A method for preparing a biomimetic organic-inorganic hybrid flame-retardant coating based on a silicon-oxygen crosslinking network
By introducing a phosphorus-containing silicon flame-retardant precursor into a silicon-oxygen crosslinking network, a biomimetic organic-inorganic hybrid flame-retardant coating is constructed, which solves the problems of easy migration of flame-retardant components and insufficient interfacial adhesion. This results in a coating with high adhesion, transparency, flame-retardant performance, and recyclability, suitable for flame-retardant protection of various substrates.
Patent Information
- Application Number
- CN202611275625.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-08-21
AI Technical Summary
Existing flame-retardant coatings have problems such as easy migration or precipitation of flame-retardant components, insufficient interfacial adhesion, poor transparency, difficulty in achieving both flame-retardant and mechanical properties, and difficulty in recycling.
Using a molecular engineering strategy, the phosphorus-containing silicon flame retardant precursor DPOP-Si was covalently introduced into the silicon-oxygen crosslinking network constructed by DOPA and silane coupling agent, forming a flame retardant coating with a biomimetic adhesive structure and an organic-inorganic hybrid structure. The silicon-oxygen crosslinking network was constructed through Michael addition reaction and silane hydrolysis-condensation reaction, and DPOP-Si participated in the formation of the covalent network structure.
It achieves improved stability and utilization efficiency of flame-retardant components, strong adhesion and good interfacial bonding between the coating and the substrate, and combines transparency, flame retardancy and mechanical properties, while also possessing chemical recycling and reprocessing capabilities.
Smart Images

Figure CN122810706B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional polymer materials and flame-retardant coating technology, specifically relating to a method for preparing a biomimetic organic-inorganic hybrid flame-retardant coating based on a silicon-oxygen crosslinking network. Background Technology
[0002] With the rapid development of fields such as construction, transportation, electronics, and aerospace, polymer materials such as polyurethane foam, wood, and plastics have been widely used due to their light weight, good processing performance, and low cost. However, these materials generally suffer from flammability, rapid combustion rates, and the release of large amounts of heat and smoke during combustion, posing significant fire safety hazards. Therefore, developing efficient, durable, and versatile flame-retardant protection technologies applicable to various substrates has become an important research direction in the field of polymer materials.
[0003] Currently, surface flame-retardant coatings have attracted widespread attention due to their advantages such as simple preparation process, wide applicability to substrates, and ability to improve the flame-retardant performance of materials without altering the main properties of the substrate. Existing flame-retardant coatings mainly employ methods such as physical blending of flame retardants or surface impregnation to construct flame-retardant systems. While these methods can improve the flame-retardant performance of materials to some extent, they generally suffer from problems such as easy migration or precipitation of flame-retardant components, insufficient interfacial bonding with the polymer matrix, and poor long-term stability. Furthermore, traditional flame-retardant coatings typically struggle to simultaneously achieve multiple properties, including flame retardancy, mechanical properties, transparency, and sustainable recyclability, limiting their application in high-end protective applications.
[0004] In recent years, biomimetic adhesion strategies and organic-inorganic hybrid networks have attracted attention due to their ability to improve the interfacial bonding between coatings and substrates and enhance the overall material properties. However, existing technologies primarily employ physical composite methods to introduce flame-retardant components, making it difficult to achieve the integrated construction of flame-retardant units and cross-linked networks. Therefore, there is still room for further improvement in flame-retardant efficiency and durability. Furthermore, how to achieve synergistic optimization of flame-retardant performance, mechanical properties, and material recyclability while ensuring high adhesion and transparency remains a pressing technical challenge in this field.
