A hafnium hydride-rare earth oxide composite neutron absorber and its preparation method

By combining high-entropy rare earth oxides with hafnium hydride, the brittleness and hydrogen migration problems of hafnium hydride materials were solved, and the material's microstructure uniformity, interface stability and mechanical properties were improved, thereby enhancing neutron absorption stability and high-temperature service reliability.

CN122771769BActive Publication Date: 2026-11-17XIAMEN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611241099.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17
Estimated Expiration
2046-08-17

AI Technical Summary

Technical Problem

Existing hafnium hydride materials suffer from problems such as increased brittleness, hydrogen migration and release, and unstable crystal structure during preparation and service, making it difficult to balance neutron absorption performance, structural stability, and mechanical properties.

Method used

By combining high-entropy rare earth oxides with hafnium hydride, and through ball milling, calcination, mechanical mixing and staged sintering, the hydrogen content and crystal structure of the hafnium hydride matrix phase and the high-entropy rare earth oxide functional phase are controlled to form a synergistic match between the cubic hafnium hydride matrix and the high-entropy rare earth oxide functional phase.

Benefits of technology

It improves the material's microstructure uniformity, interfacial stability, and mechanical properties, enhances neutron absorption stability and high-temperature service reliability, and strengthens the synergistic effect of neutron absorption and moderation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122771769B_ABST
    Figure CN122771769B_ABST
Patent Text Reader

Abstract

This invention discloses a hafnium hydride-rare earth oxide composite neutron absorber material and its preparation method, belonging to the technical field of special ceramics. The preparation method involves mixing at least five rare earth oxides, ball milling, and calcining to obtain high-entropy rare earth oxide powder. The high-entropy rare earth oxide powder is then mixed with hafnium hydride powder to obtain a composite powder, which is pressed into shape and then sintered under a hydrogen-containing protective atmosphere to obtain the hafnium hydride-rare earth oxide composite neutron absorber material. By introducing a high-entropy rare earth oxide functional phase into the hafnium hydride matrix and regulating the hafnium hydride matrix phase to a cubic phase structure, a synergistic improvement in the material's neutron absorption performance, mechanical properties, microstructure stability, and hydrogen retention performance can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of special ceramics, specifically to a hafnium hydride-rare earth oxide composite neutron absorber material and its preparation method. Background Technology

[0002] Hafnium hydride materials combine the neutron absorption properties of hafnium and the neutron moderation properties of hydrogen, and have promising applications in the field of neutron absorbing materials for control rods in nuclear reactors, space nuclear power plants, small nuclear power plants, and advanced fast reactors. They are of great significance for controlling reactivity, regulating neutron flux, and ensuring the safe operation of reactors.

[0003] However, several problems still exist in the preparation and service of hafnium hydride materials. First, hafnium hydride is a metal hydride, and its brittleness increases with higher hydrogen content, making it prone to cracking during sintering, processing, or thermal cycling. Second, under higher temperature service conditions, hydrogen in hafnium hydride may migrate and be released, leading to a decrease in the material's hydrogen content, which in turn reduces the moderation effect and neutron absorption stability. Third, the phase composition and crystal structure of hafnium hydride are closely related to its hydrogen content; significant differences exist in the crystal structure, microstructure stability, thermal stability, and mechanical properties of materials with different hydrogen contents.

[0004] To improve the overall performance of hydride materials, a second-phase functional component is often introduced to enhance neutron absorption, structural stability, or high-temperature performance. However, current composite approaches mostly focus on simple composites of the hafnium hydride phase and the functional phase, paying less attention to the relationship between the hydrogen content and crystal structure of the hafnium hydride matrix phase and the structural characteristics of the functional phase. Therefore, the uniformity of the functional phase distribution in the matrix, phase stability, and interfacial bonding are still limited, making it difficult to fully realize its composite effect and to simultaneously achieve the desired mechanical properties and hydrogen retention stability of the material. Summary of the Invention

[0005] The purpose of this invention is to provide a hafnium hydride-rare earth oxide composite neutron absorber material and its preparation method, so as to achieve synergistic matching between the matrix phase and the high-entropy rare earth oxide, thereby further improving the material's microstructure uniformity, interface stability, mechanical properties and service stability.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] A method for preparing a hafnium hydride-rare earth oxide composite neutron absorber material includes the following steps:

[0008] Step 1: Mix no less than five rare earth oxides to obtain a mixed powder, and then ball mill and calcine the mixed powder to obtain high entropy rare earth oxide powder; the calcination temperature is 1200℃~1500℃, and the holding time is 8h~15h.

[0009] Step 2: The high-entropy rare earth oxide powder and hafnium hydride powder are mechanically mixed under a protective atmosphere to obtain a composite powder; the mass ratio of the high-entropy rare earth oxide powder to the hafnium hydride powder is (100-a):a, where 95.0 ≤ a ≤ 99.0;

[0010] Step 3: The composite powder is pressed into shape and then sintered under a hydrogen-containing protective atmosphere to obtain a hafnium hydride-rare earth oxide composite neutron absorber material; the hydrogen-containing protective atmosphere is a mixture of H2 and inert gas, wherein the volume fraction of H2 is 15% to 60%.

[0011] Optionally, the rare earth oxide is selected from at least five of Eu2O3, Sm2O3, Dy2O3, Gd2O3, Er2O3, Y2O3, Yb2O3, and Ho2O3, and the mole fraction of any one of them is not less than 10% and not more than 35%.

[0012] Optionally, the high-entropy rare earth oxide includes at least one thermal neutron high absorption cross-section element and at least one resonance region / fast neutron absorption contributing element to balance broad neutron energy spectrum absorption; the thermal neutron high absorption cross-section element includes Eu, Sm and Gd; the resonance region / fast neutron absorption contributing element includes Dy, Er and Ho.

[0013] Optionally, in step 1, a high-energy ball mill is used, with a ball milling speed of 350 rpm to 500 rpm, a ball milling time of 12 h to 20 h, and a ball-to-material mass ratio of 3:1 to 10:1.

[0014] Optionally, the hafnium hydride powder is HfH2; the D50 particle size of the hafnium hydride powder is 1μm to 100μm, preferably 5μm to 50μm.

[0015] Optionally, the high-entropy rare earth oxide powder is a single-phase solid solution powder with a configuration entropy ΔS. conf ≥1.5R, where R is the ideal gas constant.

[0016] Optionally, in step 2, the mechanical mixing is performed using ball milling, with a mixing time of 1 to 10 hours, a ball milling speed of 100 to 300 rpm, and a ball-to-material mass ratio of 1:1 to 10:1. The protective atmosphere for the mechanical mixing is an inert gas, such as Ar.

