A method for fabricating electronic components with side-metallized interconnects
By performing double-sided base gold sputtering separately and dry etching twice, the problem of bubbling and discoloration at the comb edge during the fabrication of side-mounted interconnect electronic components was solved, achieving high-quality metallized interconnect.
Patent Information
- Application Number
- CN202611080194.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-07-21
AI Technical Summary
Existing side-metallized interconnect electronic components are prone to defects such as bubbling and discoloration during the manufacturing process, especially bubbling at the edges of the comb after electroplating deposition.
By using a method of separate double-sided base gold sputtering, base gold is first sputtered and deposited on one side, followed by dry etching, and then base gold is sputtered and deposited on the other side. Excess metal is removed by two dry etching processes, which solves the problem of bubbling and discoloration at the edge of the comb.
This effectively avoids bubbling and discoloration at the edges of the comb, improving the manufacturing quality and reliability of electronic components.
Smart Images

Figure CN122588511B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of manufacturing small electronic components, and more specifically, to a method for manufacturing electronic components with side-metallized interconnects. Background Technology
[0002] To meet the miniaturization requirements of electronic components, their metallization interconnection methods have evolved from traditional single-sided and double-sided metallization to three-sided and four-sided metallization, that is, in addition to metallization of the front and back sides, metallization of the sides is also carried out.
[0003] The traditional manufacturing process for existing side-metallized interconnected electronic components is as follows: first, a comb (or venetian blind) is made, and then double-sided base metal sputtering is performed (one side is sputtered first, and then the other side is sputtered). During double-sided base metal sputtering, metallization is formed not only on the front and back sides of each comb tooth of the comb (or venetian blind), but also on the sides of each comb tooth of the comb (or venetian blind).
[0004] The traditional manufacturing process of existing side-mounted metallized interconnect electronic components has the following shortcomings: the sputtered surface is prone to bubbling after electroplating, which leads to defects such as bubbling and discoloration at the edges of the comb (or louver) on that surface after dry etching. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a method for manufacturing electronic components with side-mounted metallized interconnects, which solves the defects such as bubbling and discoloration at the edges of the comb in existing processes.
[0006] A method for fabricating an electronic component with side-mounted metallized interconnects includes the following steps: S2, magnetron sputtering of base gold from the front side of the comb-shaped ceramic substrate; S3, first dry etching, removes the base gold from the back of the comb-shaped ceramic substrate; S4, front side photoresist is sprayed, dried, exposed, developed, and metal is deposited to form a ceramic substrate with metal-patterned front and side sides; S5, magnetron sputtering of base gold from the back of a comb-shaped ceramic substrate; S6 involves spraying photoresist on the back, drying, exposing, developing, and depositing metal to form a ceramic substrate with metal-patterned front, back, and side surfaces. S7, the second dry etching, removes the base metal that is not covered by the deposited metal on the ceramic substrate patterned by the deposited metal on the front, back and sides.
[0007] Optionally, the comb-shaped ceramic substrate is manufactured by the following steps: S1, the raw ceramic substrate undergoes a first cleaning, a first drying, cutting, a second cleaning, plasma cleaning and ion beam cleaning, and a second drying in sequence to form a comb-shaped ceramic substrate.
[0008] Optionally, in S1, during the first cleaning, acetone, isopropanol, anhydrous ethanol, oil stain cleaner, and dilute sulfuric acid are used in sequence for cleaning, and during the second cleaning, acetone, isopropanol, and pure water are used in sequence for cleaning.
[0009] Optionally, in S1, both the first and second drying processes are carried out in an oven at a temperature of 80°C to 150°C.
[0010] Optionally, in S1, the cutting is performed using an abrasive wheel cutter, and the cut results in a comb-shaped ceramic substrate. Each comb tooth is 20mm to 50mm long, 0.5mm to 3mm wide, and 0.1mm to 0.5mm thick, with a spacing of 0.1mm to 0.3mm between adjacent comb teeth.
