A method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation

By forming a polymer film in the interface transition zone and regulating the interface chemical environment, the problem of insufficient interfacial bond strength between alkali slag repair mortar and old concrete substrate was solved, realizing the transformation of interface failure mode and construction simplicity, and providing a quantifiable evaluation of interface strengthening.

CN122562468BActive Publication Date: 2026-11-17CCCC FIRST HIGHWAY XIAMEN ENGINEERING CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611036032.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-07-13
Publication Date
2026-11-17
Estimated Expiration
2046-07-13

AI Technical Summary

Technical Problem

Existing polymer emulsion modified repair mortar technology has failed to effectively enhance the interfacial bond strength between alkali slag repair mortar and old concrete substrate, resulting in easy delamination and damage at the interface, and lacks systematic emulsion screening methods and ease of construction.

Method used

By forming a polymer film in the interfacial transition zone and regulating the interfacial chemical environment, and by designing the ratio of alkali activator and polymer emulsion, combined with an appropriate curing regime, the interfacial damage mode is transformed from interfacial peeling to substrate cohesive damage.

Benefits of technology

This study achieves interfacial strengthening between alkali slag repair mortar and old concrete substrate, simplifies construction procedures, reduces costs, and provides a quantifiable evaluation method for interfacial strengthening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122562468B_ABST
    Figure CN122562468B_ABST
Patent Text Reader

Abstract

This invention discloses a method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation. This invention relates to the field of concrete repair mortar technology. The method involves preparing slag, fine aggregate, alkali activator, polymer emulsion, and mixing water according to a specified ratio, stirring to obtain the repair mortar, and then applying it to the surface of a pretreated old concrete substrate. Through a specific curing regime, interfacial chemical regulation and structural strengthening are achieved, transforming the bond failure mode from interfacial failure to substrate cohesive failure. The advantages of this invention are: it is the first to actively utilize the interfacial film-forming behavior of polymer emulsion to regulate the interfacial chemical environment, synergistically strengthening the repair interface from both chemical bonding and physical densification dimensions. The process is simple and controllable, and applicable to repair and reinforcement projects of various existing concrete structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of concrete repair mortar technology, specifically a method for enhancing the bonding strength of repair mortar based on polymer emulsion interface film formation. Background Technology

[0002] Preventing concrete crack propagation, surface spalling, and erosion holes has become a key focus of the construction industry. Alkali slag cement, made from slag and activated by an alkali activator (water glass + sodium hydroxide), has advantages such as early strength, rapid hardening, good durability, and low carbon emissions. It has been proven to be a suitable material for repair projects. However, the insufficient bond strength between alkali slag repair mortar and the old concrete substrate is a key bottleneck restricting its application in engineering. The interface between the repair layer and the substrate is often a weak point in mechanical structure and is prone to interfacial peeling failure under load.

[0003] Researchers have already attempted to modify alkali slag repair mortar using polymer emulsions to improve its bonding properties. A search revealed: Chinese patent CN202210373364.9 (hereinafter referred to as D1) discloses "a repair method for alkali-activated slag material modified with polyacrylic acid emulsion". This patent modifies alkali-activated slag material by adding 1-2 parts of polyacrylic acid emulsion (PAA, solid content ≥30%). The mechanism of action is described as follows: the polyacrylic acid emulsion fills the gaps in the amorphous cementitious material, embeds itself in the matrix and interlocks to form a network structure, reducing microcracks and shrinkage. However, D1 clearly states that the bonding experiment was first destroyed at the bonding interface, that is, the interface was not fundamentally strengthened. The interface is still the weakest link in the mechanical system of the whole repair system. D1's understanding of the mechanism of action of polymer emulsion in alkali-activated repair system is completely limited to the level of "physical filling inside the matrix". It regards the polymer as an inert filler and fails to recognize the special behavior of polymer emulsion particles in the interface transition zone and its ability to actively regulate the interface chemical environment.

[0004] Chinese patent CN105837137B (hereinafter referred to as D2) discloses "a composite reinforced rapid repair mortar". This patent uses redispersible latex powder and VAE emulsion to penetrate into the voids of old concrete matrix, forming a polymer and cement stone inter-filling structure. At the same time, it utilizes the expansion property of sulfoaluminate cement to fill the capillary voids on the surface of old concrete with ettringite, increasing the mechanical interlocking force. However, D2 is fundamentally different from this invention: (1) Regarding the cement system, D2 uses a sulfoaluminate cement system, whose pore solution pH value is usually 11-12, while the present invention uses an alkaline slag system, whose pore solution pH value is >13. The two have an essential difference in interfacial chemical environment—the highly alkaline environment (pH >13) of the alkaline slag system places higher demands on the chemical stability of the polymer emulsion, and the dissolution-condensation behavior of slag and the ion (Al) in the pH >13 environment are different. 3+ Ca 2+ OH - The migration rate and concentration of D2 are orders of magnitude different from those of the sulfoaluminate cement system (pH≈11-12). The polymer interfacial behavior knowledge obtained by D2 in the low alkalinity sulfoaluminate cement system cannot be directly transferred to the high alkalinity alkaline slag system. (2) At the level of mechanism cognition, D2’s understanding of the interface enhancement mechanism is still limited to the level of “physical filling + mechanical interlocking”. It does not realize that the film formed by the polymer at the interface can act as a functional barrier to regulate the chemical environment of the interface, actively change the ion concentration distribution in the interface transition zone, and thus induce the unhydrated cement particles of the substrate to undergo secondary hydration reaction, fundamentally strengthening the interface from the level of chemical bonding.