[0017] Optionally, in step 3, the sintering is pressureless sintering with an internal furnace pressure not exceeding 0.2 MPa, a maximum sintering temperature of 700℃~900℃, and a holding time of 2h~4h; specifically, it includes the following stages:

[0018] In the first stage, the temperature is maintained at 250℃~450℃ for 0.2h~2h to remove adsorbed gas and reduce residual stress in the molded blank.

[0019] In the second stage, the temperature is kept at 700℃~900℃ for 2h~4h to achieve densification and sintering of the composite powder;

[0020] The third stage involves holding the sample at 250℃~350℃ for 0.5h~5h to compensate for the partial hydrogen loss during the densification sintering process and to regulate the hydrogen content and crystal structure of the hafnium hydride matrix phase.

[0021] In the fourth stage, the cooling rate is controlled to cool to room temperature in order to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0022] In the hydrogen-containing protective atmosphere during sintering, if the H2 volume fraction is below 15%, the hydrogen partial pressure inside the furnace is insufficient, making it difficult to compensate for the hydrogen loss during the high-temperature densification sintering stage. This results in a low hydrogen content in the final hafnium hydride matrix phase, making it prone to the formation of low-hydrogen phases such as the β phase, and reducing the hydrogen retention stability of the material. If the H2 volume fraction is above 60%, the hydrogen partial pressure inside the furnace is too high, easily leading to HfH in the hafnium hydride matrix phase. x When the x-value exceeds 1.80, the H atoms tend to become more ordered in the interstitial positions, leading to tetragonal distortion of the crystal lattice and transformation into the tetragonal phase (ε phase), which in turn affects the interfacial compatibility and mechanical stability of the composite material.

[0023] During the sintering process, the volume fraction of H2 in the hydrogen-containing protective atmosphere is in the range of 15% to 60%. By adjusting the hydrogen partial pressure in the furnace, the x value of the hafnium hydride matrix phase can be stably controlled in the range of 1.50 to 1.80, which promotes the matrix phase to be dominated by the cubic phase (δ phase). This ensures good structural coordination and interfacial compatibility between the matrix phase and the high-entropy rare earth oxide functional phase, and synergistically improves the mechanical properties, density and high-temperature hydrogen retention stability of the composite material.

[0024] Preferably, the volume fraction of H2 in the hydrogen-containing protective atmosphere of the third and fourth stages is greater than that of the first and second stages. Further, in the first and second stages, the volume fraction of H2 in the hydrogen-containing protective atmosphere is 15%–30%; in the third and fourth stages, the volume fraction of H2 in the hydrogen-containing protective atmosphere is 30%–60%. Increasing the hydrogen partial pressure in the furnace before cooling can compensate for the decrease in hydrogen content caused by hydrogen loss from the matrix surface during the high-temperature densification sintering stage, and is beneficial for controlling the hydrogen content and crystal structure of the hafnium hydride matrix phase, promoting the transformation and stabilization of the resulting hafnium hydride matrix phase into a cubic phase (δ phase) HfH. x structure.

[0025] Preferably, the furnace pressure (total pressure of sintering atmosphere) is 0.05MPa to 0.20MPa.

[0026] Further, optionally, step 3 includes:

[0027] The composite powder is pressed into shape by cold isostatic pressing, with a pressing pressure of 200MPa to 400MPa and a pressing time of 15 to 40 minutes.

[0028] The pressed green body is placed in a sintering furnace. After evacuation, inert gas is introduced to adjust the furnace pressure to 0.05 MPa–0.10 MPa. Then, H2 is introduced to increase the furnace pressure to 0.06 MPa–0.14 MPa. The temperature is then increased to 250–450 °C at a rate of 3–8 °C / min and held for 0.2–2 h. The temperature is then increased to 700–900 °C at a rate of 3–8 °C / min and held for 2–4 h. H2 is introduced again to increase the furnace pressure to 0.08 MPa–0.20 MPa. The temperature is then decreased to 250–350 °C at a rate of 3–8 °C / min and held for 0.5–5 h. Finally, the furnace is cooled to room temperature at a rate of 3–8 °C / min while maintaining the above hydrogen-containing protective atmosphere.

[0029] Optionally, the hydrogen-containing protective atmosphere for sintering is an H2 / Ar mixture.

[0030] A hafnium hydride-rare earth oxide composite neutron absorber material prepared by the above preparation method comprises a hafnium hydride matrix phase and a high-entropy rare earth oxide functional phase dispersed in the matrix phase; the mass fraction of the hafnium hydride matrix phase is 95.0 wt% to 99.0 wt%, and the total mass fraction of the high-entropy rare earth oxide functional phase is 1.0 wt% to 5.0 wt%.

[0031] Optionally, the hafnium hydride matrix phase is a cubic phase (δ phase) HfH x , where x is 1.50 to 1.80; the high-entropy rare earth oxide functional phase is a cubic solid solution in which no less than five rare earth cations are randomly occupied on the cation sublattice, and its configuration entropy ΔSconf ≥ 1.5R.

[0032] Optionally, the hydrogen content of the composite neutron absorber is 0.8 wt% to 1.2 wt%, and the relative density is not less than 92%.

[0033] In this invention, the high-entropy rare earth oxide is a single-phase solid solution functional phase formed by at least five rare earth cations in the same crystal lattice, preferably a cubic single-phase solid solution functional phase. Compared with traditional single rare earth oxides or low-component rare earth oxides, high-entropy rare earth oxides have higher configurational entropy, multi-principal element disordered distribution, and more obvious lattice distortion characteristics, which are beneficial to improving the thermal stability and microstructure stability of the functional phase itself. Furthermore, the various rare earth elements in the high-entropy rare earth oxide can also contribute to the absorption of neutrons in different energy ranges, thereby improving the overall absorption capacity of the material over a wide neutron energy spectrum.

[0034] Furthermore, due to the random occupancy of various rare earth cations in the cation sublattice of high-entropy rare earth oxides, lattice distortion, stress field fluctuations, and non-uniform coordination environments can be introduced at the local scale. This multi-principal-element disordered structure is beneficial to improving the high-temperature stability of the oxide functional phase, and its high degree of lattice distortion can hinder the diffusion and migration of hydrogen in the composite material, thereby improving the hydrogen retention capacity and high-temperature service stability of hafnium hydride-based composite materials.

