had a depth of 1-2 μm, a width of 10-20 μm, and a spacing of 60-120 μm. Wipe the surface of the highly conductive layer with anhydrous ethanol swabs to remove residual etching debris, and then dry it with nitrogen. Then place it in a plasma cleaner and treat it with O2 plasma to activate the surface hydroxyl groups. The O2 plasma treatment parameters are 40-60W power and 15-25s time. Step 3: Prepare a low conductivity layer Take silicone rubber, polylactic acid, hydroxylated graphene, nano-carbon black particles and edible salt in a mass ratio of 1:(0.4-0.6):(0.01-0.03):(0.01-0.03):(1-5). Mix silicone rubber and polylactic acid, add anhydrous ethanol to adjust the viscosity to 500-700 mPa∙s, stir until uniformly mixed, then add hydroxylated graphene, nano-carbon black particles and edible salt in sequence, ultrasonically disperse at 250-350W for 20-40 min, let stand to degas for 15-25 min to obtain a low conductivity layer slurry. The low conductivity layer slurry was poured into a 3D-printed concave hexagonal array mold and pre-cured in an oven at 55-65℃ for 2-4 hours. Then, the sample was immersed in deionized water at 35-45℃ for 10-14 hours to fully dissolve and remove edible salt particles using a salt immersion method. The sample was then removed, dried and cured at 75-85℃ for 1.5-4.5 hours, and allowed to cool naturally to room temperature to obtain the low conductivity layer. Step 4: Sensor Assembly Spray KH-560 adhesive onto the surface of the high conductivity layer, align the low conductivity layer with the high conductivity layer and gently press to adhere, let stand at room temperature for 20-40 minutes for initial cross-linking, and then dry at 75-85℃ for 0.5-1.5 hours. Then, spray KH-560 adhesive onto the surface of the low conductivity layer, align the upper encapsulation layer with the low conductivity layer and gently press to adhere it. Allow it to stand at room temperature for 20-40 minutes for initial cross-linking, and then dry it at 75-85℃ for 0.5-1.5 hours to complete the overall stacking assembly. The obtained device is fixed in a tension and compression press, and heated from room temperature to 35-45℃ at a heating rate of 4-6℃ / min. It is then held at this temperature for 5-15 minutes, followed by 70-90 cycles of loading and unloading under a pressure of 0-50 kPa to form a through crack in the highly conductive layer along its thickness direction. The crack is then stabilized by holding the device at this temperature for another 20-40 minutes. Finally, the device is cooled to room temperature at a rate of 2-4℃ / min, thus completing the fabrication of an ultrasensitive, highly stable resistive flexible pressure sensor based on a negative Poisson's ratio structure.

[0026] Compared with existing technologies, the beneficial effects of this invention are reflected in: 1. The resistive flexible pressure sensor proposed in this invention introduces a double strain layer with a crack structure to achieve the switching of conductive paths under different pressures, avoiding the resistance value of the sensing unit from approaching its limit too early and ensuring a wide operating range; and combined with the crack optimization structure, it achieves the switching of conductive paths under pressure, thereby improving the sensitivity of the sensing unit.

[0027] 2. The resistive flexible pressure sensor proposed in this invention achieves a negative Poisson's ratio characteristic by designing a pore structure composed of concave hexagonal holes inside the upper and lower encapsulation layers and the low conductivity layer. When under pressure, it shrinks significantly laterally, which drives the closure of cracks in the high conductivity layer, greatly increasing the resistance change rate and further improving the sensor sensitivity.

[0028] 3. The resistive flexible pressure sensor proposed in this invention employs hydroxylated graphene in the high conductivity layer. The hydroxyl groups form stable hydrogen bonds with the sulfonic acid groups in the PEDOT:PSS molecular chain. Combined with the π-π conjugation between the graphene sheets and PEDOT:PSS, this effectively reduces surface energy differences and promotes uniform dispersion of graphene in the matrix. Furthermore, the π-π interaction between PEDOT:PSS and graphene results in a highly ordered arrangement of the PEDOT conjugated chains, enabling effective charge transfer between PEDOT and graphene. This transforms the PEDOT chain from a benzene structure to a quinone structure, improving the conductivity and electrical stability of the high conductivity layer, thereby further enhancing the sensor's sensitivity and stability.