[0005] In summary, existing polymer emulsion-modified repair mortar technologies have two blind spots in their understanding of the mechanism: first, the polymer is limited to the role of a "physical filling medium," and its film-forming behavior at the interface transition zone and its active regulation function of the interface chemical environment have not been discovered; second, the essential difference in the interface chemical environment between the alkali slag system (pH>13) and the ordinary cement system (pH≈12) has not been recognized in its impact on the polymer interface behavior. Therefore, we propose a method based on polymer emulsion interface film formation to enhance the bonding strength of repair mortar. Summary of the Invention

[0006] The purpose of this invention is to provide a method for enhancing the bonding strength of repair mortar based on polymer emulsion interface film formation.

[0007] To achieve the above objectives, the present invention provides the following technical solution: a method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation, the method comprising the following steps: Step 1: Raw material preparation: Weigh out slag, fine aggregate, alkali activator, polymer emulsion, and mixing water according to the formula. The alkali activator is prepared by water glass and sodium hydroxide, and the modulus of water glass is adjusted to 1.2-2.0. The polymer emulsion is selected from styrene-butadiene emulsion, styrene-acrylic emulsion, or epoxy resin emulsion. The emulsion dosage is 3%-20% based on the mass ratio of polymer solids to cementitious materials. The alkali equivalent, i.e., the mass ratio of sodium oxide in the alkali activator to cementitious materials, is 3%-7%. The water-cement ratio is 0.35-0.65, and the mortar-cement ratio is 0.35-0.65. Step 2, Preparation of alkaline activator solution: Dissolve sodium hydroxide in water glass solution, stir well, and let stand and cool to room temperature to obtain alkaline activator solution; Step 3: Mixing the repair mortar: After dry mixing the slag and fine aggregate evenly, add the alkali activator solution and mixing water and stir until a uniform slurry is formed. Then add the polymer emulsion and continue stirring until the emulsion is evenly dispersed to obtain the polymer emulsion modified alkali slag repair mortar. Step 4, Substrate Pretreatment and Coating: Roughen and pre-wet the surface of the old concrete substrate until it reaches a saturated and dry state. Apply the repair mortar prepared in Step 3 to the pretreated substrate surface and trowel it to form a compacted shape. Step 5, Interface film formation and curing: Cur the coated specimens for 7-28 days at a temperature of 15-30℃ and a relative humidity of ≥90% to change the bond failure mode between the repair mortar and the base concrete from interface failure to cohesive failure of the base concrete.

[0008] As a further aspect of the present invention: in step one, the slag is granulated blast furnace slag of grade S95 or higher, with a density of 2.80-2.95 g / cm³. 3 The fine aggregate is standard sand with a particle size of 0.08-2.0 mm, an alkali equivalent of 4%-6% is preferred, a water-cement ratio of 0.40-0.60 is preferred, and a mortar-cement ratio of 0.40-0.60 is preferred.

[0009] As a further aspect of the present invention: in step one, the polymer emulsion is preferably a styrene-butadiene emulsion, the solid content of the styrene-butadiene emulsion is 40%-50%, the pH value is 6-10, the viscosity is less than 100 mPa·s, the glass transition temperature is 15-25℃, and the emulsion dosage is 6%-10% based on the polymer solid content to the mass ratio of cementitious material.

[0010] As a further aspect of the present invention: In step two, the modulus of the water glass stock solution is 3.0-3.5, the Baumé degree is 38-42, and the solid content is 35%-40%. The sodium hydroxide is analytical grade with a purity ≥99%. The amount of sodium hydroxide added is 8-12g per 100g of water glass stock solution, adjusting the modulus of the water glass to 1.3-1.6. After adjusting the modulus, the solid content is 38%-45%, and the standing cooling time is 3-5h.

[0011] As a further aspect of the present invention: in step three, the dry mixing time of the slag and fine aggregate is 60-90s, the stirring time after adding the alkali activator solution and mixing water is 100-150s and the stirring speed is 70-90r / min, and the stirring time after adding the polymer emulsion is 150-210s and the stirring speed is 90-110r / min.

[0012] As a further aspect of the present invention: in step four, the old concrete substrate is a concrete surface with a strength grade of C30 or above, and the surface roughness after roughening treatment is 1.5-2.5mm. The pre-wetting treatment is carried out by spraying or brushing to make the substrate surface reach a saturated surface-dry state, and the coating thickness is 5-30mm.

[0013] As a further aspect of the present invention: in step five, the curing temperature is 20±2℃, the curing humidity is ≥95%, the curing period is 14 days, the width of the interface transition zone after curing is 45-85µm, the average calcium-silicon ratio (Ca / Si) at the interface is greater than 2.0 and the average aluminum-silicon ratio (Al / Si) is greater than 0.38.