[0005] Therefore, it is necessary to develop a biomimetic organic-inorganic hybrid flame-retardant coating and its preparation method that has a reasonable structural design, simple preparation process, can achieve the synergistic construction of flame-retardant units and silicon-oxygen cross-linked networks, and has high adhesion, flame-retardant performance, transparency and sustainable recycling performance. Summary of the Invention
[0006] This invention addresses the problems of existing flame-retardant coatings, such as easy migration or precipitation of flame-retardant components, insufficient interfacial adhesion, poor transparency, difficulty in achieving both flame-retardant and mechanical properties, and difficulty in recycling. It provides a method for preparing a biomimetic organic-inorganic hybrid flame-retardant coating based on a silicon-oxygen crosslinking network. This invention employs a molecular engineering strategy to covalently introduce the phosphorus-containing silicon flame-retardant precursor DPOP-Si into a silicon-oxygen crosslinking network constructed from DOPA and a silane coupling agent, forming a flame-retardant coating with a biomimetic adhesive structure and an organic-inorganic hybrid structure. The resulting coating can stably adhere to the surfaces of various substrates such as polyurethane foam, wood, metal, glass, and plastics, and possesses transparency, good interfacial adhesion, flame-retardant properties, and chemical recycling and reprocessing capabilities. It can be widely used in building fire protection, electronics, transportation, and aerospace fields.
[0007] The present invention discloses a method for preparing a biomimetic organic-inorganic hybrid flame-retardant coating based on a silicon-oxygen crosslinking network, comprising the following steps:
[0008] Step 1: Dissolve pentaerythritol tetraacrylate (PETEA) in DMF, add dopamine hydrochloride (DOPA), and stir the reaction at a certain temperature to allow the amino group in DOPA to undergo a Michael addition reaction with the double bond in PETEA, thus obtaining a prepolymer system.
[0009] Step 2: Add KH550 to the prepolymer system obtained in Step 1 and continue stirring to allow the silane to undergo hydrolysis and polycondensation, forming a silicon-oxygen crosslinking network with the system to obtain the PDH precursor solution.
[0010] Step 3: Add the phosphorus-containing silicon flame retardant precursor DPOP-Si to the reaction system obtained in Step 2, and continue stirring the reaction to allow DPOP-Si to participate in the formation of the silicon-oxygen crosslinking network and be uniformly introduced into the network structure through covalent interaction, thus obtaining the biomimetic organic-inorganic hybrid flame retardant precursor liquid, namely PDH-FR flame retardant precursor liquid.
[0011] Step 4: Apply the PDH-FR flame retardant precursor liquid obtained in Step 3 evenly to the substrate surface by brushing, spraying, dipping or scraping, and after curing, form a biomimetic organic-inorganic hybrid flame retardant coating based on a silicon-oxygen crosslinking network.
[0012] In step 1, the molar ratio of the double bond in PETEA to the amino group in DOPA is 1:1 to 1:1.5.
[0013] In step 1, the reaction temperature is 60-80℃ and the reaction time is 1-3 h.
[0014] In step 2, the molar ratio of KH550 to DOPA is 1:3 to 1:8.
[0015] In step 2, the hydrolysis-condensation reaction is carried out at a temperature of 60-80℃ for 1-4 hours.
[0016] In step 3, the structural formula of the phosphorus-containing silicon flame retardant precursor DPOP-Si is as follows:
[0017] .
[0018] In step 3, the amount of DPOP-Si added is 5%-40% of the mass of the silicon-oxygen crosslinking network. Here, the mass of the silicon-oxygen crosslinking network is based on the reaction system obtained in step 2.
[0019] In step 3, the reaction temperature is 60-80℃ and the reaction time is 1-4 h.
[0020] In step 4, the curing temperature is 25-80℃.
[0021] In step 4, the substrate includes one or more of polyurethane foam, wood, glass, metal, paper, fabric, and plastic.
[0022] In step 4, the thickness of the coating is 100-1000 μm.
[0023] The biomimetic organic-inorganic hybrid flame-retardant coating based on the silicon-oxygen cross-linking network of this invention can be applied to the surface of materials such as polymer foam, wood, metal, glass and plastic, and can also be applied to the surface of building materials, electronic appliances, transportation and aerospace materials to play a role in flame retardant protection.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention adopts a molecular engineering strategy to covalently introduce phosphorus-containing silicon flame retardant precursors into the silicon-oxygen crosslinking network, avoiding the problems of easy migration, easy precipitation and insufficient durability of traditional additive flame retardants, and improving the stability and utilization efficiency of flame retardant components in the coating.