[0011] Optionally, in S1, plasma cleaning is performed for 5 to 10 minutes at 500W to 1000W, with argon and O2 introduced, wherein the argon is at 10 sccm to 100 sccm and the O2 is at 10 sccm to 100 sccm; ion beam cleaning is performed for 2 to 8 minutes at a beam current of 150 mA to 200 mA.
[0012] Optionally, in S2 and S5, the sputtering power is 300W~700W and the argon flow rate is 1000sccm~2000sccm.
[0013] Optionally, in S2 and S5, the sputtering order of the base gold on the front or back side is Ti, Pt, Au; the target thickness of the base gold on the front side is: Ti layer 1000 Å~3000 Å, Pt layer 1000 Å~3000 Å, Au layer 1000 Å~3000 Å; the target thickness of the base gold on the back side is: Ti layer 1000 Å~3000 Å, Pt layer 1000 Å~3000 Å, Au layer 1000 Å~3000 Å.
[0014] Optionally, in S3 and S7, dry etching is performed in a plasma etching machine.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention separates the double-sided base gold sputtering. First, one side is sputtered to deposit and thicken the base gold, and then the other side is sputtered to deposit the base gold. Through two dry etching processes, the defects such as bubbling and discoloration at the edges of the comb are solved in the existing process. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 This is a product photo of Embodiment 1 of the present invention; Figure 2 This is a photograph of the product in Comparative Example 1 of this invention. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0019] The technical solution of the present invention will be described in detail below with reference to specific embodiments. These specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described again in some embodiments.
[0020] In Example 1 and Comparative Example 1 below, the comb teeth are 30mm long, 2mm wide, 0.4mm thick, and 0.2mm apart.
[0021] Example 1 A method for fabricating an electronic component with side-mounted metallized interconnects includes the following steps: S1, the raw ceramic substrate undergoes a first cleaning, a first drying, cutting, a second cleaning, plasma cleaning and ion beam cleaning, and a second drying in sequence to form a comb-shaped ceramic substrate.
[0022] The first cleaning process involves sequentially using acetone, isopropanol, anhydrous ethanol, oil stain remover, and dilute sulfuric acid for heated ultrasonic cleaning. After the heated ultrasonic cleaning, the ceramic substrate is rinsed with pure water. The purpose of the first cleaning is to make the ceramic substrate clean and easy to cut.
[0023] Both the first and second drying processes were carried out in an oven at a temperature of 80℃~150℃.
[0024] The cutting process uses an abrasive wheel cutter to cut the ceramic substrate into a comb-like shape.
[0025] The purpose of the second cleaning is to remove dust and dirt (the cleaning process uses acetone, isopropanol, and pure water in sequence).
[0026] Plasma cleaning is performed in a plasma cleaner for 10 minutes at a power of 750W, with argon and O2 introduced at a concentration of 50 sccm for both argon and O2.
[0027] Ion beam cleaning is performed in an ion beam cleaner for 5 minutes at a beam current of 150 mA.
[0028] S2, magnetron sputtering of the base metal from the front side of the comb-shaped ceramic substrate.
[0029] The magnetron sputtering coating machine was used with the sputtering power set to 500W and the argon flow rate set to 1600sccm. The sputtering sequence of the base gold was Ti, Pt, and Au, and the target thickness was 2000 angstroms for each film layer (i.e., 2000 angstroms for Ti layer, 2000 angstroms for Pt layer, and 2000 angstroms for Au layer on the front side).
[0030] S3, the first dry engraving, removes the base gold from the back of the comb-shaped ceramic substrate.
[0031] This dry etching was performed in a plasma etching machine. This dry etching process etched away the Ti, Pt, and Au formed on the back side of the comb-shaped ceramic substrate during magnetron sputtering in S2.
[0032] S4 involves spraying photoresist on the front side, drying, exposing, developing, and depositing metal to form a ceramic substrate with metal-patterned front and side surfaces.
