A microneedle array with super-high silicon needle electrically conductive and a preparation method thereof

CN122682183APending Publication Date: 2026-09-04SUZHOU HENGZHIQING BIOTECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610062483.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-01-25
Filing Date
2026-01-18
Publication Date
2026-09-04

AI Technical Summary

Technical Problem

现有技术中的导电微针大多由金属材料制备而成,但此种方式制备得到的钢针,对皮肤的创伤面积较大,容易导致面瘫,并且金属微针导电性能太强,受试者容易感觉到皮肤因电流通过产生明显的酸涩和不适感

Benefits of technology

[0020]本公开的微针阵列,阵列上硅针的高度比普通微针要高得多,更容易将药物递送至皮肤真皮层的中部位置,更易于药物吸收。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122682183A_ABST
    Figure CN122682183A_ABST
Patent Text Reader

Abstract

The present disclosure relates to a conductive microneedle array with super-high silicon needles and a preparation method thereof, characterized in that the microneedle array comprises silicon needles and a silicon substrate integrally formed with the silicon needles, the silicon needles are arranged in an array form on the silicon substrate, the bottom diameter of the silicon needles is 150-900 μm, the height of the silicon needles is 450-1000 μm, the hardness of the silicon needles of the microneedle array is not less than 13 N, the bottom surface of the silicon substrate of the microneedle array is uniformly coated with a conductive film with a thickness of 10-200 nm, and the conductive film is made of a metal material or a conductive alloy material. The height of the silicon needles on the microneedle array of the present disclosure is much higher than that of ordinary microneedles, and a conductive film is coated, a micro-current is generated, drug absorption is facilitated, and the irritation to the skin is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to microneedle products in the field of transdermal drug delivery, and particularly to a conductive microneedle array made of monocrystalline silicon and its preparation method. Background Technology

[0002] The skin consists of the stratum corneum, epidermis, dermis, and subcutaneous tissue. The stratum corneum, the outermost layer of the skin, is approximately 15–30 µm thick and is composed of dense keratinocytes. The epidermis lies beneath the stratum corneum, with a thickness of approximately 150–200 µm. The dermis lies beneath the epidermis, approximately 1–2 mm thick, below which lies the subcutaneous tissue. The dermis, located below the epidermis, contains blood vessels, lymphatic vessels, nerves, sensory endings, sweat glands, etc., so drugs penetrating into the dermis are quickly absorbed. Therefore, microneedles need to penetrate into the dermis to better deliver the medication and ensure maximum absorption.

[0003] Once inserted into the skin, conductive microneedles can deliver microcurrents generated by a base cell into the skin. These microcurrents can promote collagen regeneration, resulting in lifting and firming, deep skin rejuvenation, reduced risk of wound infection, and the driving of cell migration and wound healing. Currently, most conductive microneedles are made of metal materials. However, the resulting steel needles cause a large area of ​​skin trauma, potentially leading to facial paralysis. Furthermore, the high conductivity of metal microneedles can cause subjects to experience significant soreness and discomfort due to the current passing through their skin.

[0004] However, existing silicon microneedles have high resistance and poor conductivity, making them unsuitable for use as conductive microneedles. Furthermore, the height of existing silicon microneedles is generally around 50-100 μm, meaning they can only penetrate the stratum corneum. Even the highest silicon microneedle height disclosed in existing technology CN1569271A is only around 400 μm, reaching only the upper dermis, a shallow penetration that hinders drug absorption. Generally, the higher the silicon microneedle, the lower its hardness and the more prone it is to breakage. This not only reduces the reusability of microneedle products but also risks causing skin inflammation and allergies due to broken fragments.