[0026] (2) The present invention utilizes the synergistic effect of the catechol biomimetic adhesive structure and the silicon-oxygen crosslinking network to enable the obtained coating to adhere firmly to the surface of various substrates such as polyurethane foam, wood, metal, glass and plastic, and has good interfacial bonding ability and mechanical stability.
[0027] (3) The present invention constructs an organic-inorganic hybrid network structure with synergistic effect of phosphorus and silicon, which has transparency, flame retardant properties and mechanical properties, effectively improving the flame retardant protection capability of the substrate and maintaining the original appearance of the material.
[0028] (4) The coating obtained by the present invention has chemical recycling and reprocessing capabilities, and can realize the recycling of materials through chemical treatment, reduce resource waste, and meet the development needs of green manufacturing and sustainable development.
[0029] (5) The preparation process of this invention is simple and the reaction conditions are mild. It can be applied by brushing, spraying, dipping and other methods. It is suitable for flame retardant protection of substrates of different shapes and sizes and has good prospects for industrial application. Attached Figure Description
[0030] Figure 1 This is a schematic diagram illustrating the synthesis, construction, and application of the biomimetic organic-inorganic hybrid flame-retardant coating of this invention. Specifically: (A) PDH basic network construction reaction route: Dopamine hydrochloride, PETEA, and KH550 are reacted in DMF solvent at 70°C via Michael addition followed by silane hydrolysis and condensation to generate a PDH precursor network; (B) DPOP-Si precursor synthesis route: DPOP and VTES undergo a phosphine addition reaction at 80°C for 18 hours under chloroform and nitrogen protection to prepare DPOP-Si; (C) PDH-FR flame-retardant hybrid network covalent construction route: PDH precursor and DPOP-Si are co-hydrolyzed and condensed in water at 70°C, with phosphorus-containing silicon flame-retardant units covalently integrated into a silicon-oxygen crosslinking network to obtain the PDH-FR hybrid system; (D) Schematic diagram of PDH-FR coating application on multiple substrates, including polyurethane foam, wood, glass, steel, and plastics; (E) The transparency of the PDH-FR coating and the schematic diagram of the microstructure of the PDH-FR organic-inorganic hybrid cross-linking network are shown, with the cross-linking network constructed based on the biomimetic idea of mussel adhesion.
[0031] Figure 2 The Fourier transform infrared (FTIR) spectra and transparent optical properties characterization results of coating raw materials, intermediates, and finished products are shown. (A) shows the FTIR spectra of PETEA, DOPA, KH550, and PDH, with the characteristic peak assignment range marked as 3500-3200 cm⁻¹. -1 (OH / NH), 1635 cm -1 (C=C double bond), 1500 cm -1 (Aryl ring), 1200 cm -1 (COC, Si-O-Si) verifies the occurrence of Michael addition and silicon-oxygen condensation reaction; (B) is the FTIR spectrum of DPOP and DPOP-Si, with the characteristic peak marked at 2375 cm⁻¹. -1 (pH bond, disappears after reaction), 1620 cm -1(Vinyl C=C) proves that the hydrophosphine addition of DPOP and VTES is complete; (C) is the FTIR spectrum of PDH, DPOP-Si and PDH-FR, which simultaneously contains the characteristic absorption peaks of the PDH silicon-oxygen network and the phosphorus-containing silicon of DPOP-Si, proving that the flame retardant unit is covalently integrated into the crosslinking network; (D) is a transparency diagram of the PDH coating, which intuitively shows the advantages of the coating in high light transmittance and not obscuring the texture of the substrate.
[0032] Figure 3 The images show the microstructure and elemental composition analysis results of the flame-retardant coating of this invention. Among them, (A) is a scanning electron microscope (SEM) image of the PDH-FR coating and an elemental distribution diagram of C, O, N, Si, and P in EDS; (B) is a SEM image of the PDH-FR coating applied to a cross-section of wood; and (C) is a SEM image of the cross-section of the PDH coating polyurethane foam.