[0035] Furthermore, this invention uses HfH2 powder as the hafnium hydride raw material, and controls the hydrogen content and crystal structure of the hafnium hydride matrix phase in the final composite material by controlling conditions such as hydrogen partial pressure in the sintering atmosphere, sintering temperature, holding time, and cooling atmosphere, so that the obtained hafnium hydride matrix phase is preferably a cubic phase HfH2. x Where x is 1.50 to 1.80. Meanwhile, when both the hafnium hydride matrix phase and the high-entropy rare earth oxide functional phase exhibit cubic phase characteristics in their crystal structures, they are more likely to form a structurally compatible interface relationship in the composite material. This helps to reduce the degree of interface mismatch and local stress concentration at the interface, improve the stability of the interface bonding, and help to suppress the initiation and propagation of microcracks at the interface during sintering, cooling and subsequent service, as well as alleviate the local stress concentration phenomenon caused by the difference in phase structure.

[0036] Therefore, by designing a synergistic phase structure between the hafnium hydride matrix phase and the high-entropy rare earth oxide functional phase, this invention can not only enhance the synergistic effect of neutron absorption and moderation in composite materials, but also take into account the mechanical properties, hydrogen retention stability and long-term service reliability of the materials.

[0037] The aforementioned hafnium hydride-rare earth oxide composite neutron absorbing material can be applied to neutron absorbing components in nuclear reactors. The neutron absorbing components include control rods, absorber rods, shielding absorber blocks, and other neutron absorbing functional components.

[0038] Compared with the prior art, the present invention has at least the following beneficial effects:

[0039] 1. This invention constructs a composite structure consisting of a hafnium hydride matrix phase and a high-entropy rare-earth oxide functional phase by introducing a high-entropy rare-earth oxide functional phase into a hafnium hydride matrix. The high-entropy rare-earth oxide functional phase exhibits a multi-principal element disordered distribution and high configuration entropy, which is beneficial for improving the thermal and structural stability of the functional phase itself. Furthermore, the various rare-earth elements in the high-entropy rare-earth oxide can also contribute to the absorption of neutrons in different energy ranges, thereby improving the overall absorption capacity of the material over a wide neutron energy spectrum.

[0040] 2. In this invention, the random occupancy of multiple rare earth cations in the high-entropy rare earth oxide functional phase in the same lattice can cause significant lattice distortion and local stress field fluctuations, which is beneficial to hindering the diffusion and migration of hydrogen in the material, reducing the migration and release rate of hydrogen under higher temperature conditions, and improving the hydrogen retention capacity and service stability of hafnium hydride composite materials.

[0041] 3. The high-entropy rare earth oxide functional phase introduced in this invention forms a composite system with good structural compatibility with the cubic hafnium hydride matrix phase. This is beneficial to improving the interfacial bonding state and stress transmission mode, thereby reducing the risk of crack initiation and propagation during sintering, processing and thermal cycling, which in turn helps to increase the sintering density of hafnium hydride materials and improve their mechanical properties.

[0042] 4. This invention, through the synergistic design of hafnium hydride matrix phase and high-entropy rare earth oxide functional phase, enables the material to possess the neutron absorption effect of hafnium, the neutron moderation effect of hydrogen, and the synergistic absorption effect of multiple rare earth elements on a broad neutron energy spectrum. This is beneficial to improving the material's broad-spectrum neutron absorption capability and achieving synergistic optimization of neutron absorption performance and structural stability. Attached Figure Description

[0043] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments are briefly described below. It should be understood that the following drawings are merely illustrative drawings used to assist in illustrating the technical concept of the present invention and do not constitute a limitation on the scope of protection of the present invention.

[0044] Figure 1 This is a schematic diagram of the process flow for preparing hafnium hydride-rare earth oxide composite neutron absorber material according to an embodiment of the present invention.

[0045] Figure 2 The X-ray diffraction (XRD) spectra of the composite neutron absorbing material and the comparative sample obtained in Example 1 of this invention are shown.

[0046] Figure 3 The images shown are scanning electron microscope (SEM) images and energy dispersive spectroscopy (EDS) analysis results of the composite neutron absorbing material obtained in Example 1 of this invention.

[0047] Figure 4 This is a thermal dehydrogenation temperature curve of the composite neutron absorber material obtained in Example 1 of the present invention. Detailed Implementation

[0048] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0049] Unless otherwise defined, the technical or scientific terms used in this invention shall have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.

[0050] The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material in this embodiment of the invention is as follows: Figure 1 As shown, the process includes the following steps: First, at least five rare earth oxide raw materials are mixed in a set molar ratio, and then subjected to high-energy ball milling and high-temperature calcination under a protective atmosphere. The product is then crushed, ground, and sieved to obtain single-phase high-entropy rare earth oxide powder. Subsequently, the high-entropy rare earth oxide powder is mechanically mixed with hafnium hydride powder under a protective atmosphere to obtain hafnium hydride-high-entropy rare earth oxide composite powder. Then, the composite powder is cold isostatically pressed and then sintered in stages under a hydrogen-containing protective atmosphere to obtain hafnium hydride-rare earth oxide composite neutron absorber material.

[0051] The prepared hafnium hydride-rare earth oxide composite neutron absorber material comprises a hafnium hydride matrix phase and a high-entropy rare earth oxide functional phase dispersed in the matrix phase. The high-entropy rare earth oxide functional phase is a single-phase solid solution formed by the random occupancy of no fewer than five rare earth cations on a cation sublattice. The hafnium hydride matrix phase primarily provides neutron absorption by hafnium and neutron moderation by hydrogen, while the high-entropy rare earth oxide functional phase primarily provides synergistic absorption contributions from multiple rare earth elements to neutrons in different energy ranges, and helps improve the material's microstructure stability and high-temperature service stability.

[0052] Example 1

[0053] This embodiment provides a method for preparing a hafnium hydride-rare earth oxide composite neutron absorber material.

[0054] (I) Preparation of high-entropy rare earth oxide powders

[0055] Eu2O3, Sm2O3, Dy2O3, Gd2O3 and Er2O3 were selected as rare earth oxide raw materials.

[0056] Among them, the purity of Eu2O3 powder is 99.9% and the D50 particle size is 0.35μm; the purity of Sm2O3 powder is 99.9% and the D50 particle size is 0.28μm; the purity of Dy2O3 powder is 99.9% and the D50 particle size is 0.42μm; the purity of Gd2O3 powder is 99.9% and the D50 particle size is 0.36μm; and the purity of Er2O3 powder is 99.9% and the D50 particle size is 0.40μm.

[0057] The five rare earth oxides were mixed in an equimolar ratio, with each component having a molar fraction of 20 mol%, corresponding to a configuration entropy ΔS. conf It is 1.609R.

[0058] Based on a total feed amount of 2.50g, weigh out 0.44g of Eu2O3 powder, 0.42g of Sm2O3 powder, 0.56g of Dy2O3 powder, 0.54g of Gd2O3 powder, and 0.54g of Er2O3 powder, and add them together into a zirconia ball mill jar. Use zirconia balls as the grinding medium, control the ball-to-powder mass ratio at 6:1, and carry out high-energy ball milling and mixing under an Ar protective atmosphere.