[0005] Therefore, how to ensure that the silicone microneedles have good conductivity to conduct the microcurrent generated by the machine to achieve a lifting and firming cosmetic effect, while also ensuring that the microneedles have moderate hardness and are not easily broken, causing little trauma to the skin and not aggravating the skin's inflammatory response, is one of the urgent problems to be solved in the field of conductive silicone microneedles. Furthermore, since the silicone needles penetrate deep into the dermis, how to minimize the inflammatory response and ensure the safety of the silicone needles is also an aspect that the field of silicone microneedles needs to continuously improve. Summary of the Invention

[0006] This disclosure aims to provide a conductive microneedle array with ultra-high silica needles and its preparation method. By improving the structural design and preparation process of the microneedles, the limitations of the prior art are overcome, and a conductive microneedle array is prepared while maintaining the low allergenicity and safety of the microneedle product, providing a new solution for the field of transdermal drug delivery.

[0007] To achieve the above objectives, one aspect of this disclosure provides a conductive microneedle array with ultra-high silicon needles, characterized in that the microneedle array includes silicon needles and a silicon substrate integrally formed with the silicon needles, the silicon needles are arranged in an array on the silicon substrate, the bottom diameter of the silicon needles is 150-900 μm, the height of the silicon needles is 450-1000 μm, the hardness of the silicon needles in the microneedle array is not less than 13N, and a conductive thin film with a thickness of 10-200 nm is uniformly coated on the bottom surface of the silicon substrate of the microneedle array, the conductive thin film being made of a metal material or a conductive alloy material.

[0008] In some embodiments, the conductive film of the microneedle array is made of a metallic material; in some embodiments, the conductive film is selected from one or more of gold, silver, platinum, copper, iron, and aluminum; in some embodiments, the conductive film is made of metallic aluminum.

[0009] In some embodiments, the bottom diameter of the silicon needles in the microneedle array is 150–900 μm; in other embodiments, the bottom diameter of the silicon needles in the microneedle array is 200–900 μm, 250–900 μm, 300–900 μm, or 350–900 μm.

[0010] In some specific implementations, the bottom diameter of the microneedle array is 150μm, 160μm, 170μm, 180μm, 190μm, 200μm, 210μm, 220μm, 230μm, 240μm, 250μm, 260μm, 270μm, 280μm, 290μm, 300μm, 310μm, 320μm, 330μm, 340μm, 350μm, 360μm, 370μm, 380μm, 390μm, 400μm, 450μm, 500μm, 550μm, 600μm, 650μm, 700μm, 750μm, 800μm, 850μm, or 900μm.

[0011] In some embodiments, the height of the silicon needles in the microneedle array is 450–1000 μm; in other embodiments, the height of the silicon needles in the microneedle array is 500–1000 μm, 600–1000 μm, 700–1000 μm, 800–1000 μm, or 900–1000 μm.

[0012] In some specific embodiments, the height of the silicon needles in the microneedle array is 450μm, 460μm, 470μm, 480μm, 490μm, 500μm, 510μm, 520μm, 530μm, 540μm, 550μm, 560μm, 570μm, 580μm, 590μm, 600μm, 610μm, 620μm, 630μm, 640μm, 650μm, 660μm, 670μm, 680μm, 690μm, 700μm, 710μm, 720μm, 730μm, 740μm, 750μm, 760μm, 770μm, 780μm, 790μm, 800μm, 810μm, 820μm, 830μm, 840μm, 850μm, 860μm, 870μm, 880μm, 890μm, 900μm, 910μm, 920μm, 930μm, 940μm, 950μm, 960μm, 970μm, 980μm, 990μm, 1000μm In some embodiments, the silicon needles of the microneedle array have a hardness of not less than 13N; in some embodiments, the silicon needles of the microneedle array have a hardness of not less than 14N, not less than 16N, not less than 18N, not less than 20N, and not less than 21N.

[0013] In some specific implementations, the hardness of the silicon needles in the microneedle array is not less than 13N, not less than 13.5N, not less than 14N, not less than 14.5N, not less than 15N, not less than 15.5N, not less than 16N, not less than 16.5N, not less than 17N, not less than 17.5N, not less than 18N, not less than 18.5N, not less than 19N, not less than 19.5N, not less than 20N, not less than 20.5N, and not less than 21N.