[0033] Figure 4 This document presents the flame-retardant performance and char residue analysis results of the flame-retardant coating applied to polyurethane (PU) foam according to the present invention. PU refers to polyurethane foam without the flame-retardant coating; PU-PDH refers to polyurethane foam with a PDH coating; and PU-PDH-FR refers to polyurethane foam with a PDH-FR flame-retardant coating. Among them, (A) is the heat release rate change curve during the cone calorimetry test, with the ignition time (TTI) marked: PU=11 s, PU-PDH=32 s, PU-PDH-FR=40 s. PDH-FR significantly prolongs the ignition time and reduces the peak heat release. (B) is the smoke release rate change curve during the cone calorimetry test. The flame retardant coating significantly inhibits smoke generation. (C) is the total smoke release change curve during the combustion process of different samples. PDH-FR promotes char formation and reduces the thermal decomposition of the substrate. (D) is the SEM image and EDS elemental analysis results of the residual char layer after combustion. The microscopic SEM morphology of the residual char, the EDS surface distribution and mass ratio of C / O / Si / N / P elements in the residual char are as follows: pure PU residual char is loose and porous; PU-PDH residual char has no dense barrier layer; PU-PDH-FR forms a continuous dense expanded char layer. The surface of the char layer is rich in Si and P flame retardant elements, which construct a heat insulation and oxygen barrier.
[0034] Figure 5 The results show the flame retardant performance test results of the flame retardant coating of the present invention. Among them, (A) shows the limiting oxygen index (LOI) test results of different samples, which quantitatively reflects the improvement of the critical oxygen concentration for flame retardancy of PDH-FR; (B) shows the vertical burning test results, which verify the excellent self-extinguishing and non-dripping flame retardant characteristics of PDH-FR.
[0035] Figure 6The figures show the tensile and interfacial lap shear strength test results of PDH and PDH-FR coatings. Specifically: (A) Tensile stress-strain curves of PDH and PDH-FR coatings, comparing the tensile toughness and fracture strength of the two coatings; (B) A bar chart of the lap shear strength of the PDH-FR coating on seven substrates: wood, steel, polystyrene (PS), polyurethane (PU), polyester resin (PET), polyethylene (PE), and glass, demonstrating that the coating exhibits high interfacial adhesion to metal, polymer, inorganic, and wood substrates.
[0036] Figure 7 The images show the results of the high-temperature burn test and the microcaloric combustion (MCC) heat release test. In the image, (A) shows the morphology of the sample after the burn test. The coating thickness is about 400 μm. At high temperature, a char layer is quickly formed to block the flame, and there is no large-area burn-through of the substrate. (B) shows the results of the microcaloric combustion (MCC) test. The phosphorus-silicon hybrid coating significantly reduces the peak value of the combustion heat release.
[0037] Figure 8 This document presents a complete set of physical characterization images for the long-term solvent resistance stability and chemical recycling of the coating. Specifically: (A) Comparative images of the coating after 10 days of immersion in multiple solvents at room temperature, visually demonstrating that the coating exhibits no swelling, dissolution, or discoloration in most organic solvents and alkaline aqueous solutions; (B) A flowchart of the PDH-FR chemical closed-loop recycling process: coating breakage → solvent dissolution and high-temperature depolymerization → regeneration of precursor solution → film reforming; (C) Accompanying photographs and corresponding FTIR spectra of samples from three cycles, verifying the stability of the coating structure and optical properties after multiple cycles. Detailed Implementation
[0038] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments. Without departing from the concept of the present invention, those skilled in the art can make appropriate adjustments to the types of raw materials, proportions, reaction conditions, and construction methods, all of which fall within the scope of protection of the present invention.
[0039] Raw materials and reagents:
[0040] The main raw materials and reagents used in the embodiments of this invention are as follows:
[0041] Pentaerythritol tetraacrylate (PETEA): analytical grade, purity ≥95%, purchased from Aladdin Reagent Co., Ltd.