[0059] The high-energy ball milling conditions were: ball milling speed 420 rpm, ball milling time 16 h.

[0060] After ball milling, the resulting mixed powder was placed in an alumina crucible and calcined in a high-temperature furnace. The calcination conditions were: heating to 1300℃ at a rate of 5℃ / min, holding at that temperature for 10 hours, and then cooling to room temperature with the furnace. The calcined product was crushed, ground, and sieved to obtain high-entropy rare earth oxide powder A.

[0061] (II) Preparation of composite powder

[0062] Weigh 29.10g of HfH2 powder and mix it with 0.90g of the above-mentioned high-entropy rare earth oxide powder A to obtain a composite powder raw material.

[0063] The HfH2 powder has a purity of 99.0% and a D50 particle size of 16μm.

[0064] Based on the total mass of the composite powder raw materials, the content of HfH2 powder is 97.0 wt%, and the content of high entropy rare earth oxide powder A is 3.0 wt%.

[0065] HfH2 powder and high-entropy rare earth oxide powder A were added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 260 rpm, ball-to-powder mass ratio 4:1, and mixing time 5 h. After mixing, a homogeneous composite powder B was obtained.

[0066] (III) Pressing and Sintering

[0067] Composite powder B was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 250 MPa, holding time 20 min. After pressing, a circular green body was obtained.

[0068] The sintering process is as follows:

[0069] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.08 MPa, followed by the introduction of hydrogen and the adjustment of the furnace atmosphere pressure to 0.10 MPa (i.e., the volume fraction of hydrogen in the hydrogen-containing protective atmosphere is 20%).

[0070] In the first stage, the temperature is increased to 400℃ at a rate of 5℃ / min and held for 40min.

[0071] In the second stage, the temperature was increased to 800℃ at a rate of 5℃ / min and held for 3 hours.

[0072] In the third stage, hydrogen gas was continued to be introduced, and the atmosphere pressure inside the furnace was adjusted to 0.15 MPa. The temperature was then reduced to 300°C at a rate of 5°C / min and held for 1 hour.

[0073] In the fourth stage, the hydrogen-containing protective atmosphere is maintained and cooled to room temperature at 5°C / min to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0074] After sintering, a circular hafnium hydride-rare earth oxide composite neutron absorber sample S1 was obtained, with a diameter of 20 mm and a thickness of 4 mm.

[0075] Example 2

[0076] This embodiment provides a method for preparing a hafnium hydride-rare earth oxide composite neutron absorber material.

[0077] (I) Preparation of high-entropy rare earth oxide powders

[0078] Eu2O3, Sm2O3, Dy2O3, Gd2O3 and Ho2O3 were selected as rare earth oxide raw materials.

[0079] Among them, the purity of Eu2O3 powder is 99.9% and the D50 particle size is 0.35μm; the purity of Sm2O3 powder is 99.9% and the D50 particle size is 0.28μm; the purity of Dy2O3 powder is 99.9% and the D50 particle size is 0.42μm; the purity of Gd2O3 powder is 99.9% and the D50 particle size is 0.36μm; and the purity of Ho2O3 powder is 99.9% and the D50 particle size is 0.38μm.

[0080] The five rare earth oxides were mixed in an equimolar ratio, with each component having a molar fraction of 20 mol%, corresponding to a configuration entropy ΔS. conf It is 1.609R.

[0081] Based on a total feed amount of 1.80g, weigh out 0.31g of Eu2O3 powder, 0.30g of Sm2O3 powder, 0.40g of Dy2O3 powder, 0.39g of Gd2O3 powder, and 0.40g of Ho2O3 powder, and add them together into a zirconia ball mill jar. Use zirconia balls as the grinding medium, control the ball-to-powder mass ratio at 5:1, and carry out high-energy ball milling and mixing under an Ar protective atmosphere.

[0082] The high-energy ball milling conditions were: ball milling speed 400 rpm and ball milling time 14 h.

[0083] After ball milling, the resulting mixed powder was placed in an alumina crucible and calcined in a high-temperature furnace. The calcination conditions were: heating to 1280℃ at a rate of 5℃ / min, holding at that temperature for 9 hours, and then cooling to room temperature with the furnace. The calcined product was crushed, ground, and sieved to obtain high-entropy rare earth oxide powder A.

[0084] (II) Preparation of composite powder

[0085] Weigh 29.40g of HfH2 powder and mix it with 0.60g of the above-mentioned high-entropy rare earth oxide powder A to obtain a composite powder raw material.

[0086] The HfH2 powder has a purity of 99.0% and a D50 particle size of 20μm.

[0087] Based on the total mass of the composite powder, the content of HfH2 powder is 98.0 wt%, and the content of high entropy rare earth oxide powder A is 2.0 wt%.

[0088] HfH2 powder and high-entropy rare earth oxide powder A were added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 220 rpm, ball-to-powder mass ratio 3:1, and mixing time 4 h. After mixing, a homogeneous composite powder B was obtained.

[0089] (III) Pressing and Sintering

[0090] Composite powder B was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 230 MPa, holding time 20 min. After pressing, a circular green sheet was obtained.

[0091] The sintering process is as follows:

[0092] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.08 MPa, followed by the introduction of hydrogen and the adjustment of the furnace atmosphere pressure to 0.10 MPa.

[0093] In the first stage, the temperature is increased to 360℃ at a rate of 5℃ / min and held for 25min.

[0094] In the second stage, the temperature was increased to 740℃ at a rate of 5℃ / min and held for 120min.

[0095] In the third stage, hydrogen gas was continued to be introduced, and the atmosphere pressure inside the furnace was adjusted to 0.14 MPa. The temperature was then reduced to 280°C at a rate of 5°C / min and held for 1 hour.

[0096] In the fourth stage, the hydrogen-containing protective atmosphere is maintained and cooled to room temperature at 5°C / min to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0097] After sintering, a circular hafnium hydride-rare earth oxide composite neutron absorber sample S2 was obtained, with a diameter of 20 mm and a thickness of 4 mm.

[0098] Example 3

[0099] This embodiment provides a method for preparing a hafnium hydride-rare earth oxide composite neutron absorber material.

[0100] (I) Preparation of high-entropy rare earth oxide powders

[0101] Eu2O3, Sm2O3, Dy2O3, Gd2O3 and Yb2O3 were selected as rare earth oxide raw materials.

[0102] The purity of Eu2O3 powder is 99.9%, and the D50 particle size is 0.35 μm; the purity of Sm2O3 powder is 99.9%, and the D50 particle size is 0.28 μm; the purity of Dy2O3 powder is 99.9%, and the D50 particle size is 0.42 μm; the purity of Gd2O3 powder is 99.9%, and the D50 particle size is 0.36 μm; and the purity of Yb2O3 powder is 99.9%, and the D50 particle size is 0.39 μm.