[0029] 4. The resistive flexible pressure sensor proposed in this invention utilizes laser-guided directional crack technology. By using a laser to etch crack guide grooves on the surface of a highly conductive layer, the cracks are strictly propagated along the guide grooves, avoiding random crack generation in the sensor. At the same time, the location and number of cracks can be controlled by preset distribution positions and spacing of the guide grooves, thereby achieving high consistency in the manufacturing process and high stability in use.

[0030] 5. The resistive flexible pressure sensor proposed in this invention uses coaxial electrospun polyimide micro / nano hollow fibers in the encapsulation layer, which can effectively block the conduction of external heat to the interior, keep the sensor operating temperature stable, suppress the generation of interlayer thermal stress, and thus avoid the non-stressed opening and closing of cracks; and the conductive filler used in the sensor sensitive layer is compounded with hydroxyl graphene with a negative temperature resistivity and nano carbon black with a positive temperature resistivity, which offsets the temperature sensitivity of a single material, so that the sensor has good anti-temperature drift characteristics.

[0031] 6. The resistive flexible pressure sensor proposed in this invention uses KH-560 silane coupling agent to achieve bonding between the low conductivity layer, the high conductivity layer, and the upper encapsulation. Chemical bonding enhances the interlayer bonding strength, and the elastic moduli of the low conductivity layer, the high conductivity layer, and the upper and lower encapsulation layers are matched, reducing interlayer stress concentration during repeated loading and unloading processes. In addition, the low conductivity layer composite foam is made by synergistically controlling the hierarchical pore structure, which has excellent shape recovery ability and overcomes the deformation problem of traditional negative Poisson's ratio foam after large deformation, giving the sensor a high fatigue threshold and good stability. Attached Figure Description

[0032] Figure 1 This is a schematic diagram of the cross-sectional structure of the inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to the present invention.

[0033] Figure 2 This is a schematic diagram of a concave hexagonal array mold used to fabricate the upper and lower encapsulation layers and the low conductivity layer.

[0034] Figure 3 This is a schematic diagram of the etching of the high conductivity layer nanoguide groove and the crack propagation after cyclic ballast loading in this invention.

[0035] Figure 4 This is a schematic diagram illustrating the interaction principle between the highly conductive layer PEDOT:PSS and hydroxylated graphene in this invention.

[0036] Figure 5 This is a schematic diagram of the sensing mechanism and local conductive path of the flexible resistive pressure sensor of the present invention.

[0037] Figure 6 The pressure sensing characteristic curve of the flexible resistive pressure sensor of the present invention is shown.

[0038] Figure 7 This is the stepped pressure characteristic curve of the flexible resistive pressure sensor of the present invention.

[0039] Figure 8 The image shows the cyclic stability test curve of the flexible resistive pressure sensor of the present invention.

[0040] The labels in the diagram are: 1 upper encapsulation layer, 2 low conductivity layer, 3 concave hexagonal hole, 4 high conductivity layer, 5 guide groove, 6 crack, 7 lower encapsulation layer, and 8 signal electrode. Detailed Implementation

[0041] The embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The following embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given. However, the protection scope of the present invention is not limited to the following embodiments.

[0042] The polyimide micro / nano hollow fibers used in the following examples were prepared by coaxial electrospinning, and the specific method can be found in patent CN 106498558A. The pretreatment method was as follows: the polyimide micro / nano hollow fibers were immersed in a 1:1 volume ratio mixture of anhydrous ethanol and acetone, and ultrasonically dispersed at 300W for 30 min at room temperature. Then, they were repeatedly rinsed with deionized water until the pH of the rinsing solution was neutral. Next, they were immersed in an ethanol solution of silane coupling agent KH-550 at a concentration of 15-25 mg / mL and magnetically stirred until homogeneous. Finally, they were removed and dried in a vacuum oven at 80℃ for 4 h.