[0014] One aspect of this disclosure provides a method for fabricating a microneedle array with ultra-high silicon needles, comprising the following steps: Using a P-type or N-type single-crystal silicon wafer as the microneedle substrate, with a resistance of 0.01 to 0.02 Ωcm, it is cleaned and dried; (2) A silicon dioxide thin film, silicon nitride thin film, or single metal thin film is formed on the silicon wafer as a masking material layer; (3) Photoresist is uniformly coated on the masking material layer described in step (2); (4) A circular array pattern with a diameter of 150-900 μm is transferred to the photoresist through a photolithography process to form an array-shaped circular masking film protective layer; (5) The masking material layers in the array that are not protected by the masking film protective layer are removed until the single-crystal silicon wafer is exposed; (6) Using the ICP-RIE system and the Bosch process, the single crystal silicon wafer exposed in step 5 is etched until an array cylinder with a height of about 450-1000 μm is etched out; (7) The mask protection layer and the masking material layer at the top of the cylinder are removed in sequence; (8) The top of the cylinder is etched with an etching solution containing 80-95 wt% KOH to form a solid micro needle tip and obtain a micro solid silicon needle array chip; (9) A conductive thin film is coated on the array chip prepared in step 8 using physical deposition or chemical deposition.

[0015] In some embodiments, the step of coating the conductive thin film in the preparation method is performed by physical deposition; in some embodiments, the physical deposition method is sputtering.

[0016] In some embodiments, the step of coating the conductive thin film in the preparation method employs chemical deposition; in some embodiments, the chemical deposition method is chemical vapor deposition. In some embodiments, the chemical vapor deposition method includes the following steps: after pretreatment of the microneedle array, a gas containing a metal source is introduced to generate a metal film on the bottom surface of the silicon substrate.

[0017] In some embodiments, the KOH-containing corrosive solution comprises 80-95 wt% of an aqueous KOH solution and 5-20 wt% of a buffer solution; in some embodiments, the KOH-containing corrosive solution comprises 85-95 wt% of an aqueous KOH solution and 5-15 wt% of a buffer solution; in some embodiments, the KOH-containing corrosive solution comprises 90-95 wt% of an aqueous KOH solution and 5-10 wt% of a buffer solution.

[0018] In some embodiments, the buffer solution comprises one or more components such as organic alcohols, inorganic salts, and sugars, and purified water; in some embodiments, the buffer solution comprises 1-50 wt% organic alcohols, 0-30 wt% inorganic salts, 0-30 wt% sugars, and purified water. In some embodiments, the organic alcohol component of the buffer solution is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, and isoamyl alcohol; in some embodiments, the inorganic salt component of the buffer solution is selected from one or more of sodium chloride, magnesium chloride, potassium chloride, and aluminum chloride; in some embodiments, the sugar component of the buffer solution is selected from one or more of fructose, glucose, and sucrose.

[0019] In some specific embodiments, the buffer solution comprises 20-50 wt% ethanol, 10-30 wt% sodium chloride, and purified water; in some specific embodiments, the buffer solution comprises 20-50 wt% propanol, 10-30 wt% sodium chloride, and purified water; in some specific embodiments, the buffer solution comprises 20-50 wt% isopropanol, 10-30 wt% sodium chloride, and purified water; in some specific embodiments, the buffer solution comprises 20-50 wt% ethanol, 10-30 wt% glucose, and purified water; in some specific embodiments, the buffer solution comprises 20-50 wt% isopropanol, 10-30 wt% glucose, and purified water.

[0020] The microneedle array disclosed herein has silicon needles that are much taller than ordinary microneedles, making it easier to deliver drugs to the middle of the dermis and thus easier for drug absorption.

[0021] The microneedle array disclosed herein ensures that the silicon needles have an ultra-high height while also maintaining moderate hardness and being resistant to breakage, thereby guaranteeing the reusability of the microneedle products.