[0103] The five rare earth oxides were mixed in an equimolar ratio, with each component having a molar fraction of 20 mol%, corresponding to a configuration entropy ΔS. conf It is 1.609R.

[0104] Based on a total feed amount of 3.00g, weigh out 0.53g of Eu2O3 powder, 0.50g of Sm2O3 powder, 0.67g of Dy2O3 powder, 0.64g of Gd2O3 powder, and 0.66g of Yb2O3 powder, and add them together into a zirconia ball mill jar. Use zirconia balls as the grinding medium, control the ball-to-powder mass ratio at 6:1, and carry out high-energy ball milling and mixing under an Ar protective atmosphere.

[0105] The high-energy ball milling conditions were: ball milling speed 450 rpm and ball milling time 18 h.

[0106] After ball milling, the resulting mixed powder was placed in an alumina crucible and calcined in a high-temperature furnace. The calcination conditions were: heating to 1320℃ at a rate of 5℃ / min, holding at that temperature for 10 hours, and then cooling to room temperature with the furnace. The calcined product was crushed, ground, and sieved to obtain high-entropy rare earth oxide powder A.

[0107] (II) Preparation of composite powder

[0108] Weigh 29.10g of HfH2 powder and mix it with 0.90g of the above-mentioned high-entropy rare earth oxide powder A to obtain a composite powder raw material.

[0109] The HfH2 powder has a purity of 99.0% and a D50 particle size of 16μm.

[0110] Based on the total mass of the composite powder, the content of HfH2 powder is 97.0 wt%, and the content of high entropy rare earth oxide powder A is 3.0 wt%.

[0111] HfH2 powder and high-entropy rare earth oxide powder A were added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 260 rpm, ball-to-powder mass ratio 4:1, and mixing time 5 h. After mixing, a homogeneous composite powder B was obtained.

[0112] (III) Pressing and Sintering

[0113] Composite powder B was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 300 MPa, holding time 25 min. After pressing, a circular green body was obtained.

[0114] The sintering process is as follows:

[0115] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.10 MPa, followed by the introduction of hydrogen and the adjustment of the furnace atmosphere pressure to 0.12 MPa.

[0116] In the first stage, the temperature is increased to 400℃ at a rate of 5℃ / min and held for 40min.

[0117] In the second stage, the temperature is increased to 800℃ at a rate of 5℃ / min and held for 80min.

[0118] In the third stage, hydrogen gas was continued to be introduced, and the atmosphere pressure inside the furnace was adjusted to 0.15 MPa. The temperature was then reduced to 350°C at a rate of 5°C / min and held for 1 hour.

[0119] In the fourth stage, the mixture is kept under the above-mentioned hydrogen-containing protective atmosphere and cooled to room temperature at 5°C / min to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0120] After sintering, a circular hafnium hydride-rare earth oxide composite neutron absorber sample S3 was obtained, with a diameter of 20 mm and a thickness of 4 mm.

[0121] Example 4

[0122] This embodiment provides a method for preparing a hafnium hydride-rare earth oxide composite neutron absorber material.

[0123] (I) Preparation of high-entropy rare earth oxide powders

[0124] Eu2O3, Sm2O3, Dy2O3, Gd2O3 and Ho2O3 were selected as rare earth oxide raw materials.

[0125] Among them, the purity of Eu2O3 powder is 99.9% and the D50 particle size is 0.35μm; the purity of Sm2O3 powder is 99.9% and the D50 particle size is 0.28μm; the purity of Dy2O3 powder is 99.9% and the D50 particle size is 0.42μm; the purity of Gd2O3 powder is 99.9% and the D50 particle size is 0.36μm; and the purity of Ho2O3 powder is 99.9% and the D50 particle size is 0.38μm.

[0126] The five rare earth oxides were mixed in an equimolar ratio, with each component having a molar fraction of 20 mol%, corresponding to a configuration entropy ΔSconf of 1.609R.

[0127] Based on a total feed amount of 1.80g, weigh out 0.31g of Eu2O3 powder, 0.30g of Sm2O3 powder, 0.40g of Dy2O3 powder, 0.39g of Gd2O3 powder, and 0.40g of Ho2O3 powder, and add them together into a zirconia ball mill jar. Use zirconia balls as the grinding medium, control the ball-to-powder mass ratio at 5:1, and carry out high-energy ball milling and mixing under an Ar protective atmosphere.

[0128] The high-energy ball milling conditions were: ball milling speed 400 rpm and ball milling time 14 h.

[0129] After ball milling, the resulting mixed powder was placed in an alumina crucible and calcined in a high-temperature furnace. The calcination conditions were: heating to 1280℃ at a rate of 5℃ / min, holding at that temperature for 9 hours, and then cooling to room temperature with the furnace. The calcined product was crushed, ground, and sieved to obtain high-entropy rare earth oxide powder A.

[0130] (II) Preparation of composite powder

[0131] Weigh 29.10g of HfH2 powder and mix it with 0.90g of the above-mentioned high-entropy rare earth oxide powder A to obtain a composite powder raw material.

[0132] The HfH2 powder has a purity of 99.0% and a D50 particle size of 16μm.

[0133] Based on the total mass of the composite powder raw materials, the content of HfH2 powder is 97.0 wt%, and the content of high entropy rare earth oxide powder A is 3.0 wt%.

[0134] HfH2 powder and high-entropy rare earth oxide powder A were added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 260 rpm, ball-to-powder mass ratio 4:1, and mixing time 5 h. After mixing, a homogeneous composite powder B was obtained.

[0135] (III) Pressing and Sintering

[0136] Composite powder B was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 250 MPa, holding time 20 min. After pressing, a circular green body was obtained.

[0137] The sintering process is as follows:

[0138] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.07 MPa, followed by hydrogen gas and the furnace atmosphere pressure is adjusted to 0.10 MPa. The total furnace atmosphere pressure and H2 volume fraction are kept constant throughout the sintering process.

[0139] In the first stage, the temperature is increased to 400℃ at a rate of 5℃ / min and held for 40min.

[0140] In the second stage, the temperature was increased to 800℃ at a rate of 5℃ / min and held for 3 hours.

[0141] In the third stage, while maintaining the above-mentioned hydrogen-containing protective atmosphere, the temperature is lowered to 300℃ at a rate of 5℃ / min and held for 1 hour.

[0142] In the fourth stage, the hydrogen-containing protective atmosphere is maintained and cooled to room temperature at 5°C / min to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0143] After sintering, a disc-shaped hafnium hydride-rare earth oxide composite neutron absorber sample S4 was obtained, with a diameter of 20 mm and a thickness of 4 mm.