[0043] The KH-560 used in the following examples was purchased from Shanghai McLean Biotechnology Co., Ltd. (AR, 97.0%).

[0044] The hydroxylated graphene used in the following examples was purchased from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., with a sheet diameter of 1-3 μm and a thickness of 1-5 nm.

[0045] The silicone rubber used in the following examples was purchased from Shanghai Maclean Biochemical Technology Co., Ltd. (viscosity 5000 mPa / s). The anhydrous ethanol used in the following examples was purchased from Shanghai Maclean Biotechnology Co., Ltd. (AR, 99.5%). The KH-550 used in the following examples was purchased from Shanghai Maclean Biotechnology Co., Ltd. (AR, 99.0%). The polylactic acid used in the following examples was purchased from Shanghai Maclean Biotechnology Co., Ltd. (Mw ~20,000). The polyvinyl alcohol used in the following examples was purchased from Shanghai Maclean Biochemical Technology Co., Ltd. (Type 1797, degree of alcoholysis: 98.0~99.0 mol%). The PEDOT:PSS solution used in the following examples was purchased from Shanghai Ouyi Organic Optoelectronic Materials Co., Ltd. (solid content 1.5%).

[0046] The nano-carbon black particles used in the following examples were purchased from Shanghai Maclean Biotechnology Co., Ltd. (AR, 99.5%). Example 1 The embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The following embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given. However, the protection scope of the present invention is not limited to the following embodiments.

[0047] like Figures 1-2The figures show a cross-sectional view of the resistive flexible pressure sensor provided in this embodiment, and a concave hexagonal array mold for fabricating the upper and lower encapsulation layers and the low conductivity layer, respectively. The sensor includes an upper encapsulation layer 1, a low conductivity layer 2, a high conductivity layer 4, a lower encapsulation layer 7, and a signal electrode 8. The upper encapsulation layer, the low conductivity layer, and the lower encapsulation layer all employ a pore structure composed of concave hexagonal holes, giving them a negative Poisson's ratio characteristic. The high conductivity layer has linear, regular cracks penetrating its thickness, dividing it into multiple discontinuous square blocks. The lower encapsulation layer has two through-holes, each containing a signal electrode. The upper end of the signal electrode is electrically connected to the high conductivity layer, and the lower end protrudes 300 μm relative to the bottom of the lower encapsulation layer.

[0048] The resistive flexible pressure sensor of this embodiment is manufactured according to the following steps: Step 1: Prepare the upper and lower encapsulation layers. Add 8.98g of silicone rubber to 4.5mL of anhydrous ethanol and stir continuously in an 85℃ constant temperature water bath until dissolved. Then add 1mL of ethanol solution of 20mg / mL silane coupling agent KH-550 and stir for 5min until completely dissolved. Then slowly add 1g of pretreated polyimide micro / nano hollow fiber while stirring at low speed. Stir mechanically for 30min and let stand for 15min to remove bubbles. Then add 30g of edible salt and stir until mixed evenly to obtain the mixed liquid slurry.

[0049] The mixed liquid slurry was slowly poured into a 3D-printed concave hexagonal array mold and pre-cured in a 60℃ oven for 3 hours. The sample was then immersed in 40℃ deionized water for 12 hours to fully dissolve and remove edible salt particles using a salt immersion method. The sample was then removed, dried and cured at 80℃ for 3 hours, and allowed to cool naturally to room temperature, yielding the initial blanks for the upper and lower encapsulation layers. Both the upper and lower encapsulation layers had a thickness of 700 μm, an electrical conductivity of 0.0005 S / cm, and an elastic modulus of 1.3 MPa.

[0050] The upper encapsulation layer preform was placed in a plasma cleaner and treated with O2 plasma to activate the surface hydroxyl groups. Two through-holes, penetrating the thickness of the lower encapsulation layer preform, were created using laser drilling. These through-holes correspond to the electrode connection areas of the highly conductive layer. The inner walls of the through-holes were activated with O2 plasma, and conductive silver paste was poured into the through-holes and cured at 60°C for 2 hours to form the signal electrode. The O2 plasma treatment parameters were 50W and 20s. The lower end of the signal electrode protrudes 300μm beyond the bottom of the lower encapsulation layer.