[0014] As a further aspect of the present invention: the preferred method for the styrene-butadiene emulsion is to screen the optimal emulsion from styrene-butadiene emulsion, styrene-acrylic emulsion, and epoxy resin emulsion using three-dimensional evaluation indicators: interfacial film integrity, ion migration regulation efficiency, and adhesion enhancement magnitude, and to use the interfacial chemical strengthening index as the evaluation criterion. As a basis for quantitative screening, the formula for calculating the interfacial chemical strengthening index I is as follows: ; in, This represents the average calcium-to-silicon ratio at the interface transition region. This represents the mean calcium-to-silicon ratio of the un-emulsion-doped baseline group. This represents the average aluminum-to-silicon ratio at the interface transition zone. This represents the average aluminum-to-silicon ratio of the undoped emulsion reference group. Indicates the interface density score. The value is determined based on the proportion of pore area in the backscattered electron imaging image at the interface transition region. When the proportion of pore area is ≤1%, =5, 1% < pore area ratio ≤ 3% =4.3% < pore area ratio ≤ 5% =3.5% < pore area ratio ≤ 10% =2, when the pore area ratio is >10% =1, Indicates the contribution weighting coefficient of calcium-silicon ratio and =0.40-0.50, Indicates the aluminum-silicon ratio contribution weighting coefficient and =0.20-0.30, Indicates the interface density contribution weighting coefficient and =0.20-0.40, and + + =1, when When the strength is ≥1.50, it is considered strong interfacial strengthening, and the bond failure mode is cohesive failure of the substrate concrete. When 1.20 ≤ When the value is <1.50, it is considered moderate interface strengthening, and the bond failure mode is a mixed mode of interface failure and matrix cohesive failure. A value <1.20 indicates weak interfacial strengthening, and the bonding failure mode is interfacial failure. This is determined by calculating the interfacial chemical strengthening index corresponding to the styrene-butadiene emulsion, styrene-acrylic emulsion, and epoxy resin emulsion. Select The emulsion with the highest value is selected.

[0015] Compared with the prior art, the beneficial effects of the present invention by adopting the above technical solution are as follows: 1. This invention utilizes the film-forming behavior of polymer emulsions in the interfacial transition zone to regulate the interfacial chemical environment. Combined with the synergistic design of mix proportions and curing regimes, it achieves a qualitative change in the bond failure mode from interfacial failure to cohesive failure of the substrate concrete. It solves the industry problems of insufficient interfacial bond strength between alkali slag repair mortar and old concrete substrate, the interface always being a weak mechanical link, and easy interfacial delamination failure under load. It breaks through the cognitive limitations of existing technologies that regard polymers only as inert fillers inside the matrix or physical filling media at the interface. 2. This invention establishes a quantitative evaluation system with the interfacial chemical strengthening index as the core, which can scientifically screen the optimal polymer emulsion and reveal its structure-activity relationship at the molecular level. It solves the problems of existing technologies lacking a systematic emulsion screening method and being unable to accurately predict the differences in interfacial strengthening performance of different emulsions. It clarifies that there are significant differences in the interfacial strengthening performance of different polymer emulsions, and provides a quantifiable evaluation basis for the modification design of similar repair materials. 3. This invention solves the problems of complex repair procedures, high construction costs, and difficulty in adapting to rapid on-site construction of existing concrete structures by using simple and controllable processes without the need for additional interface treatment agents or mechanical anchoring measures. It can achieve fundamental strengthening of the repair interface with conventional industrial raw materials through simple mixing and curing procedures, and can be directly applied to on-site repair operations of various existing concrete structures. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the method steps in an embodiment of the present invention; Figure 2 This is a schematic diagram comparing the interfacial chemical strengthening index in embodiments of the present invention; Figure 3 This is a schematic diagram showing a comprehensive comparison of the technical effects in the embodiments of the present invention; Figure 4 The X-ray diffraction (XRD) patterns of each group of samples in this invention are shown. Figure 5Thermogravimetric analysis (TG-DTG) curves of each group of samples in this invention; Figure 6 These are backscattered electron (BSE) morphology images of the interface transition region of each group of samples in this invention. Figure 7 These are cross-sectional morphology images of the bonded tensile failure sections of various groups of samples in this invention. Detailed Implementation

[0017] The specific embodiments of the present invention will be further described below with reference to the accompanying drawings. It should be noted that the description of these embodiments is for the purpose of helping to understand the present invention, but does not constitute a limitation of the present invention.