[0144] Comparative Example 1

[0145] This comparative example provides a method for preparing pure hafnium hydride materials without high-entropy rare earth oxide functional phases.

[0146] (a) Raw material preparation

[0147] Weigh 30.00g of HfH2 powder as raw material.

[0148] The HfH2 powder has a purity of 99.0% and a D50 particle size of 18μm.

[0149] (ii) Powder processing

[0150] The HfH2 powder was added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 240 rpm, ball-to-powder mass ratio 3:1, and mixing time 4 h. After mixing, powdered raw material C1 was obtained.

[0151] (III) Pressing and Sintering

[0152] Powdered raw material C1 was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 250 MPa, holding time 20 min. After pressing, a circular green sheet was obtained.

[0153] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.08 MPa, followed by the introduction of hydrogen and the adjustment of the furnace atmosphere pressure to 0.10 MPa.

[0154] The subsequent sintering process is as follows:

[0155] In the first stage, the temperature is increased to 400℃ at a rate of 5℃ / min and held for 40min.

[0156] In the second stage, the temperature was increased to 800℃ at a rate of 5℃ / min and held for 3 hours.

[0157] In the third stage, hydrogen gas was continued to be introduced, and the atmosphere pressure inside the furnace was adjusted to 0.15 MPa. The temperature was then reduced to 250℃~350℃ at a rate of 5℃ / min and held for 1 hour.

[0158] In the fourth stage, the hydrogen-containing protective atmosphere is maintained and cooled to room temperature at 5°C / min to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0159] After sintering, a circular pure hafnium hydride material sample C1-1 was obtained, with a diameter of 20 mm and a thickness of 4 mm.

[0160] Comparative Example 2

[0161] This comparative example provides a method for preparing a hafnium hydride-rare earth oxide composite material using a common multi-component rare earth oxide mechanical mixture as the functional phase.

[0162] (I) Preparation of ordinary multi-component rare earth oxide mixed powder

[0163] Eu2O3, Sm2O3, Dy2O3, Gd2O3 and Er2O3 were selected as rare earth oxide raw materials.

[0164] Among them, the purity of Eu2O3 powder is 99.9% and the D50 particle size is 0.35μm; the purity of Sm2O3 powder is 99.9% and the D50 particle size is 0.28μm; the purity of Dy2O3 powder is 99.9% and the D50 particle size is 0.42μm; the purity of Gd2O3 powder is 99.9% and the D50 particle size is 0.36μm; and the purity of Er2O3 powder is 99.9% and the D50 particle size is 0.40μm.

[0165] The five rare earth oxides were mixed in an equimolar ratio, with each component having a molar fraction of 20 mol.

[0166] Based on a total feed amount of 2.50g, weigh out 0.44g of Eu2O3 powder, 0.42g of Sm2O3 powder, 0.56g of Dy2O3 powder, 0.54g of Gd2O3 powder, and 0.54g of Er2O3 powder, and add them together into a zirconia ball mill jar. Use zirconia balls as the grinding medium and perform low-energy mixing treatment under an Ar protective atmosphere.

[0167] The mixing conditions were: ball mill speed 180 rpm, ball-to-material mass ratio 2:1, and mixing time 2 h.

[0168] After mixing, a common multi-component rare earth oxide mixed powder A is obtained. The mixed powder A is only a mechanical mixture of various rare earth oxide particles, and has not undergone high-energy ball milling and high-temperature calcination to form a single-phase solid solution. Therefore, it does not belong to high-entropy rare earth oxide powder.

[0169] (II) Preparation of composite powder

[0170] Weigh 29.10g of HfH2 powder and mix it with 0.90g of the above-mentioned common multi-component rare earth oxide mixed powder A to obtain composite powder raw material.

[0171] The HfH2 powder has a purity of 99.0% and a D50 particle size of 16μm.

[0172] Based on the total mass of the composite powder, the content of HfH2 powder is 97.0 wt%, and the content of ordinary multi-component rare earth oxide mixed powder A is 3.0 wt%.

[0173] HfH2 powder and a mixed powder A of common multi-component rare earth oxides were added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 260 rpm, ball-to-powder mass ratio 4:1, and mixing time 5 h. After mixing, a homogeneous composite powder B was obtained.

[0174] (III) Pressing and Sintering

[0175] Composite powder B was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 250 MPa, holding time 20 min. After pressing, a circular green body was obtained.

[0176] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.08 MPa, followed by the introduction of hydrogen and the adjustment of the furnace atmosphere pressure to 0.10 MPa.

[0177] The subsequent sintering process is as follows:

[0178] In the first stage, the temperature is increased to 400℃ at a rate of 5℃ / min and held for 40min.

[0179] In the second stage, the temperature was increased to 800℃ at a rate of 5℃ / min and held for 3 hours.

[0180] In the third stage, hydrogen gas was continued to be introduced, and the atmosphere pressure inside the furnace was adjusted to 0.15 MPa. The temperature was then reduced to 350°C at a rate of 5°C / min and held for 1 hour.

[0181] In the fourth stage, the hydrogen-containing protective atmosphere is maintained and cooled to room temperature at 5°C / min to stabilize the phase composition of the obtained hafnium hydride matrix phase.

[0182] After sintering, a disc-shaped hafnium hydride-ordinary multi-component rare earth oxide composite material sample C2-1 was obtained, with a diameter of 20 mm and a thickness of 4 mm.

[0183] Comparative Example 3

[0184] This comparative example provides a method for preparing a hafnium hydride-high entropy rare earth oxide composite material using a hafnium hydride matrix phase dominated by a tetragonal phase.

[0185] (I) Preparation of high-entropy rare earth oxide powders

[0186] Eu2O3, Sm2O3, Dy2O3, Gd2O3 and Er2O3 were selected as rare earth oxide raw materials.

[0187] Among them, the purity of Eu2O3 powder is 99.9% and the D50 particle size is 0.35μm; the purity of Sm2O3 powder is 99.9% and the D50 particle size is 0.28μm; the purity of Dy2O3 powder is 99.9% and the D50 particle size is 0.42μm; the purity of Gd2O3 powder is 99.9% and the D50 particle size is 0.36μm; and the purity of Er2O3 powder is 99.9% and the D50 particle size is 0.40μm.

[0188] The five rare earth oxides were mixed in an equimolar ratio, with each component having a molar fraction of 20 mol%, corresponding to a configuration entropy ΔSconf of 1.609R.