[0022] The microneedle array disclosed herein, compared to ordinary microneedles, not only has ultra-high silica content but is also coated with a conductive film, which greatly increases the conductivity of the silica needles. This allows the microcurrent generated by the base cell to be introduced into the skin, which can promote the skin's absorption of beauty serums or medications, promote collagen regeneration, lift and tighten, deeply rejuvenate the skin, reduce the risk of wound infection, drive cell migration and promote wound healing, and at the same time reduce skin inflammation and allergy symptoms.

[0023] The microneedle array disclosed herein is simpler to manufacture and lower in cost than microneedle arrays made by directly using steel needles made of metal or by directly coating metal materials onto silicon needles. It also results in a smaller area of ​​skin trauma, reducing discomfort after microneedle insertion and lowering the risk of facial paralysis caused by metal microneedles.

[0024] Terminology Explanation To facilitate understanding of this disclosure, some technical and scientific terms are specifically defined below. Unless otherwise expressly defined herein, all other technical and scientific terms used herein have the meanings commonly understood by one of ordinary skill in the art to which this disclosure pertains.

[0025] The term "microneedle hardness" refers to the critical buckling force of a microneedle measured before it breaks using a universal testing machine through an axial compression test.

[0026] The term "bottom side of silicon substrate" refers to the side of a silicon substrate that does not have silicon pins. Attached Figure Description

[0027] Figure 1 Here is a scanning electron microscope image of the ultra-high silicon needle prepared in Example 1; Figure 2 This is a scanning electron microscope image of the ultra-high silicon needle prepared in Example 2; Figure 3 This is a schematic diagram of the ultra-high silicon needle with a conductive thin film prepared according to this disclosure; Figure 4 This is a schematic diagram of the ultra-high silicon needle with a conductive thin film prepared according to this disclosure.

[0028] Explanation of reference numerals in the attached figures Detailed Implementation

[0029] To make the technical solutions and beneficial effects of this disclosure more apparent and understandable, a detailed description is provided below by citing specific embodiments. The accompanying drawings are not necessarily drawn to scale, and local features may be enlarged or reduced to more clearly show the details of the local features; unless otherwise defined, the technical and scientific terms used herein have the same meanings as those in the technical field to which this application pertains.

[0030] In the description of this disclosure, it should be understood that the terms “center,” “upper,” “lower,” “front,” “rear,” “left,” “right,” “vertical,” “horizontal,” “top,” “bottom,” “inner,” and “outer,” etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this disclosure and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this disclosure.

[0031] Example 1: Fabrication of an ultra-high silicon needle array with a conductive thin film The basic fabrication process is as follows: (1) Use a single-crystal silicon wafer as the microneedle substrate, clean and dry it; (2) Form a silicon dioxide thin film, silicon nitride thin film or single metal thin film on the silicon wafer as a masking material layer; (3) Coat the masking material layer described in step (2) with photoresist uniformly; (4) Transfer a circular array pattern with a diameter of 500μm onto the photoresist through photolithography to form an array-shaped circular masking protective layer; (5) Remove the masking material layers in the array that are not protected by the masking protective layer until the single-crystal silicon wafer is exposed; 6) Using an ICP-RIE system and the Bosch process, the exposed single-crystal silicon wafer from step 5 is etched until an array of cylinders with a height of approximately 800 μm is etched out; (7) The mask protective layer and the masking material layer at the top of the cylinders are removed sequentially; (8) The top of the cylinders is etched using an etching solution containing KOH, wherein the KOH etching solution contains 85 wt% KOH and 15 wt% buffer solution, and the buffer solution further contains 20 wt% ethanol, 20 wt% sodium chloride and purified water, to obtain the following... Figure 1 The silicon needles shown. (9) A layer of aluminum film is uniformly coated on the bottom of the silicon needle array obtained in step (8) by chemical vapor deposition, thereby obtaining the conductive microneedle array chip.