[0018] Furthermore, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0019] The following unified method was used for characterizing the microscopic properties and determining the failure mode in all embodiments and comparative examples of this invention: (1) X-ray diffraction (XRD) test: Powder samples from the interface transition zone of the cured sample were taken and tested using a Cu target X-ray diffractometer with a scanning range of 2. =5°-70°, scan rate 5° / min, used to analyze the phase composition of hydration products and the intensity of characteristic peaks of CASH gel; (2) Thermogravimetric analysis (TG-DTG) test: Take the powder sample in the interface transition zone and heat it from room temperature to 1000℃ at a heating rate of 10℃ / min under nitrogen atmosphere. Record the mass loss curve and differential heat flow curve. Calculate the mass loss of CASH gel, hydrotalcite and polymer, and carbonate phase in three intervals: 50-250℃, 250-550℃, and 600-900℃ respectively. (3) Backscattered electron imaging and energy dispersive spectroscopy (BSE-EDS): After the interface cross-section sample is inlaid with epoxy resin and polished, the backscattered electron image of the interface transition zone is collected by scanning electron microscope to observe the interface compactness and porosity distribution; at the same time, the energy dispersive spectroscopy is used to perform point scanning and line scanning tests, and the Ca, Si and Al element contents are tested point by point along the vertical interface direction. The average value of multiple points in the interface transition zone is taken to calculate Ca / Si and Al / Si. (4) Determination of bond failure mode: After the tensile bond test, observe the morphology of the failure surface. If the failure surface is located inside the old concrete substrate, and the surface aggregate and grout of the substrate are pulled off and attached to the side of the repair mortar, it is determined to be the cohesive failure of the substrate. If the failure surface is completely located at the interface between the repair mortar and the substrate, and there is no material residue on either side, it is determined to be the interface failure.

[0020] In the attached figures, SBRM8 corresponds to Embodiment 1, SAEM8 corresponds to Embodiment 2, EPM8 corresponds to Embodiment 3, and ARM0 corresponds to Embodiment 1. Please see the appendix Figure 1 -Appendix Figure 7 This invention relates to a method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation, the method comprising the following steps: Step 1: Raw material preparation: Weigh out the slag, fine aggregate, alkali activator, polymer emulsion, and mixing water according to the formula. The alkali activator is prepared by water glass and sodium hydroxide. The modulus of water glass is adjusted to 1.2-2.0. The polymer emulsion is selected from styrene-butadiene emulsion, styrene-acrylic emulsion, or epoxy resin emulsion. The emulsion dosage is 3%-20% based on the mass ratio of polymer solids to cementitious materials. The alkali equivalent, i.e., the mass ratio of sodium oxide in the alkali activator to cementitious materials, is 3%-7%. The water-cement ratio is 0.35-0.65, and the mortar-cement ratio is 0.35-0.65. Step 2, Preparation of alkaline activator solution: Dissolve sodium hydroxide in water glass solution, stir well, and let stand and cool to room temperature to obtain alkaline activator solution; Step 3: Mixing the repair mortar: After dry mixing the slag and fine aggregate evenly, add the alkali activator solution and mixing water and stir until a uniform slurry is formed. Then add the polymer emulsion and continue stirring until the emulsion is evenly dispersed to obtain the polymer emulsion modified alkali slag repair mortar. Step 4, Substrate Pretreatment and Coating: Roughen and pre-wet the surface of the old concrete substrate until it reaches a saturated and dry state. Apply the repair mortar prepared in Step 3 to the pretreated substrate surface and trowel it to form a compacted shape. Step 5, Interface film formation and curing: Cur the coated specimens for 7-28 days at a temperature of 15-30℃ and a relative humidity of ≥90% to change the bond failure mode between the repair mortar and the base concrete from interface failure to cohesive failure of the base concrete. Example 1

[0021] This embodiment provides a method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation, using styrene-butadiene emulsion (SBRM8) as the preferred emulsion. The specific steps are as follows: Step 1: Raw material preparation: Weigh 592.2g of S95 grade slag, 1349.8g of standard sand, 196.0g of water glass stock solution (modulus 3.3, Baumé degree 40, solid content 37.5%), 20.0g of sodium hydroxide (analytical grade, purity ≥99%), and 122.7g of emulsion liquid corresponding to 54.0g of polymer solids in styrene-butadiene emulsion (solid content 44%, pH value 6-10, viscosity <100mPa·s, glass transition temperature 20℃), and add 158.2g of water.

[0022] The alkali equivalent is controlled at 5%, the emulsion content is 8% based on the ratio of polymer solid content to cementitious material mass, the water-cement ratio is 0.50, and the mortar-cement ratio is 0.50.

[0023] Step 2: Preparation of alkaline activator solution: Dissolve 20.0g of sodium hydroxide in 196.0g of water glass stock solution, stir until the sodium hydroxide is completely dissolved, and let stand and cool to room temperature for 4 hours to obtain an alkaline activator solution with a modulus of 1.5 and a solid content of 41.8%.

[0024] Step 3: Mixing the repair mortar: Add the slag and standard sand into a planetary mortar mixer and dry mix for 60 seconds until uniform. Add the alkali activator solution and added water and stir at 80 r / min for 120 seconds until a uniform slurry is formed. Then add the styrene-butadiene emulsion and stir at 100 r / min for 180 seconds until the emulsion is evenly dispersed to obtain the styrene-butadiene emulsion modified alkali slag repair mortar.

[0025] Step 4: Substrate pretreatment and coating: Roughen the surface of the C30 concrete substrate test block to achieve a surface roughness of 2.0 mm, pre-wet it until the substrate surface reaches a saturated surface dry state, apply the repair mortar prepared in Step 3 to the substrate surface, trowel it to compact it, and apply a coating thickness of 12 mm.