[0042] Dopamine hydrochloride (DOPA): analytical grade, purity ≥99%, purchased from Aladdin Reagent Co., Ltd.
[0043] γ-aminopropyltriethoxysilane (KH550): analytical grade, purity ≥98%, purchased from Aladdin Reagent Co., Ltd.
[0044] Phosphorus-containing siloxane flame-retardant precursor (DPOP-Si): Prepared in-house, its synthesis method is as follows: In a 1000 mL three-necked reaction flask equipped with a mechanical stirrer, add 0.50 mol of DPOP (diphenylphosphine oxide) solid powder and 0.525 mol of VTES (vinyltriethoxysilane) liquid sequentially, followed by 20 mL of chloroform. Continuously purge the flask with high-purity nitrogen to replace the air inside, maintaining a nitrogen inert protective atmosphere throughout the reaction. Start mechanical stirring until DPOP and VTES are completely dissolved and the system is a homogeneous, transparent solution. Heat to 80℃ and maintain this temperature with continuous stirring for 18 h. The PH active bond in the DPOP structure undergoes a hydrophosphine addition reaction with the vinyl group of VTES, generating the DPOP-Si product in situ.
[0045] N,N-Dimethylformamide (DMF): Analytical grade, purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0046] Triethylamine (TEA): analytical grade, purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0047] Dichloromethane (DCM): analytical grade, purchased from Sinopharm Chemical Reagent Co., Ltd.
[0048] Test instruments and methods:
[0049] Fourier transform infrared spectroscopy (FTIR): A Nicolet 6700 Fourier transform infrared spectrometer was used, with a scanning range of 4000-400 cm⁻¹. -1 4 cm resolution -1 The number of scans was 32. The sample was prepared using the KBr pelleting method.
[0050] Scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS): The microstructure of the samples was observed using a SU8220 Hitachi, Japan type field emission scanning electron microscope with an accelerating voltage of 5 kV; the elemental distribution analysis was performed using a matching X-ray energy dispersive spectroscopy (EDS) instrument with an accelerating voltage of 15 kV.
[0051] Limiting Oxygen Index (LOI): Tested using an HC-2 oxygen index analyzer manufactured by Jiangning Analytical Instrument Factory, in accordance with ASTM D2863-97. The sample size was 130 mm × 6.5 mm × 3 mm.
[0052] Vertical burning test (UL-94): The CZF-2 horizontal and vertical burning tester manufactured by Jiangning Analytical Instrument Factory was used to test according to the standard ASTM D3801. The sample size was 130 mm × 13 mm × 3 mm.
[0053] Cone Calorimetry (CONE): The TTech-GBT16172 cone calorimeter from Taistek (Suzhou) Testing Instruments Technology Co., Ltd. was used for testing according to ISO 5660 standard. The thermal radiation power was 35 kW / m², and the sample size was 100 mm × 100 mm × 20 mm.
[0054] Micro combustion calorimetry (MCC): A Govmark MCC-2 micro combustion calorimeter was used, with a heating rate of 1℃ / s, a temperature range of 100-700℃, and a sample mass of approximately 5 mg.
[0055] Tensile property testing: The HZ-1004 universal testing machine of Dongguan Lixian Instrument Technology Co., Ltd. was used to test according to the standard GB / T 1040.3-2006. The tensile rate was 10 mm / min. The sample was dumbbell-shaped. Each sample was tested 5 times and the average value was taken.
[0056] Overlap shear strength test: The HZ-1004 universal testing machine was used to test according to the standard GB / T 7124-2008. The overlap area was 12.5 mm × 25 mm, the tensile rate was 5 mm / min, and each sample was tested 5 times and the average value was taken.
[0057] Solvent resistance test: The coating samples were immersed in solvent and left at room temperature for 10 days. The changes in the appearance of the coating were observed and the mass retention rate was tested.
[0058] Burning test with a propane torch: The sample surface was directly burned with a propane torch flame at a temperature of approximately 1100℃ for 60 seconds. The temperature change on the back of the sample and the morphology after burning were recorded.