[0189] Based on a total feed amount of 2.50g, weigh out 0.44g of Eu2O3 powder, 0.42g of Sm2O3 powder, 0.56g of Dy2O3 powder, 0.54g of Gd2O3 powder, and 0.54g of Er2O3 powder, and add them together into a zirconia ball mill jar. Use zirconia balls as the grinding medium, control the ball-to-powder mass ratio at 6:1, and carry out high-energy ball milling and mixing under an Ar protective atmosphere.

[0190] The high-energy ball milling conditions were: ball milling speed 420 rpm, ball milling time 16 h.

[0191] After ball milling, the resulting mixed powder was placed in an alumina crucible and calcined in a high-temperature furnace. The calcination conditions were: heating to 1300℃ at a rate of 5℃ / min, holding at that temperature for 10 hours, and then cooling to room temperature with the furnace. The calcined product was crushed, ground, and sieved to obtain high-entropy rare earth oxide powder A.

[0192] (II) Preparation of composite powder

[0193] Weigh 29.10g of HfH2 powder and mix it with 0.90g of the above-mentioned high-entropy rare earth oxide powder A to obtain a composite powder raw material.

[0194] The HfH2 powder has a purity of 99.0% and a D50 particle size of 16μm.

[0195] Based on the total mass of the composite powder, the content of HfH2 powder is 97.0 wt%, and the content of high entropy rare earth oxide powder A is 3.0 wt%.

[0196] HfH2 powder and high-entropy rare earth oxide powder A were added to a zirconia ball mill jar and mechanically mixed under an Ar protective atmosphere. The mechanical mixing conditions were: ball milling speed 260 rpm, ball-to-powder mass ratio 4:1, and mixing time 5 h. After mixing, a homogeneous composite powder B was obtained.

[0197] (III) Pressing and Sintering

[0198] Composite powder B was loaded into a flexible mold for cold isostatic pressing and formed. The cold isostatic pressing conditions were: pressing pressure 250 MPa, holding time 20 min. After pressing, a circular green body was obtained.

[0199] The green blank is placed in a sintering furnace, and after repeated vacuuming and argon purging 2 to 3 times, an Ar atmosphere is introduced to 0.05 MPa, followed by the introduction of hydrogen and the adjustment of the furnace atmosphere pressure to 0.20 MPa.

[0200] The subsequent sintering process is as follows:

[0201] In the first stage, the temperature is increased to 400℃ at a rate of 5℃ / min and held for 40min.

[0202] In the second stage, the temperature was increased to 800℃ at a rate of 5℃ / min and held for 3 hours.

[0203] In the third stage, hydrogen gas was continued to be introduced and the furnace atmosphere pressure was maintained at 0.50 MPa. The temperature was lowered to 300°C at 5°C / min and held for 2 hours to increase the hydrogen content in the material, so that the resulting hafnium hydride matrix phase was mainly tetragonal.

[0204] In the fourth stage, the hydrogen-containing protective atmosphere is maintained and the temperature is cooled to room temperature at a rate of 5°C / min.

[0205] After sintering, a circular hafnium hydride-high entropy rare earth oxide composite material sample C3-1 with a tetragonal phase as the main component was obtained. The sample diameter was 20 mm and the thickness was 4 mm.

[0206] Performance Testing and Result Analysis

[0207] The samples obtained in Examples 1-4 and Comparative Examples 1-3 were subjected to phase analysis, compressive strength, surface hardness and hydrogen desorption temperature tests. The test items and test conditions are shown in Table 1. The performance test results of Examples 1-4 and Comparative Examples 1-3 are shown in Table 2.

[0208] Table 1 Test Items and Test Conditions

[0209]

[0210] Table 2 Performance test results of Examples 1-4 and Comparative Examples 1-3

[0211]

[0212] Figure 2 The X-ray diffraction (XRD) patterns of the composite neutron absorbing material obtained in Example 1 and the samples of Comparative Examples 1-3 are shown. Figure 3 The images shown are scanning electron microscope (SEM) images and energy dispersive spectroscopy (EDS) analysis results of the composite neutron absorbing material obtained in Example 1. Figure 4 This is a thermal dehydrogenation temperature curve of the composite neutron absorber material obtained in Example 1. Figure 2 As can be seen, in the composite neutron absorber material obtained in Example 1, the diffraction peaks of the hafnium hydride matrix phase and the cubic phase HfH x Corresponding to the standard diffraction peaks, no tetragonal HfH was observed. x The characteristic diffraction peaks of other impurity phases indicate that the obtained hafnium hydride matrix phase is a cubic phase HfH. x For other impurity phases, such as the tetragonal phase, that are not detected by XRD, their content can be considered to be below the XRD detection limit under these test conditions. (Except for the cubic phase HfH) x In addition to the matrix phase diffraction peaks, a set of independent single-phase diffraction peaks also exists. No characteristic peaks of individual rare earth oxide phases were observed, indicating the formation of a single-phase solid solution high-entropy rare earth oxide functional phase. Comparative Example 1 sample contains only HfH. x Matrix phase diffraction peaks. In Comparative Example 2, multiple sets of independent characteristic peaks corresponding to the individual structures of each rare earth oxide were observed, indicating that its functional phase remains a multiphase mechanical mixture and has not formed a solid solution. HfH of Comparative Example 3 sample. xThe matrix phase diffraction peak positions differ significantly from those of Example 1, exhibiting a predominantly tetragonal phase characteristic, while the diffraction characteristics of its high-entropy rare-earth oxide functional phase are basically consistent with those of Example 1. Figure 3 As can be seen, the high-entropy rare earth oxide functional phase in the sample of Example 1 is uniformly and diffusely distributed in the matrix phase in the form of fine particles, without obvious agglomeration, and the interface bonding is tight, with no obvious pores or microcracks. Energy dispersive spectroscopy analysis shows that each rare earth element is uniformly distributed and highly overlapping in the measured area, without local enrichment, further verifying that this functional phase is a single-phase solid solution with atomic-scale homogeneous mixing. Figure 4 As can be seen, the mass of the sample in Example 1 decreased slowly with increasing temperature during the heating process. After reaching a certain temperature, the mass loss rate accelerated significantly, and the curve showed an inflection point, corresponding to the initial temperature of large-scale hydrogen release. Compared with Comparative Examples 1-3, the hydrogen release initiation temperature of Example 1 was significantly higher, indicating that the introduction of the single-phase solid solution high-entropy rare earth oxide functional phase and the structural regulation of the cubic hafnium hydride matrix phase are both beneficial to delaying hydrogen release and improving the hydrogen retention capacity and service stability of the material. This is consistent with the mechanism of lattice distortion hindering hydrogen diffusion and improving the compatibility of the matrix-functional phase interface.