[0026] Step 5, Interfacial film formation and curing: Place the specimen in a standard curing room with a temperature of 20±2℃ and a relative humidity of ≥95% for 14 days.

[0027] After curing, performance tests were conducted, and the results are as follows: The bond failure mode was cohesive failure of the substrate concrete, and the surface area of ​​the substrate with pull-out was the largest (see appendix). Figure 7 ).

[0028] A continuous and dense polymer film layer exists at the interface transition region, and the width of the interface transition region narrows to 45-85 micrometers (see appendix). Figure 6 ); Energy dispersive spectroscopy (EDS) was used to measure the calcium-to-silicon ratio at the interface. The mean is greater than 2.0, and the aluminum-silicon ratio is... The mean is greater than 0.38; X-ray diffraction analysis showed 2 A distinct CASH gel dispersion diffraction peak appears near 29.5° (see appendix). Figure 4 ); Thermogravimetric-differential thermogravimetric analysis showed that the CASH gel had the highest mass loss among all groups (see appendix). Figure 5 ).

[0029] The above data confirms that styrene-butadiene emulsion plays an optimal role in interfacial chemical regulation in alkaline slag repair mortar systems.

[0030] Line scan tests were performed on the interface transition region along the vertical direction using an energy dispersive spectrometer. Two characteristic points were selected within the interface transition region, and the calcium-silicon ratios were measured to be 2.01 and 3.86, and the aluminum-silicon ratios were 0.42 and 0.38, respectively. The average value of the two points was taken as the average element ratio at the interface.

[0031] With interfacial chemical strengthening index Conduct quantitative evaluation and take =0.45、 =0.25、 =0.30, under the conditions of this embodiment, the reference group without emulsion was not added. =1.28、 =0.31, calculated as follows: ; ; Backscattered electron imaging analysis shows that the pore area in the interface transition region accounts for approximately 0.8%. Scoring criteria (≤1%) =5, substituting into the formula, we get =2.85.

[0032] ≥1.50, judged as strong interface strengthening, which is completely consistent with the cohesive failure mode of the substrate concrete observed in practice, and The value was the highest among the three emulsion groups, and quantitatively confirmed that the styrene-butadiene emulsion was the optimal emulsion. Example 2

[0033] The difference between this embodiment and Embodiment 1 is that the styrene-butadiene emulsion is replaced with styrene-acrylic emulsion (solid content 45%, pH value 8-9, viscosity 80-3000 mPa·s). In the styrene-acrylic emulsion, 54.0g of polymer solids corresponds to 120.0g of emulsion liquid. The remaining proportions and steps are the same as in Embodiment 1.

[0034] Tests were conducted after 14 days of curing, and the results are as follows: The bond failure mode was cohesive failure of the substrate concrete, but the area of ​​the pulled-out substrate surface was smaller than that in Example 1 (see Appendix). Figure 7 ).

[0035] The polymer film continuity is moderate at the interface transition region, and the width of the interface transition region is 60-100 micrometers (see appendix). Figure 6 ); Energy dispersive spectroscopy (EDS) was used to measure the calcium-to-silicon ratio at the interface. The average value is 1.8-2.0, and the aluminum-silicon ratio is... The mean is 0.37-0.39; The CASH gel mass loss was slightly lower than in Example 1 (see Appendix). Figure 4 Appendix Figure 5 ).

[0036] Line scan tests were performed on the interface transition region along the vertical direction using an energy dispersive spectrometer. Two characteristic points were selected within the interface transition region, and the calcium-silicon ratios were measured to be 1.81 and 2.85, and the aluminum-silicon ratios were 0.37 and 0.39, respectively. The average value of the two points was taken as the average elemental ratio at the interface.

[0037] Calculated with the same weights and the same benchmark value : ; ; Backscattered electron imaging analysis shows that the pore area accounts for approximately 2.5%, according to... Scoring criteria (1%-3%) =4, calculated to =2.33.

[0038] ≥1.50 is considered strong interface enhancement, but its The value is lower than that in Example 1, which quantitatively reflects that the overall interfacial strengthening ability of styrene-acrylic emulsion is weaker than that of styrene-butadiene emulsion.

[0039] The main reason is that the proportion of styrene units in the molecular structure of styrene-acrylic emulsion is lower than that in styrene-butadiene emulsion, and the molecular chain contains hydrophilic acrylate polar groups. The polymer film formed by it has weaker compactness and hydrophobic barrier ability than that of styrene-butadiene emulsion, and its barrier effect on high-alkali activating liquid is limited, resulting in a relatively weaker degree of ion enrichment and secondary hydration induction effect at the interface transition region. Example 3

[0040] The difference between this embodiment and Embodiment 1 is that the styrene-butadiene emulsion is replaced with an epoxy resin emulsion (20% solid content). The 43.2g of polymer solids in the epoxy resin emulsion corresponds to 216.0g of emulsion liquid. The added water is adjusted to 62.2g to keep the water-to-binder ratio unchanged at 0.50. The remaining proportions and steps are the same as in Embodiment 1.