[0059] Example 1:
[0060] The preparation method of the biomimetic organic-inorganic hybrid flame-retardant coating based on the silicon-oxygen crosslinking network in this embodiment is as follows:
[0061] (1) Preparation of PDH precursor
[0062] PETEA was dissolved in DMF and stirred at room temperature until completely dissolved. DOPA·HCl was then added, and the mixture was reacted at 70°C for 2 h, allowing a Michael addition reaction to occur between the primary amine in DOPA and the acrylate double bonds in PETEA. After the reaction was complete, KH550 was added to the system, and the reaction was continued at 70°C for another 2 h, causing KH550 to undergo hydrolysis and polycondensation, further constructing a silica crosslinking network to obtain the PDH precursor solution.
[0063] In this embodiment, the molar ratio of the double bonds in PETEA to the total amount of amino groups in DOPA and KH550 is 1:1.11, and the molar ratio of DOPA to KH550 is 5:1. In this embodiment, the amount of PETEA added is 0.02 mol, and DOPA and KH550 are added according to the above molar ratio. PETEA, DOPA, and KH550 are weighed according to the above molar ratio and reacted to prepare the PDH coating.
[0064] (2) Preparation of phosphorus-containing silicon flame retardant precursor DPOP-Si
[0065] The specific synthesis steps are as follows: Take a 1000 mL three-necked reaction flask equipped with a mechanical stirrer, and add 0.50 mol of DPOP (diphenylphosphine oxide) solid powder and 0.525 mol of VTES (vinyltriethoxysilane) liquid sequentially. Add 20 mL of chloroform, and continuously purge the air inside the flask with high-purity nitrogen to replace it, maintaining a nitrogen inert protective atmosphere throughout the reaction. Start mechanical stirring until DPOP and VTES are completely dissolved and the system is a homogeneous and transparent solution; raise the temperature to 80℃ and maintain the temperature with continuous stirring for 18 h. The PH active bond in the DPOP structure undergoes a hydrophosphine addition reaction with the vinyl group of VTES, generating the DPOP-Si product in situ.
[0066] (3) Preparation of PDH-FR flame retardant precursor liquid
[0067] The PDH precursor solution obtained in step (1) was cooled to room temperature, and the phosphorus-containing silicon flame retardant precursor DPOP-Si was added. The reaction was continued for 2 h with stirring, so that DPOP-Si participated in the formation of the silicon-oxygen crosslinking network and was integrated into the network structure through covalent bonds, thus obtaining the PDH-FR flame retardant precursor solution.
[0068] The amount of the phosphorus-containing siloxane flame retardant precursor added accounts for 20% of the total mass of the crosslinked network.
[0069] (4) Preparation of flame-retardant coating
[0070] The obtained PDH-FR flame retardant precursor liquid was uniformly applied to the surface of wood, polyurethane foam, glass and metal substrates. The coating was applied by scraping with a film scraper, and the coating thickness was controlled to be about 600 μm. Then, it was cured at room temperature for 24 h to obtain a uniform and continuous biomimetic organic-inorganic hybrid flame retardant coating based on a silicon-oxygen crosslinking network.
[0071] The substrates include, but are not limited to, polyurethane foam, wood, metal, glass, plastic, paper, and fabric.
[0072] like Figure 1 As shown, this invention utilizes Michael addition reaction and silane hydrolysis-condensation reaction to construct a silicon-oxygen crosslinking network with a catechol biomimetic adhesion structure, and further covalently integrates phosphorus-containing siloxane flame retardant units into the network to form an organic-inorganic hybrid flame retardant coating.
[0073] Example 2:
[0074] The structures of the obtained PDH and PDH-FR coatings were characterized by Fourier transform infrared spectroscopy, and the results are as follows: Figure 2 As shown.
[0075] Figure 2 Figure A shows that the double bond-related absorption peak of acrylate in PETEA is significantly weakened, while the Si-O-Si related characteristic absorption appears in PDH, indicating that aza-Michael addition and silane hydrolysis-condensation reaction occur.