[0051] Step 2: Prepare a highly conductive layer Add 0.5g PVA to 5mL of deionized water, stir in a 90℃ constant temperature water bath until completely dissolved, and cool to room temperature; then add PEDOT:PSS solution (containing 1.2g PEDOT:PSS), 0.05g hydroxylated graphene and 0.05g nano carbon black particles in sequence, stir for 10min, sonicate at 200W for 15min, let stand for 10min to degas, and obtain a highly conductive slurry.

[0052] A highly conductive layer paste was applied to the lower encapsulation layer using screen printing and then cured in an 80℃ oven for 30 minutes to form the highly conductive layer. The screen printing speed was 5 mm / s, and the screen printing pressure was 0.2 MPa. The highly conductive layer had a thickness of 200 μm, a conductivity of 3600 S / cm, and an elastic modulus of 1 MPa.

[0053] A 532nm wavelength laser was used to etch crack guide grooves on the surface of a highly conductive layer at a power of 10mW and a scanning speed of 100μm / s. The crack guide grooves were 1μm deep, 15μm wide, and 80μm apart.

[0054] Gently wipe the surface of the highly conductive layer with anhydrous ethanol swabs to remove etching residues and dry it with nitrogen gas; then place it in a plasma cleaner and treat it with O2 plasma to activate the surface hydroxyl groups; the O2 plasma treatment parameters are 50W power and 20s time.

[0055] Step 3: Prepare a low conductivity layer Mix 5g of silicone rubber with 2.5g of polylactic acid, add 10mL of anhydrous ethanol to adjust the viscosity to 600mPa·s, and stir in an 80℃ constant temperature water bath for 15min until uniform; then add 0.08g of hydroxylated graphene, 0.08g of nano carbon black particles and 15g of edible salt in sequence, sonicate at 300W for 30min, and let stand for 20min to degas, to obtain a low conductivity layer slurry.

[0056] The low-conductivity layer slurry was slowly poured into a 3D-printed concave hexagonal array mold and pre-cured in a 60℃ oven for 3 hours. The sample was then immersed in 40℃ deionized water for 12 hours, and edible salt particles were completely dissolved and removed using a salt immersion method. The sample was then removed, dried and cured at 80℃ for 3 hours, and allowed to cool naturally to room temperature to obtain the low-conductivity layer. The low-conductivity layer had a thickness of 1000 μm, an electrical conductivity of 8 S / cm, and an elastic modulus of 1.5 MPa.

[0057] Step 4: Sensor Assembly KH-560 adhesive was sprayed onto the surface of the high conductivity layer. The low conductivity layer was aligned with the high conductivity layer and gently pressed together. The layers were allowed to stand at room temperature for 30 minutes for initial cross-linking, and then dried at 80°C for 1 hour.

[0058] Then, spray KH-560 adhesive onto the surface of the low conductivity layer, align the upper encapsulation layer with the low conductivity layer, press gently to adhere, let stand at room temperature for 30 minutes for initial cross-linking, and then dry at 80℃ for 1 hour.

[0059] The obtained device was fixed on a tension and compression machine, and the constant temperature module was turned on and set to 40℃. The temperature was increased from room temperature to 40℃ at a rate of 5℃ / min. The temperature was held for 10 minutes, and then the device was subjected to 80 cycles of loading and unloading under a pressure of 30 kPa to form a through crack along the thickness direction of the highly conductive layer. The temperature was held for another 30 minutes to stabilize the crack, and then the temperature was reduced to room temperature at a rate of 3℃ / min. This completed the fabrication of the inverted ultrasensitive resistive flexible pressure sensor based on the negative Poisson's ratio structure.

[0060] Figure 3 This is a schematic diagram illustrating the principle of crack guide groove etching and crack propagation after cyclic ballast loading in this embodiment. A parallel array of guide grooves is formed on the surface of the high-conductivity layer using laser etching, creating a pre-defined channel for stress concentration. Subsequently, under a controlled temperature of 40°C, 80 cycles of loading-unloading are performed at a pressure of 30 kPa and a loading rate of 1 mm / min. Utilizing the extreme stress concentration effect at the guide grooves, the crack propagates directionally along the axis of the guide grooves, ultimately forming a continuous through-crack within the high-conductivity layer.