[0041] Tests were conducted 14 days after curing, and the results are as follows: The bond failure mode was cohesive failure of the substrate concrete, but the surface area of ​​the substrate with pull-out was the smallest, with only the central part being pulled out (see Appendix). Figure 7 ).

[0042] Line scan tests were performed on the interface transition region along the vertical direction using an energy dispersive spectrometer. Two characteristic points were selected within the interface transition region, and the calcium-silicon ratios were measured to be 1.80 and 2.56, and the aluminum-silicon ratios were 0.34 and 0.24, respectively. The average value of the two points was taken as the average element ratio at the interface.

[0043] The continuity and compactness of the polymer film are poor in the interfacial transition region (see appendix). Figure 6 ); Energy dispersive spectroscopy (EDS) was used to measure the calcium-to-silicon ratio at the interface. The average value is 1.8-2.0, and the aluminum-silicon ratio is... The mean is 0.24-0.34; The mass loss of CASH gel was significantly lower than that in Example 1 (see Appendix). Figure 4 Appendix Figure 5 ).

[0044] Calculated with the same weights and the same benchmark value : ; ; Backscattered electron imaging analysis shows that the pore area accounts for approximately 7%, according to Scoring criteria (5%-10%) =2, calculated to =1.60.

[0045] It just barely exceeds the threshold for strong interface enhancement, but its The value was only 56% of that in Example 1, quantitatively reflecting that the epoxy resin emulsion had the weakest interfacial strengthening ability.

[0046] The main reason is that the film-forming mechanism of epoxy resin emulsion is chemical reaction curing rather than physical fusion. The continuity and flexibility of the film structure formed at the interface transition zone are not as good as those of styrene-butadiene emulsion, and its alkali barrier ability and internal curing effect are weaker.

[0047] Comparative Example 1 (Unadulterated emulsion baseline group ARM0) The difference between this comparative example and Example 1 is that no polymer emulsion is added in step one, and the amount of water added is adjusted to 224.2g to maintain a water-to-gel ratio of 0.50. The remaining steps are the same as in Example 1.

[0048] Tests were conducted 14 days after curing, and the results are as follows: The bond failure mode was interfacial failure, meaning the repair mortar completely delaminated from the base concrete at the interface (see attached). Figure 7 ).

[0049] There are obvious gaps and holes in the interface transition area (see appendix). Figure 6 ); Energy dispersive spectroscopy (EDS) was used to measure the calcium-to-silicon ratio at the interface. All less than 2.0, aluminum-silicon ratio Significantly lower than Example 1; The CASH gel mass loss was the lowest among all groups (see appendix). Figure 4 Appendix Figure 5 ).

[0050] Line scan tests were performed on the interface transition region along the vertical direction using an energy dispersive spectrometer. Two characteristic points were selected within the interface transition region, and the calcium-silicon ratios were measured to be 1.12 and 1.76, and the aluminum-silicon ratios were 0.21 and 0.25, respectively. The average value of the two points was taken as the average elemental ratio at the interface.

[0051] Calculated using the same weights and the same benchmark value =0.99, <1.20 indicates weak interface strengthening, consistent with experimental results of interface destruction.

[0052] This comparative example demonstrates that without the addition of polymer emulsion, alkali slag repair mortar cannot form a polymer film at the interface transition zone or achieve interface chemical environment regulation, making the interface a weak mechanical link.

[0053] Comparative Example 2 (Low Dosage of Polyacrylic Acid Emulsion) This comparative example is analyzed with reference to the existing technology of polyacrylic acid emulsion modification scheme: The existing technology discloses the modification of alkali-activated slag materials by using low-dosage polyacrylic acid emulsion. Its mechanism of action is that the polyacrylic acid emulsion fills the gaps in amorphous cementitious materials, embeds itself into the matrix and interlocks to form a network structure, and reduces microcracks.

[0054] The polymer solid content of this scheme is extremely low, far below the content range of the present invention.

[0055] At such extremely low dosages, the number density of polyacrylic acid polymer particles in the matrix is ​​insufficient to aggregate and fuse at the interface transition zone to form a continuous polymer film. The polymer particles are dispersed and filled in the pores of the matrix before reaching the interface transition zone, making it impossible to establish a barrier to regulate the interface chemical environment.

[0056] The existing technology itself clearly states that its bonding tests all fail first at the bonding interface, meaning that the interface is still the weakest point in terms of mechanics.

[0057] The low-dosage scheme failed to achieve the transition from interfacial destruction mode to substrate cohesive destruction. The fundamental reason is that it did not recognize the regulatory function of the polymer on the interfacial chemical environment after film formation in the interfacial transition region. The polymer was only used as a physical filling medium inside the matrix, and the dosage was seriously insufficient to form a continuous film layer in the interfacial transition region.

[0058] Comparative Example 3 (VAE scheme for sulfoaluminate cement system) This comparative example is analyzed with reference to the existing technology of VAE emulsion scheme for sulfoaluminate cement system: The existing technology discloses the use of redispersible latex powder and VAE emulsion to penetrate into the voids of old concrete matrix and form a structure in which polymer and cement stone are mutually filled.