[0032] The morphology of the prepared silicon needles was analyzed using a DB500 focused ion beam electron beam dual-beam microscope, which revealed that the bottom diameter of the silicon needle was 385 μm, the tip diameter was 51 nm, and the height of the silicon needle was 674 μm.

[0033] Example 2 Fabrication of ultra-high silicon needles under different conditions The preparation conditions and methods are the same as in Example 1, but the diameter of the circular array pattern in step four is adjusted to 900 μm, and the KOH etching solution in step eight is adjusted to contain 90 wt% KOH and 10 wt% buffer solution. The buffer solution further contains 30 wt% isopropanol, 20 wt% glucose, and purified water, resulting in the following... Figure 2 The silicon needle shown.

[0034] The morphology of the prepared silicon needles was analyzed using a DB500 focused ion beam electron beam dual-beam microscope, which revealed that the bottom diameter of the silicon needle was 775 μm, the tip diameter was 70 nm, and the height was 937 μm.

[0035] Comparative Example 1: Microneedle chip prepared according to the method disclosed in Example 1 of CN1569271A Preparation process: using single-sided polished monocrystalline silicon <100> The raw material, 500 micrometers thick, is first cleaned with a cleaning solution containing 5 parts deionized water, 1 part 30 wt% hydrogen peroxide, and 1 part 30 wt% ammonia at near 80 degrees Celsius, and then dried at 150 degrees Celsius for 10 minutes. A silicon dioxide layer approximately 1 micrometer thick is then thermally oxidized at 900–1100 degrees Celsius onto single-crystal silicon. <100> The silicon dioxide film is grown on both sides separately. Then, a layer of aluminum film, approximately 500 Å thick, is deposited on one side using vacuum deposition. A uniform 1-2 μm thick layer of Shipley 1818 photoresist is applied to the aluminum film using spin coating. After pre-baking (soft baking) at 90 degrees Celsius for 5 minutes, a solid circular mask (quartz glass coated with a chromium film is used in standard semiconductor processes, and the mask material is universal) is used to cover the single-crystal silicon with photoresist. This mask is formed in a 20×20 array within a 4 square millimeter unit, with a diameter of 80 μm and a spacing of 200 μm. <100> The substrate is exposed for 4 seconds, then developed and dried at 120 degrees Celsius for about 30 minutes. An aluminum film is etched onto the exposed areas using ion etching (RIE) technology, followed by further etching of the unprotected silicon dioxide areas. After the silicon dioxide is etched, deep reactive ion etching (DRIE) is used to etch the single-crystal silicon in the etched silicon dioxide areas. <100> The substrate is deeply etched until the etching depth reaches 150 micrometers, at which point the etching is stopped to obtain a cylinder. The photoresist, aluminum film, and silicon dioxide on the surface of the cylinder are removed, and then the cylinder is placed in a KOH solution at 40–80 degrees Celsius for etching for 30–70 minutes to obtain a pointed cone-shaped microneedle.

[0036] The morphology of the prepared silicon needles was analyzed using a DB500 focused ion beam electron beam dual-beam microscope. The solid microneedles had a tip diameter of 1 μm, a bottom diameter of 32 μm, and a height of 56 μm.