[0033] S5, magnetron sputtering of the base metal from the back of a comb-shaped ceramic substrate.
[0034] The magnetron sputtering coating machine was used with the sputtering power set to 500W, the argon flow rate set to 1600sccm, and the sputtering sequence being Ti, Pt, Au. The target thickness was 2000 angstroms for each film layer (i.e., 2000 angstroms for Ti layer, 2000 angstroms for Pt layer, and 2000 angstroms for Au layer on the back side).
[0035] S6 involves spraying photoresist on the back, drying, exposing, developing, and depositing metal to form a ceramic substrate with metal-patterned front, back, and side surfaces.
[0036] S7, the second dry etching, removes the base metal not covered by deposited metal on the ceramic substrate patterned by deposited metal on the front, back and sides, to obtain a ceramic substrate with side metallized interconnects.
[0037] This dry etching was performed in a plasma etching machine, where the underlying gold not covered by the deposited metal was etched away.
[0038] In this embodiment, the ceramic substrate with side metallized interconnects is cut a second time to obtain the electronic component unit with side metallized interconnects.
[0039] The product photos in this embodiment are as follows: Figure 1 .
[0040] Comparative Example 1 A method for fabricating an electronic component with side-mounted metallized interconnects includes the following steps: S1, the raw ceramic substrate undergoes a first cleaning, a first drying, cutting, a second cleaning, plasma cleaning and ion beam cleaning, and a second drying in sequence to form a comb-shaped ceramic substrate.
[0041] The first cleaning process involves sequentially using acetone, isopropanol, anhydrous ethanol, oil stain remover, and dilute sulfuric acid for heated ultrasonic cleaning. After the heated ultrasonic cleaning, the ceramic substrate is rinsed with pure water. The purpose of the first cleaning is to make the ceramic substrate clean and easy to cut.
[0042] Both the first and second drying processes were carried out in an oven at a temperature of 80℃~150℃.
[0043] The cutting process uses an abrasive wheel cutter to cut the ceramic substrate into a comb-like shape.
[0044] The purpose of the second cleaning is to remove dust and dirt (cleaning can be done sequentially using acetone, isopropanol, pure water, etc.).
[0045] Plasma cleaning is performed in a plasma cleaner for 10 minutes at a power of 750W, with argon and O2 introduced at a concentration of 50 sccm for both argon and O2.
[0046] Ion beam cleaning is performed in an ion beam cleaner for 5 minutes at a beam current of 150 mA.
[0047] S2, first perform magnetron sputtering of the base gold from the front side of the comb-shaped ceramic substrate, and then perform magnetron sputtering of the base gold from the back side of the comb-shaped ceramic substrate.
[0048] The magnetron sputtering coating machine was used with the sputtering power set to 500W and the argon flow rate set to 1600sccm. The sputtering sequence of the base gold was Ti, Pt, and Au, and the target thickness was 2000 angstroms for each film layer (i.e., 2000 angstroms Ti layer, 2000 angstroms Pt layer, 2000 angstroms Au layer on the front side, and 2000 angstroms Ti layer, 2000 angstroms Pt layer, 2000 angstroms Au layer on the back side).
[0049] S3 involves spin-coating photoresist on the front and back sides, drying, exposure, development, and metal deposition to form a ceramic substrate with metal-patterned front, back, and side surfaces.
[0050] S4, dry etching, removes the base metal not covered by deposited metal on the front, back and side metallized ceramic substrate to obtain a ceramic substrate with side metallized interconnects.
[0051] This dry etching was performed in a plasma etching machine, where the underlying gold not covered by the deposited metal was etched away.
[0052] The ceramic substrate with side-metallized interconnects fabricated in this comparative example is cut a second time to obtain electronic component units with side-metallized interconnects.
[0053] The product photos in this comparison are as follows: Figure 2 .