[0059] However, this solution has two key differences from the present invention that are not comparable.

[0060] First, system differences: This scheme uses a sulfoaluminate cement system, whose pore solution pH value is significantly lower than that of the alkaline slag system of the present invention. In the highly alkaline environment of the alkali slag system, the ester groups of the vinyl acetate units in the VAE emulsion will undergo significant hydrolysis, leading to continuous deterioration of the structural integrity of the VAE polymer film during the curing process and loss of its barrier function against the alkali-activated solution.

[0061] In contrast, the hydrophobic benzene ring of the styrene unit in styrene-butadiene emulsion exhibits excellent chemical stability under highly alkaline conditions. This is the fundamental reason why the teachings of existing VAE technology cannot be directly transferred to alkaline slag systems.

[0062] Second, the mechanism is different: the interface enhancement of this scheme is only at the level of "physical penetration and filling + ettringite expansion and mechanical interlocking", without involving the active regulation of the interface chemical environment by the polymer membrane.

[0063] Therefore, even if VAE emulsion is applied to the alkaline slag system according to the dosage and curing system of this invention, VAE cannot maintain an effective polymer membrane barrier in a high-alkali environment, cannot achieve the interfacial chemical regulation effect of ion enrichment-induced secondary hydration, and thus cannot achieve the transformation of the bonding failure mode from interfacial failure to substrate cohesive failure.

[0064] Comparative Example 4 (Horizontal comparison of three emulsions, verification of unpredictability) This comparative example verifies the unpredictability of optimal emulsion selection by comparing test data from Examples 1, 2, and 3 under identical conditions. The comparative data show that the three emulsions exhibit significantly different adhesion-enhancing effects and a marked gradient in their interfacial chemical strengthening indices under identical formulations and curing regimes, demonstrating that the selection of the optimal emulsion was unpredictable prior to this invention.

[0065] Summary and comparison of technical effects To visually demonstrate the performance differences between the various embodiments and the comparative examples, the following parameters were included: 14-day tensile bond strength improvement rate, bond failure mode, average interfacial calcium-silicon ratio, average interfacial aluminum-silicon ratio, and interfacial chemical strengthening index. The six core indicators of CASH gel quality loss are summarized below: Table 1 Comparison of technical effects of each embodiment and comparative example.

[0066] As shown in Table 1, the interfacial chemical strengthening index of Example 1 (SBRM8 group) The performance of the three emulsions was the highest among all groups, with the highest corresponding increase in 14-day tensile bond strength and CASH gel mass loss. The bond failure mode was cohesive failure within the substrate concrete. Example 2 (SAEM8 group) showed moderate performance, while Example 3 (EPM8 group) had the lowest performance among the three emulsions. Comparative Example 1 (ARM0, the baseline group without emulsion) showed the lowest values ​​for interface failure and all indicators. The three emulsions... The value gradient quantitative verification confirmed the decisive influence of emulsion type on the interface strengthening effect.

[0067] Features compared with existing technologies To clearly demonstrate the essential differences between this invention and existing technologies in core dimensions such as polymer action localization, interface enhancement mechanism, and adhesion failure mode, a comparison of features in each dimension is summarized below: Table 2. Comparison of features between the present invention and prior art.

[0068] As shown in Table 2, compared with the existing technology that positions polymers as "inert fillers inside the matrix" or "interfacial physical penetration filling media", this invention achieves two fundamental breakthroughs: First, at the cognitive level, it is the first time that the film-forming behavior of polymer emulsions at the interface transition zone of the alkali slag repair system and its active regulation function on the interface chemical environment have been discovered; Second, at the effect level, it achieves a qualitative change in the bond failure mode from "interfacial failure" to "cohesive failure of the substrate concrete", rather than just a quantitative increase in bond strength. Existing technologies clearly record that their bond experiments all fail at the interface, and the cement system used is fundamentally different from that of this invention.

[0069] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Any variations and modifications can be made by those skilled in the art without departing from the spirit and scope of the invention. Therefore, any modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention, without departing from the scope of the invention, fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation, characterized in that, The method includes the following steps: Step 1: Raw material preparation: Weigh out slag, fine aggregate, alkali activator, polymer emulsion, and mixing water according to the formula. The alkali activator is prepared by water glass and sodium hydroxide, and the modulus of water glass is adjusted to 1.2-2.

0. The polymer emulsion is selected from styrene-butadiene emulsion, styrene-acrylic emulsion, or epoxy resin emulsion. The emulsion dosage is 3%-20% based on the mass ratio of polymer solids to cementitious materials. The alkali equivalent, i.e., the mass ratio of sodium oxide in the alkali activator to cementitious materials, is 3%-7%. The water-cement ratio is 0.35-0.65, and the mortar-cement ratio is 0.35-0.