[0037] Comparative Example 2: Microneedle chip prepared according to the method disclosed in Example CN111675190A Select a single-sided polished monocrystalline silicon wafer with a (100) crystal plane. The selected monocrystalline silicon wafer is N-type with a resistivity of 5 Ω·cm. After cleaning with standard cleaning solutions RCA1 (molar ratio of water:ammonia:hydrogen peroxide is 5:1:1) and RCA2 (molar ratio of water:hydrochloric acid:hydrogen peroxide is 5:1:1), it is cleaned with deionized water and dehydrated and dried. (2) The monocrystalline silicon wafer is oxidized and grown with a layer of silicon dioxide in the order of wet oxygen-dry oxygen. The oxidation temperature is controlled below 1100℃, and the wet oxygen and dry oxygen times are both 5h. (3) A 200nm thick layer of silicon nitride is deposited on the surface of silicon dioxide by PECVD. The substrate temperature for PECVD deposition is 300-450℃, and the pressure is 10-270Pa. (4) Photoresist is then spin-coated onto silicon nitride. The pattern on the mask is transferred to the photoresist through photolithography. The pattern on the mask is an array of circular spots. The photoresist after photolithography forms an array of circular masking film. AZ9260 photoresist is used. The spin-coating speed of the photoresist is 2500 r / min, the time is 35s, and the thickness of the photoresist film is 10μm. Then, the single crystal silicon wafer is pre-baked at 95℃ for 9min. After the single crystal silicon wafer is naturally cooled, the mask pattern is photolithographically ... (5) First, the silicon nitride is dry-etched using a reactive ion etching machine. After the silicon dioxide is exposed, the silicon dioxide is wet-etched using a mixture of hydrogen fluoride and hydrofluoric acid until the single-crystal silicon wafer is exposed. In this embodiment, the reactive ion etching machine has a power of 100W, a CHF3 gas flow rate of 100sccm, a vacuum degree of 2.5Pa, and an etching time of 106min. Wet etching is performed using a mixture of hydrogen fluoride and hydrofluoric acid (BOE solution, 6 parts of 40wt% hydrogen fluoride and 1 part of 49wt% hydrofluoric acid). (6) Using an inductively coupled plasma etching system, the single-crystal silicon wafer exposed in step 5 is anisotropically etched using the deep silicon etching Bosch process to etch an array of cylinders on the single-crystal silicon wafer. In this embodiment, the power of the inductively coupled plasma etching system is 1000W, the etching and passivation time is 6s / 4s per cycle, the etching rate is 0.4μm / cycle, and the etching resistance ratio of the single crystal silicon wafer to the masking film is 42:1; (7) the masking film, silicon nitride and silicon dioxide at the top of the cylinder are removed in sequence, and the top of the cylinder is etched isotropically with KOH solution at 40-80 degrees, and the etching time is 30-70min to form a solid microneedle tip cone, and a micro solid silicon needle array chip is obtained.

[0038] The morphology of the prepared silicon needles was analyzed using a DB500 focused ion beam electron beam dual-beam microscope, which revealed that the bottom diameter of the silicon needle was 60 μm, the tip diameter was 80 nm, and the height of the silicon needle was 180 μm.

[0039] Example 3 Hardness Test Axial compression tests were conducted using a universal testing machine to measure the force required for mechanical fracture of the microneedles. The test method involved placing the microneedle tip-side up on a stainless steel plate. A P / 25 probe was used to compress the microneedle body placed on the stainless steel plate. The probe's trigger force was set to 0.049 N, and the maximum compression distance was 5 mm. The sensor recorded the pressure applied when the probe contacted the sample until the maximum compression distance was reached. The critical buckling force of the microneedle before fracture was obtained and used as an evaluation of its hardness and toughness. The results are shown in Table 1. The hardness of the silicon needles in the microneedle arrays prepared in Examples 1, 2, Comparative Example 1, and 2 were tested using the above method. The test results are as follows.

[0040] Table 1 Example 1 18.1 Example 2 16.9 Comparative Example 1 18.9 Comparative Example 2 18.3

[0041] Example 4 Needle fatigue test Using the most common pork skin as the test object, the microneedle arrays prepared in Examples 1 and 2 and Comparative Examples 1 and 2 were used as implantation chips. All arrays were 4mm*4mm in size (36 needles evenly distributed on each array). The chips were attached to the end of the implantation device. The power switch was pressed, and the rotating DC motor drove the eccentric wheel mechanism, causing the end of the implantation device to vibrate up and down with the microneedles. The frequency was controlled between 50Hz and 150Hz. The vibrating microneedles were placed naturally on the surface of the pork skin. Due to the up-and-down vibration of the microneedles, they continuously pierced the epidermis. To avoid piercing in the same place, the device was moved to another piece of pork skin every 5 seconds. The continuous acupuncture time was 20 minutes, 40 minutes, 60 minutes, 90 minutes, and 120 minutes. Five sets of acupuncture experiments were conducted for each type of microneedle. After the acupuncture process was completed, the microneedle array was removed, and the number of broken needles was observed under a microscope. The number of unbroken needles was recorded. The statistical average test results under different experimental parameters are shown in the table below.