[0076] Figure 2 Figure B shows that the characteristic PH absorption peak in DPOP is significantly weakened or disappears after the reaction, indicating that DPOP undergoes an addition reaction with VTES to form DPOP-Si.
[0077] Figure 2 The middle C figure further shows that PDH-FR retains the characteristic structure of the PDH network and exhibits characteristic absorption peaks related to phosphorus-containing siloxanes, indicating that DPOP-Si was successfully introduced into the PDH hybrid network.
[0078] Figure 2 The transparency photograph shown in Figure D indicates that the obtained PDH coating has high transparency and can maintain the visibility of the original color, texture and pattern of the substrate.
[0079] Example 3:
[0080] The microstructure of the PDH-FR coating was observed using scanning electron microscopy (SEM), and the elemental distribution was analyzed using energy dispersive spectroscopy (EDS). The results are as follows: Figure 3 As shown.
[0081] Figure 3Figure A shows that PDH-FR forms a continuous and uniform coating layer on the surface of the polyurethane foam skeleton.
[0082] EDS results showed that C, N, O, Si and P elements were uniformly distributed throughout the entire skeleton surface, indicating that the phosphorus-containing siloxane flame retardant component was uniformly integrated into the entire silicon-oxygen crosslinking network.
[0083] Figure 3 Image B shows a cross-sectional SEM image of PDH-FR coated wood and the elemental distribution of Si. Figure 3 The middle image (C) shows a cross-sectional SEM image of PDH-coated polyurethane foam. It can be seen that PDH and PDH-FR can completely encapsulate the polyurethane foam skeleton without blocking the cell structure.
[0084] Example 4:
[0085] PDH-FR was coated onto the surface of polyurethane foam, and its combustion behavior was evaluated using cone calorimetry. Figure 4 As shown, compared with untreated polyurethane foam, the PDH-FR coating can reduce heat and smoke release during combustion. Further observation of the SEM morphology of the residual char layer after combustion and EDS analysis of the elemental composition of the char residue were performed. A continuous and dense charred protective layer was formed after combustion, while Si and P elements were retained in the char residue, indicating that the phosphorus-silicon components participated in the formation of the condensed phase protective layer.
[0086] Example 5:
[0087] The flame retardant performance of PDH-FR was evaluated using limiting oxygen index and vertical burning tests.
[0088] like Figure 5 As shown in Figure A, PDH-FR has a high limiting oxygen index; Figure 5 Figure B shows that the UL-94 test further demonstrates that PDH-FR has good flame retardant properties. Subsequently, PDH-FR was immersed in different solvents, and the changes in the coating appearance and structure were observed to evaluate its solvent resistance. PDH-FR was further treated in a chemical recycling system to dissociate the dynamic network, and the resulting recycled system reformed the film, evaluating the chemical recycling and reprocessing performance of the material (Example 8).
[0089] Example 6:
[0090] The tensile properties of PDH and PDH-FR self-supporting films were tested using a universal testing machine. The interfacial adhesion performance of PDH-FR to different substrates was evaluated using an lap shear test. Tensile tests were conducted according to GB / T 1040.3-2006, with a tensile rate of 10 mm / min. Each sample group was tested five times, and the average value was taken. Lap shear tests were conducted according to GB / T 7124-2008, with an overlap area of 12.5 mm × 25 mm and a tensile rate of 5 mm / min. Each sample group was tested five times, and the average value was taken.
[0091] like Figure 6 As shown, PDH-FR has good mechanical properties and can form strong interfacial bonds with wood, steel, glass and a variety of polymer substrates, demonstrating good universal adhesion ability.
[0092] Example 7:
[0093] Further high-temperature flame burning tests were conducted on the PDH-FR coating, with a coating thickness of approximately 400 μm.
[0094] The sample surface was continuously burned with a blowtorch, and the morphology of the sample during the combustion process and the surface state after combustion were observed. Figure 7 As shown in Figure A, PDH-FR can rapidly form a carbonized protective layer upon heating, providing thermal protection to the substrate. Simultaneously, MCC testing was used to further evaluate the combustion exothermic characteristics of PDH-FR, such as... Figure 7 As shown in Figure B, PDH-FR exhibits a lower peak value for combustion exothermics.