[0054] from Figure 1 and Figure 2 It can be seen that, Figure 2 The comb's edges developed defects such as bubbling and discoloration. Figure 1 These phenomena do not occur. The blistering is caused by diffraction during magnetron sputtering of the base metal. Metal from the unsputtered surface will diffract onto the back side. If this is not removed by dry etching, it will appear as... Figure 2 Steps formed at the edges of the comb teeth can easily cause bubbling during deposition and annealing processes. This invention addresses this by using single-sided magnetron sputtering of the base metal, dry etching away excess diffracted metal, then increasing the film thickness to the required level through deposition, and then magnetron sputtering the base metal on the second side again. This allows the diffracting effect generated by the second side sputtering to affect the surface of the first side deposition layer, which is then dry-etched away in step S7.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for fabricating an electronic component with side-mounted metallized interconnects, characterized in that, The steps are as follows: S1, the raw ceramic substrate is sequentially subjected to the first cleaning, the first drying, cutting, the second cleaning, plasma cleaning and ion beam cleaning, and the second drying to form a comb-shaped ceramic substrate; S2, magnetron sputtering of base gold from the front side of the comb-shaped ceramic substrate; S3, the first dry engraving, removes the base gold from the back of the comb-shaped ceramic substrate; S4, front side photoresist is sprayed, dried, exposed, developed, and metal is deposited to form a ceramic substrate with metal-patterned front and side sides; S5, magnetron sputtering of base gold from the back of a comb-shaped ceramic substrate; S6 involves spraying photoresist on the back, drying, exposing, developing, and depositing metal to form a ceramic substrate with metal-patterned front, back, and side surfaces. S7, second dry etching, removes the base gold not covered by deposited metal on the ceramic substrate patterned by deposited metal on the front, back and sides. In S3 and S7, dry etching is performed in a plasma etching machine.
2. The method for fabricating an electronic component with side-mounted metallized interconnects according to claim 1, characterized in that, In S1, during the first cleaning, acetone, isopropanol, anhydrous ethanol, oil stain cleaner, and dilute sulfuric acid are used in sequence. During the second cleaning, acetone, isopropanol, and pure water are used in sequence.
3. The method for fabricating an electronic component with side-mounted metallized interconnects according to claim 1, characterized in that, In S1, both the first and second drying processes are carried out in an oven at a temperature of 80℃~150℃.
4. The method for fabricating an electronic component with side-mounted metallized interconnects according to claim 1, characterized in that, In S1, the cutting is done using an abrasive wheel cutter, which forms a comb-shaped ceramic substrate. Each comb tooth is 20mm~50mm long, 0.5mm~3mm wide, and 0.1mm~0.5mm thick, with a spacing of 0.1mm~0.3mm between adjacent comb teeth.
5. The method for fabricating an electronic component with side-mounted metallized interconnects according to claim 1, characterized in that, In S1, plasma cleaning lasts for 5 to 10 minutes at 500 W to 1000 W, with argon and O2 introduced at 10 sccm to 100 sccm and 10 sccm to 100 sccm respectively. Ion beam cleaning lasts for 2 to 8 minutes at a beam current of 150 mA to 200 mA.
6. The method for fabricating an electronic component with side-mounted metallized interconnects according to claim 1, characterized in that, In S2 and S5, the sputtering power is 300W~700W and the argon flow rate is 1000sccm~2000sccm.
7. The method for fabricating an electronic component with side-mounted metallized interconnects according to claim 6, characterized in that, In S2 and S5, the sputtering sequence of the base gold on the front or back side is Ti, Pt, Au; the target thickness of the base gold on the front side is: Ti layer 1000 Å~3000 Å, Pt layer 1000 Å~3000 Å, Au layer 1000 Å~3000 Å; the target thickness of the base gold on the back side is: Ti layer 1000 Å~3000 Å, Pt layer 1000 Å~3000 Å, Au layer 1000 Å~3000 Å.
Citation Information
Patent Citations
Metallization coating method for through hole of film circuit
CN107419230A
Thin film circuit with large-area side wall metal pattern and preparation method thereof