[0042] Table 2 Example 1 36.0 36.0 36.0 33.8 31.0 Example 2 36.0 36.0 36.0 33.1 30.4 Comparative Example 1 34.0 32.2 30.0 27.4 22.8 Comparative Example 2 33.7 31.8 29.8 26.1 21.0

[0043] Conclusion: The microneedle array with ultra-high silicon needles provided in this disclosure has excellent fatigue resistance and damage resistance, and the needles will not break within 60 minutes of use.

[0044] Example 5: Skin Redness and Swelling Irritation Test Twenty subjects aged 20-30 years were randomly selected. All subjects had good skin condition with no obvious skin damage. The subjects were randomly divided into two groups of 10 each. In the first group, the left cheek used an iontophoresis device equipped with the array prepared in Example 1, and the right cheek used an iontophoresis device equipped with the array prepared in Comparative Example 1. In the second group, the left cheek used a beauty device equipped with the array prepared in Example 2, and the right cheek used an iontophoresis device equipped with the array prepared in Comparative Example 2. All subjects used the iontophoresis device on both cheeks for 3 minutes each, moving it across the skin to an unused area every 5 seconds. After use, subjects rated their subjective feelings on a scale of 1 to 10 (scores can be non-integers). Higher scores indicated more severe redness and irritation. The final score was determined by the average score of all subjects.

[0045] Table 3

[0046] Conclusion: The skin irritation caused by the array with ultra-high silica needles provided in this disclosure is basically similar to that caused by ordinary high-density microneedle arrays.

[0047] It should be understood that the above embodiments are exemplary and are not intended to encompass all possible implementations included in the claims. Various modifications and changes can be made to the above embodiments without departing from the scope of this disclosure. Similarly, the various technical features of the above embodiments can be arbitrarily combined to form other embodiments of this disclosure that may not be explicitly described. Therefore, the above embodiments only illustrate several implementations of this disclosure and do not limit the scope of protection of this patent disclosure.

Claims

1. A conductive microneedle array with ultra-high silicon needles, characterized in that, The microneedle array includes silicon needles and a silicon substrate integrally formed with the silicon needles. The silicon needles are arranged in an array on the silicon substrate. The bottom diameter of the silicon needles is 150-900 μm, the height of the silicon needles is 450-1000 μm, and the hardness of the silicon needles in the microneedle array is not less than 13N. The bottom surface of the silicon substrate of the microneedle array is uniformly coated with a conductive film with a thickness of 10-200 nm. The conductive film is made of metal material or conductive alloy material.

2. The microneedle array according to claim 1, characterized in that, The conductive film is made of a metallic material, preferably one or more of gold, silver, platinum, copper, and aluminum.

3. The microneedle array according to claim 1, characterized in that, The bottom diameter of the silicon needle is 200-900 μm, the height of the silicon needle is 500-1000 μm, and the hardness of the silicon needle in the microneedle array is not less than 14 N.

4. The microneedle array according to claim 1, characterized in that, The bottom diameter of the silicon needle is 250-900 μm, the height of the silicon needle is 600-1000 μm, and the hardness of the silicon needle in the microneedle array is not less than 15 N.

5. The microneedle array according to claim 1, characterized in that, The bottom diameter of the silicon needle is 300-900 μm, the height of the microneedle is 700-1000 μm, and the hardness of the silicon needle in the microneedle array is not less than 16 N.

6. The microneedle array according to claim 1, characterized in that, The bottom diameter of the silicon needle is 350-900 μm, the height of the microneedle is 800-1000 μm, and the hardness of the silicon needle in the microneedle array is not less than 16 N.