[0061] Figure 4 This diagram illustrates the interaction principle between the highly conductive layer PEDOT:PSS and hydroxylated graphene in this embodiment. By employing hydroxylated graphene, stable hydrogen bonds are formed between the hydroxyl groups and the sulfonic acid groups in the PEDOT:PSS molecular chain. Combined with the π-π conjugation between the graphene sheets and PEDOT:PSS, the surface energy difference is effectively reduced, promoting the uniform dispersion of graphene in the matrix. Furthermore, the π-π interaction between PEDOT:PSS and graphene results in a highly ordered arrangement of the PEDOT conjugated chains, enabling effective charge transfer between PEDOT and graphene. This transforms the PEDOT chain from a benzene structure to a quinone structure, improving the conductivity and electrical stability of the highly conductive layer, thereby further enhancing the sensitivity and stability of the sensor.

[0062] Figure 5This diagram illustrates the sensing mechanism and local conductive path of the resistive flexible pressure sensor provided in this embodiment. Initially, due to the through-crack in the highly conductive layer, current cannot be conducted along the continuous mesh path of the highly conductive layer. The electron transport path at the crack is from the highly conductive layer to the less conductive layer, bypassing the crack and returning to the highly conductive layer, repeating this process. This is equivalent to connecting several low-resistance highly conductive layers and high-resistance low-conductive layers in series. When pressure is applied to the sensor, the less conductive layer undergoes lateral contraction due to the negative Poisson's ratio effect, causing the crack in the highly conductive layer to tend to close. At this time, the main electron transport path is through the highly conductive layer of the sensor. In the diagram, R1 and R2 represent the resistances of the segments separated by the crack in the highly conductive layer in the initial state; R3 represents the equivalent resistance of the less conductive layer in the initial state; and R represents the equivalent resistance of the conductive path through the highly conductive layer under pressure.

[0063] Figure 6 The pressure sensing characteristic curve of the resistive flexible pressure sensor provided in this embodiment shows that: within the pressure operating range of 0-15 kPa, the sensor sensitivity S is approximately 33.8 kPa. -1 When the pressure range is 15-40 kPa, the sensitivity S is approximately 9.4 kPa. -1 .

[0064] Figure 7 This is the stepped pressure characteristic test curve of the resistive flexible pressure sensor prepared in this embodiment. Stepped pressure loading tests were conducted on the sensor, and the results show that within a pressure range of 0-30 kPa, the sensor can achieve a stable and continuous electrical response, exhibiting excellent pressure sensing performance and operational stability.

[0065] Figure 8 The graph shows the stability test results of the resistive flexible pressure sensor in this embodiment under 5000 cycles of periodic loading / unloading within a pressure range of 0-20 kPa. The test results show that after 5000 cycles, the sensor maintains stable electrical characteristics, fully demonstrating that the sensor has excellent long-term stability, good consistency, and repeatability.

[0066] The above-described embodiments are merely preferred embodiments of the present invention, and are described in a relatively specific and detailed manner. They are not intended to limit the present invention. Any modifications, variations, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An inverted-chip ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure, characterized in that: The flexible pressure sensor has a stacked structure, consisting of an upper encapsulation layer with negative Poisson bit characteristics, a low conductivity layer with negative Poisson bit characteristics, a high conductivity layer with positive Poisson ratio characteristics, and a lower encapsulation layer with negative Poisson bit characteristics, from top to bottom. The upper encapsulation layer, the low conductivity layer, and the lower encapsulation layer all employ a pore structure composed of concave hexagonal holes, which gives them a negative Poisson's ratio characteristic. The highly conductive layer has linear, regular cracks that penetrate its thickness, which divide the highly conductive layer into multiple discontinuous square blocks. The lower encapsulation layer has two through holes inside, and a signal electrode is cast into each through hole. The upper end of the signal electrode is electrically connected to the high conductivity layer, and the lower end protrudes 100-500μm relative to the bottom of the lower encapsulation layer.