[0213] As shown in Table 2, compared with Comparative Example 1, the microhardness, compressive strength, relative density, and hydrogen desorption stability of the composite neutron absorbing materials obtained in Examples 1-4 are significantly improved. This indicates that introducing high-entropy rare-earth oxide functional phases into the hafnium hydride matrix helps to improve the overall performance of the material. This is because the high-entropy rare-earth oxide functional phases can act as neutron absorption enhancement phases dispersed in the matrix. Furthermore, their multi-principal-unit disordered distribution and high configurational entropy are beneficial for improving microstructure stability and inhibiting hydrogen diffusion and migration within the material, thereby improving the material's strength, densification, and hydrogen retention stability.

[0214] Compared to Comparative Example 2, the high-entropy rare-earth oxide functional phases used in Examples 1-4 were single-phase solid solutions formed by the random occupancy of no fewer than five rare-earth cations, while the functional phase in Comparative Example 2 was merely a mechanical mixture of various rare-earth oxide particles, without forming a single-phase solid solution structure. Therefore, the functional phases in Examples 1-4 were more uniformly distributed in the matrix, resulting in a more stable interface state. Furthermore, the lattice distortion and localized stress field fluctuations caused by the high-entropy structure were beneficial in suppressing hydrogen migration and high-temperature hydrogen loss, leading to materials that outperformed Comparative Example 2 in terms of strength, relative density, and the initial temperature of large-scale hydrogen release.

[0215] Compared with Comparative Example 3, the hafnium hydride matrix phase used in Example 1 is a cubic phase HfH. xIn Comparative Example 3, the hafnium hydride matrix phase is predominantly tetragonal, indicating that the crystal structure of the hafnium hydride matrix phase can be effectively controlled by adjusting the sintering and hydrogen retention process parameters. Although both examples use high-entropy rare earth oxides as functional phases, the cubic hafnium hydride matrix in Example 1 exhibits better structural coordination and interfacial compatibility with the high-entropy rare earth oxide functional phase. This is more conducive to improving the interfacial bonding state and stress transfer mode, reducing the risk of local stress concentration and microcrack initiation and propagation during sintering, cooling, and subsequent thermal cycling. Therefore, Example 1 is superior to Comparative Example 3 in terms of microhardness, compressive strength, relative density, and large-scale hydrogen release initiation temperature, indicating that controlling the hafnium hydride matrix phase to be predominantly cubic is more conducive to achieving a synergistic improvement in the mechanical properties and hydrogen retention stability of the composite neutron absorber material.

[0216] Furthermore, the test results from Examples 1 to 4 also show that, within the composition and process range defined by this invention, different combinations of high-entropy rare earth oxide components can yield high-performance hafnium hydride-rare earth oxide composite neutron absorbers, indicating that the scheme of this invention has good compositional adaptability and process feasibility.

[0217] In summary, this invention introduces a high-entropy rare-earth oxide functional phase into the hafnium hydride matrix and modulates the hafnium hydride matrix phase into a cubic phase structure, thereby achieving a synergistic improvement in the neutron absorption performance, mechanical properties, structural stability, and hydrogen retention performance of the material.

[0218] The above embodiments are only used to further illustrate the hafnium hydride-rare earth oxide composite neutron absorber material and its preparation method according to the present invention. However, the present invention is not limited to the embodiments. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a hafnium hydride-rare earth oxide composite neutron absorber material, characterized in that, Includes the following steps: Step 1: Mix at least five rare earth oxides to obtain a mixed powder, then ball-mill and calcine the mixed powder to obtain high-entropy rare earth oxide powder; the calcination temperature is 1200℃~1500℃, and the holding time is 8h~15h; the rare earth oxides are selected from at least five of Eu2O3, Sm2O3, Dy2O3, Gd2O3, Er2O3, Y2O3, Yb2O3, and Ho2O3; Step 2: The high-entropy rare earth oxide powder and hafnium hydride powder are mechanically mixed under a protective atmosphere to obtain a composite powder; the mass ratio of the high-entropy rare earth oxide powder to the hafnium hydride powder is (100-a):a, where 95.0 ≤ a ≤ 99.0; Step 3: The composite powder is pressed into shape and then sintered under a hydrogen-containing protective atmosphere to obtain a hafnium hydride-rare earth oxide composite neutron absorber material; the hydrogen-containing protective atmosphere is a mixture of H2 and inert gas, wherein the volume fraction of H2 is 15% to 60%.

2. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 1, characterized in that: The molar fraction of any of the rare earth oxides in the mixed powder is not less than 10% and not more than 35%.

3. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 1, characterized in that: The high-entropy rare earth oxide includes at least one thermal neutron high absorption cross-section element and at least one resonance region / fast neutron absorption contributing element. The thermal neutron high absorption cross-section element includes Eu, Sm and Gd; the resonance region / fast neutron absorption contributing element includes Dy, Er and Ho.

4. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 1, characterized in that: The hafnium hydride powder is HfH2; the D50 particle size of the hafnium hydride powder is 1μm to 100μm.

5. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 1, characterized in that: The high-entropy rare earth oxide powder is a single-phase solid solution powder with a configuration entropy ΔS. conf ≥1.5R, where R is the ideal gas constant.

6. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 1, characterized in that: In step 2, the mechanical mixing is carried out by ball milling, with a mixing time of 1h to 10h, a ball milling speed of 100rpm to 300rpm, and a ball-to-material mass ratio of 1:1 to 10:

1.

7. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 1, characterized in that, In step 3, the sintering is pressureless sintering with an internal furnace pressure not exceeding 0.2 MPa, and includes the following stages: The first stage involves maintaining the temperature at 250℃~450℃ for 0.2h~2h. The second stage involves maintaining the temperature at 700℃~900℃ for 2h~4h. The third stage involves maintaining the temperature at 250℃~350℃ for 0.5h~5h. The fourth stage involves cooling to room temperature.

8. The preparation method of the hafnium hydride-rare earth oxide composite neutron absorber material according to claim 7, characterized in that: The volume fraction of H2 in the hydrogen-containing protective atmosphere of the third and fourth stages is greater than that in the first and second stages.

9. A hafnium hydride-rare earth oxide composite neutron absorber material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: It includes a hafnium hydride matrix phase and a high-entropy rare earth oxide functional phase dispersed in the matrix phase.

10. The hafnium hydride-rare earth oxide composite neutron absorber material according to claim 9, characterized in that: The hafnium hydride matrix phase is a cubic phase HfH. x , where x is 1.50 to 1.80; the high-entropy rare earth oxide functional phase is a cubic solid solution in which no less than five rare earth cations are randomly occupied on the cation sublattice.

Citation Information

Patent Citations

  • Boron carbide-based composite ceramic material and preparation method thereof

    CN111848170A

  • Hafnium hydride neutron absorbing material and preparation method thereof

    CN116750718A