65. Step 2, Preparation of alkaline activator solution: Dissolve sodium hydroxide in water glass solution, stir evenly, and let stand and cool to room temperature to obtain alkaline activator solution; Step 3: Mixing the repair mortar: After dry mixing the slag and fine aggregate evenly, add the alkali activator solution and mixing water and stir until a uniform slurry is formed. Then add the polymer emulsion and continue stirring until the emulsion is evenly dispersed to obtain the polymer emulsion modified alkali slag repair mortar. Step 4, Substrate Pretreatment and Coating: Roughen and pre-wet the surface of the old concrete substrate until it reaches a saturated and dry state. Apply the repair mortar prepared in Step 3 to the pretreated substrate surface and trowel it to form a compacted shape. Step 5, Interface film formation and curing: Curing the coated specimens for 7-28 days at a temperature of 15-30℃ and a relative humidity of ≥90% to change the bond failure mode between the repair mortar and the base concrete from interface failure to cohesive failure of the base concrete. The polymer emulsions were screened from styrene-butadiene emulsions, styrene-acrylic emulsions, and epoxy resin emulsions using three-dimensional evaluation indicators: interfacial film integrity, ion migration regulation efficiency, and adhesion enhancement magnitude. The interfacial chemical strengthening index was also considered. As a basis for quantitative screening, the formula for calculating the interfacial chemical strengthening index I is as follows: ; in, This represents the average calcium-to-silicon ratio at the interface transition region. This represents the mean calcium-to-silicon ratio of the un-emulsion-doped baseline group. This represents the average aluminum-to-silicon ratio at the interface transition zone. This represents the average aluminum-to-silicon ratio of the undoped emulsion reference group. Indicates the interface density score. The value is determined based on the proportion of pore area in the backscattered electron imaging image at the interface transition region. When the proportion of pore area is ≤1%, =5, 1% < pore area ratio ≤ 3% =4.3% < pore area ratio ≤ 5% =3.5% < pore area ratio ≤ 10% =2, when the pore area ratio is >10% =1, Indicates the contribution weighting coefficient of calcium-silicon ratio and =0.40-0.50, Indicates the aluminum-silicon ratio contribution weighting coefficient and =0.20-0.30, Indicates the interface density contribution weighting coefficient and =0.20-0.40, and + + =1, when When the strength is ≥1.50, it is considered strong interfacial strengthening, and the bond failure mode is cohesive failure of the substrate concrete. When 1.20 ≤ When the value is <1.50, it is considered moderate interface strengthening, and the bond failure mode is a mixed mode of interface failure and matrix cohesive failure. A value <1.20 indicates weak interfacial strengthening, and the bonding failure mode is interfacial failure. This is determined by calculating the interfacial chemical strengthening index corresponding to the styrene-butadiene emulsion, styrene-acrylic emulsion, and epoxy resin emulsion. Select The emulsion with the highest value is selected.

2. The method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation according to claim 1, characterized in that, In step one, the slag is S95 grade or higher granulated blast furnace slag with a density of 2.80-2.95 g / cm³. 3 The fine aggregate is standard sand with a particle size of 0.08-2.0 mm, an alkali equivalent of 4%-6%, a water-cement ratio of 0.40-0.60, and a cement-sand ratio of 0.40-0.

60.

3. The method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation according to claim 2, characterized in that, In step one, the polymer emulsion is a styrene-butadiene emulsion with a solid content of 40%-50%, a pH value of 6-10, a viscosity of less than 100 mPa·s, a glass transition temperature of 15-25℃, and an emulsion dosage of 6%-10% based on the mass ratio of polymer solid content to cementitious material.

4. The method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation according to claim 3, characterized in that, In step two, the water glass stock solution has a modulus of 3.0-3.5, a Baumé degree of 38-42, and a solid content of 35%-40%. The amount of sodium hydroxide added is 8-12g per 100g of water glass stock solution, adjusting the water glass modulus to 1.3-1.

6. After adjusting the modulus, the solid content is 38%-45%, and the standing cooling time is 3-5h.

5. The method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation according to claim 4, characterized in that, In step three, the dry mixing time of the slag and fine aggregate is 60-90s, the stirring time after adding the alkali activator solution and mixing water is 100-150s and the stirring speed is 70-90r / min, and the stirring time after adding the polymer emulsion is 150-210s and the stirring speed is 90-110r / min.

6. The method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation according to claim 5, characterized in that, In step four, the old concrete substrate is a concrete surface with a strength grade of C30 or above. The surface roughness after roughening is 1.5-2.5mm. The pre-wetting treatment is carried out by spraying or brushing to make the substrate surface reach a saturated surface-dry state, and the coating thickness is 5-30mm.

7. The method for enhancing the bonding strength of repair mortar based on polymer emulsion interfacial film formation according to claim 6, characterized in that, In step five, the curing temperature is 20±2℃, the curing humidity is ≥95%, the curing period is 14 days, and after curing, the width of the interface transition zone is 45-85µm, the average calcium-silicon ratio at the interface is greater than 2.0 and the average aluminum-silicon ratio is greater than 0.38.

Citation Information

Patent Citations

  • A composite enhanced rapid repair mortar

    CN105837137B

  • Polyacrylic emulsion modified alkali-activated slag material for repairing and preparation method of polyacrylic emulsion modified alkali-activated slag material

    CN114956748A