2. The inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to claim 1, characterized in that: The concave hexagonal hole has an angle α = 60°-75°, a length of 400-600μm, a width of 300-400μm, and a spacing of 700-1000μm between two adjacent concave hexagonal holes.

3. The inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to claim 1, characterized in that: The width of the regular crack is 10-20 μm, and the distance between two adjacent cracks is 60-120 μm.

4. The inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to claim 1, characterized in that: The low conductivity layer is prepared by mixing silicone rubber, polylactic acid, hydroxylated graphene and nano carbon black particles, and the elastic modulus of the low conductivity layer is 1.2-1.8 MPa.

5. The inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to claim 1, characterized in that: The highly conductive layer is prepared by mixing polyvinyl alcohol (PVA), PEDOT:PSS, hydroxylated graphene, and nano-carbon black particles, and the elastic modulus of the highly conductive layer is 0.8-1.3 MPa.

6. The inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to claim 1, characterized in that: Both the upper and lower encapsulation layers are made of silicone rubber composite material, which consists of silicone rubber, polyimide micro / nano hollow fibers, and silane coupling agent KH-550. The elastic modulus of both the upper and lower encapsulation layers is 1.0-1.6 MPa.

7. The inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure according to claim 1, characterized in that: The thickness of the high conductivity layer is 10-300 μm, and the conductivity is not less than 3000 S / cm; the thickness of the low conductivity layer is 0.5-2 mm, and the conductivity is not higher than 15 S / cm; the thickness of the upper encapsulation layer and the lower encapsulation layer are both 0.5-2 mm, and the conductivity is not higher than 0.001 S / cm.