7. The microneedle array according to claim 1, characterized in that, The bottom diameter of the silicon needle is 350-900 μm, the height of the microneedle is 900-1000 μm, and the hardness of the silicon needle in the microneedle array is not less than 16 N.

8. A method for preparing a microneedle array as described in claim 1, characterized in that, The steps include (1) using a single-crystal silicon wafer as a microneedle substrate, cleaning and drying it; (2) forming a silicon dioxide thin film, silicon nitride thin film or single metal thin film on the silicon wafer as a masking material layer; (3) uniformly coating photoresist on the masking material layer in step (2); (4) transferring a circular array pattern with a diameter of 150-900μm onto the photoresist through a photolithography process to form an array-shaped circular masking protective layer; (5) removing the masking material layers in the array that are not protected by the masking protective layer until the single-crystal silicon wafer is exposed; (6) using IC The P-RIE system uses the Bosch process to etch the single-crystal silicon wafer exposed in step 5 until an array cylinder with a height of about 450-1000 μm is etched out; (7) the mask protection layer and the masking material layer at the top of the cylinder are removed in sequence; (8) the top of the cylinder is etched with an etching solution containing 80-95 wt% KOH to form a solid micro needle tip and obtain a micro solid silicon needle array chip; (9) a conductive film is coated on the array chip prepared in step 8 using physical deposition or chemical deposition.

9. A method for preparing a microneedle array as described in claim 8, characterized in that, The KOH-containing corrosive solution comprises 80-95 wt% of an aqueous KOH solution and 5-20 wt% of a buffer solution, wherein the buffer solution comprises 1-50 wt% of organic alcohols, 0-30 wt% of inorganic salts, 0-30 wt% of sugars, and purified water.

10. A method for preparing a microneedle array as described in claim 8, characterized in that, The KOH-containing corrosive solution comprises 85-95 wt% of an aqueous KOH solution and 5-15 wt% of a buffer solution, more preferably, the KOH-containing corrosive solution comprises 90-95 wt% of an aqueous KOH solution and 5-10 wt% of a buffer solution.

11. A method for preparing a microneedle array as described in claims 9-10, characterized in that, The buffer solution contains organic alcohols selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, and isoamyl alcohol; the buffer solution contains inorganic salts selected from one or more of sodium chloride, magnesium chloride, potassium chloride, and aluminum chloride; and the buffer solution contains sugars selected from one or more of fructose, glucose, and sucrose.

12. A method for preparing a microneedle array as described in claims 9-10, characterized in that, The buffer solution contains 20-50 wt% ethanol, 10-30 wt% glucose or sodium chloride, and purified water. Preferably, the buffer solution contains 20-50 wt% ethanol, 10-30 wt% glucose, and purified water.

13. A method for preparing a microneedle array as described in claims 9-10, characterized in that, The buffer solution contains 20-50 wt% propanol, 10-30 wt% glucose or sodium chloride, and purified water, preferably containing 20-50 wt% propanol, 10-30 wt% glucose, and purified water.

14. A method for preparing a microneedle array as described in claims 9-10, characterized in that, The buffer solution contains 20-50 wt% isopropanol, 10-30 wt% glucose or sodium chloride, and purified water, preferably 20-50 wt% isopropanol, 10-30 wt% glucose, and purified water.

15. A method for preparing a microneedle array as described in claims 8-10, characterized in that, The conductive film coating method in step (9) is chemical vapor deposition, which includes the following steps: after pre-treating the microneedle array, a gas containing a metal source is introduced to generate a metal film on the bottom surface of the silicon substrate.

16. A method for preparing a microneedle array as described in claims 8-10, characterized in that, The method for coating the metal film in step (9) is sputtering.

Citation Information

Patent Citations

  • Preparation method of miniature solid silicon needle

    CN111675190A

  • Minisize solid silicon needle array chip and its preparation method and use

    CN1569271A