[0095] Example 8:
[0096] The PDH-FR coating was placed in different organic solvents and alkaline aqueous solutions and immersed at room temperature for 10 days. The appearance, integrity and color changes of the coating before and after immersion were observed.
[0097] like Figure 8 As shown in Figure A, after long-term immersion, the PDH-FR coating still maintains good structural integrity, and no obvious swelling, peeling or dissolution is observed.
[0098] The PDH-FR was then chemically recovered. The coating was crushed and placed in a recycled solvent, where the dynamic network was dissociated under heating conditions to obtain a reprocessable precursor system; subsequently, a reprocessable coating was obtained through re-film formation. Figure 8 As shown in Figure B, PDH-FR can achieve closed-loop recycling through a process of "coating breakage—solvent dissolution / high-temperature depolymerization—precursor regeneration—re-film formation," and can be recycled multiple times. The FTIR spectra before and after cycling remain basically consistent, indicating that the material has good chemical recyclability and cycling stability. Figure 8(C) Figure.
Claims
1. A method for preparing a biomimetic organic-inorganic hybrid flame-retardant coating based on a silicon-oxygen crosslinking network, characterized in that... Includes the following steps: Step 1: Dissolve pentaerythritol tetraacrylate in a solvent, add dopamine hydrochloride, stir and react to allow the amino group in dopamine hydrochloride to undergo a Michael addition reaction with the double bond in pentaerythritol tetraacrylate, thus obtaining the prepolymer system. Step 2: Add KH550 to the prepolymer system obtained in Step 1 and continue stirring to allow the silane to undergo hydrolysis and polycondensation, forming a silicon-oxygen crosslinking network with the system to obtain the PDH precursor solution. Step 3: Add the phosphorus-containing silicon flame retardant precursor DPOP-Si to the reaction system obtained in Step 2, and continue to stir the reaction so that DPOP-Si participates in the formation process of silicon-oxygen crosslinking network and is uniformly introduced into the network structure through covalent interaction to obtain the biomimetic organic-inorganic hybrid flame retardant precursor liquid, namely PDH-FR flame retardant precursor liquid. Step 4: The PDH-FR flame retardant precursor liquid obtained in Step 3 is uniformly coated on the surface of the substrate and cured to form a biomimetic organic-inorganic hybrid flame retardant coating based on a silicon-oxygen crosslinking network. In step 1, the molar ratio of the double bond in pentaerythritol tetraacrylate to the total amount of dopamine hydrochloride and amino groups in KH550 is 1:1.
11.
2. The preparation method according to claim 1, characterized in that: In step 1, the reaction temperature is 60-80°C and the reaction time is 1-3 h.
3. The preparation method according to claim 1, characterized in that: In step 2, the molar ratio of KH550 to dopamine hydrochloride is 1:3 to 1:
8.
4. The preparation method according to claim 1, characterized in that: In step 2, the hydrolysis-condensation reaction is carried out at a temperature of 60-80°C for 1-4 hours.
5. The preparation method according to claim 1, characterized in that: In step 3, the structural formula of the phosphorus-containing silicon flame retardant precursor DPOP-Si is as follows: 。 6. The preparation method according to claim 1, characterized in that: In step 3, the reaction temperature is 60-80°C and the reaction time is 1-4 h.
7. The preparation method according to claim 1, characterized in that: In step 4, the curing temperature is 25-80°C.
8. The preparation method according to claim 1, characterized in that: In step 4, the substrate includes one or more of polyurethane foam, wood, glass, metal, paper, fabric, and plastic.
9. The preparation method according to claim 1, characterized in that: In step 4, the thickness of the coating is 100-1000 μm.
Citation Information
Patent Citations
Recyclable phosphorus-containing polysiloxane flame-retardant binder and coating
CN117209769A
Corrosive wear detection device for inner wall of wellbore tubular column
CN121762429A