8. A method for fabricating an inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure as described in any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Prepare the upper and lower encapsulation layers. Silicone rubber is added to anhydrous ethanol and continuously stirred in a constant temperature water bath at 80-90℃ until dissolved. Then, an ethanol solution of silane coupling agent KH-550 with a concentration of 15-25 mg / mL is added and stirred until completely dissolved. While stirring, polyimide micro / nano hollow fibers are slowly added and ultrasonically mixed evenly. Then, mechanically stirred for 20-40 minutes and allowed to stand to remove bubbles to obtain a silicone rubber composite slurry. Then, edible salt is added at 2-5 times the total mass of the composite slurry and stirred until evenly mixed to obtain a mixed liquid slurry. Based on the total mass of silicone rubber, polyimide micro / nano hollow fibers, and silane coupling agent KH-550 as 100%, polyimide micro / nano hollow fibers account for 6%-12%, silane coupling agent KH-550 accounts for 0.1%-0.3%, and the balance is silicone rubber. The mixed liquid slurry was slowly poured into the 3D-printed concave hexagonal array mold and pre-cured in an oven at 55-65℃ for 2-4 hours. Then, the sample was immersed in deionized water at 35-45℃ for 10-14 hours to fully dissolve and remove edible salt particles using a salt immersion method. The sample was then removed, dried and cured at 75-85℃ for 1.5-4.5 hours, and allowed to cool naturally to room temperature to obtain the initial blanks of the upper and lower encapsulation layers. The upper encapsulation layer preform is placed in a plasma cleaner and O2 plasma treatment is used to activate the surface hydroxyl groups. Two through holes penetrating the thickness of the lower encapsulation layer preform are made using laser drilling. The through holes correspond to the electrode connection area of ​​the high conductivity layer. The inner wall of the through holes is activated by O2 plasma treatment. Conductive silver paste is poured into the through holes and cured at 55-65℃ for 1-3 hours to form the signal electrode. The O2 plasma treatment parameters are 40-60W and 15-25s. The lower end of the signal electrode protrudes 100-500μm from the bottom of the lower encapsulation layer. Step 2: Prepare a highly conductive layer Polyvinyl alcohol (PVA) is added to deionized water and stirred in a constant temperature water bath at 85-95℃ until completely dissolved. After cooling to room temperature, a PEDOT:PSS solution with a solid content of 1-3%, hydroxylated graphene, and nano-carbon black particles are added. The mixture is stirred for 5-15 minutes, ultrasonically mixed until homogeneous, and allowed to stand for 5-15 minutes to remove bubbles, thus obtaining a highly conductive slurry. Based on the total mass of PVA, PEDOT:PSS, hydroxylated graphene, and nano-carbon black particles as 100%, PVA accounts for 20%-30%, hydroxylated graphene accounts for 1.2%-3%, nano-carbon black particles account for 1.8%-4.2%, and the remainder is PEDOT:PSS. The highly conductive paste is applied to the lower encapsulation layer using screen printing and then dried in an oven at 75-85℃ for 20-40 minutes to cure. The coating speed is 3-5 mm / s and the coating pressure is 0.1-0.2 MPa. A 532nm wavelength laser was used to etch crack guide grooves on the surface of a highly conductive layer at a power of 10-20 mW and a scanning speed of 100-200 μm / s. The crack guide grooves had a depth of 1-2 μm, a width of 10-20 μm, and a spacing of 60-120 μm. Wipe the surface of the highly conductive layer with anhydrous ethanol swabs to remove etching residue, then dry with nitrogen. It was then placed in a plasma cleaner and treated with O2 plasma to activate the surface hydroxyl groups; the O2 plasma treatment parameters were 40-60W power and 15-25s time. Step 3: Prepare a low conductivity layer Take silicone rubber, polylactic acid, hydroxylated graphene, nano-carbon black particles and edible salt in a mass ratio of 1:0.4-0.6:0.01-0.03:0.01-0.03:1-5. Mix silicone rubber and polylactic acid, add anhydrous ethanol to adjust the viscosity to 500-700 mPa∙s, stir until uniformly mixed, then add hydroxylated graphene, nano-carbon black particles and edible salt in sequence, ultrasonically disperse at 250-350W for 20-40 min, let stand to degas for 15-25 min to obtain a low conductivity layer slurry. The low conductivity layer slurry was poured into a 3D-printed concave hexagonal array mold and pre-cured in an oven at 55-65℃ for 2-4 hours. Then, the sample was immersed in deionized water at 35-45℃ for 10-14 hours to fully dissolve and remove edible salt particles using a salt immersion method. The sample was then removed, dried and cured at 75-85℃ for 1.5-4.5 hours, and allowed to cool naturally to room temperature to obtain the low conductivity layer. Step 4: Sensor Assembly Spray KH-560 adhesive onto the surface of the high conductivity layer, align the low conductivity layer with the high conductivity layer and gently press to adhere, let stand at room temperature for 20-40 minutes for initial cross-linking, and then dry at 75-85℃ for 0.5-1.5 hours. Then, spray KH-560 adhesive onto the surface of the low conductivity layer, align the upper encapsulation layer with the low conductivity layer and gently press to adhere it. Allow it to stand at room temperature for 20-40 minutes for initial cross-linking, and then dry it at 75-85℃ for 0.5-1.5 hours to complete the overall stacking assembly. The obtained device is fixed in a tension and compression press, and heated from room temperature to 35-45℃ at a heating rate of 4-6℃ / min. It is held at this temperature for 5-15 minutes, and then subjected to 70-90 cycles of loading and unloading under a pressure of 0-50kPa to form a through crack in the highly conductive layer along the thickness direction. The crack is stabilized by holding the device at this temperature for another 20-40 minutes, and then cooled to room temperature at a rate of 2-4℃ / min. This completes the fabrication of the inverted ultrasensitive resistive flexible pressure sensor based on a negative Poisson's ratio structure.

Citation Information

Patent Citations

  • Flexible strain sensor with crack structure and preparation method thereof

    CN105783697A

  • Coaxial electrospun polyimide micro / nano hollow structure material and preparation method thereof

    CN106498558A

  • Flexible pressure sensor based on crack array structure and preparation method of sensor

    CN109655180A

  • Wide-range flexible resistance type pressure sensor and preparation method thereof

    CN113340484A

  • Strain sensor array based on negative Poisson's ratio structure and preparation method and application thereof

    CN114076564A