A construction waste-based non-fired brick and its preparation method
By combining composite slag base material with rapid-hardening sulfoaluminate cement and acrylic copolymer, and using high-pressure semi-dry molding and curing process, high-strength and high-density construction slag base non-fired bricks are prepared. This solves the problems of high energy consumption and insufficient performance of non-fired solidified products in the existing technology, and realizes efficient and stable utilization of slag resources.
Patent Information
- Application Number
- CN202611367775.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-09-04
AI Technical Summary
Existing methods of utilizing construction waste have problems of high energy consumption and low efficiency. Furthermore, non-fired solidified products have low early compressive strength, poor water stability, and are prone to disintegration and mudification when exposed to water, which cannot meet the mechanical and water stability safety standards of the foundation.
High-strength, high-density non-fired bricks based on construction waste are prepared by combining composite slag base material with rapid-hardening sulfoaluminate cement and acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer, through specific aggregate ratio, high-pressure semi-dry molding and curing process.
It improves the mechanical load-bearing capacity, water erosion resistance and long-term structural stability of non-fired bricks, solves the problems of low early strength, insufficient water stability and easy disintegration and mud formation when exposed to water in traditional preparation processes, reduces energy consumption and improves the product qualification rate.
Smart Images

Figure CN122853814B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new building materials technology, specifically to a construction waste-based non-fired brick and its preparation method. Background Technology
[0002] Construction projects generate a large amount of construction waste, which constitutes a significant proportion of all construction waste. Currently, the main methods for handling construction waste include off-site transportation and stockpiling, as well as open-air landfilling. These methods not only reduce the resource utilization efficiency of construction waste, but also pose a risk of secondary pollution to surface water, groundwater, and surrounding soil if the trace heavy metals and organic matter they may contain are not effectively solidified.
[0003] Exploring green, high-value-added sustainable resource utilization pathways for construction waste is a development trend aimed at overcoming the aforementioned industry challenges. However, many difficulties exist in practical applications: traditional methods of utilizing construction waste involve sintering processes to produce building materials, which are accompanied by high energy consumption and carbon emissions. Furthermore, using it solely for roadbed subgrades or mine backfilling has low resource utilization efficiency. In the transition to green, low-carbon, non-fired solidification products, the industry faces the challenge of the poor bonding and stabilization effects of traditional cementing materials on construction waste. Even with significantly increased proportions of conventional cementing materials like cement, the solidified products still suffer from fatal defects such as low early compressive strength, easy softening upon contact with water, and even rapid disintegration into mud, failing to meet basic mechanical and water stability safety standards. This lack of applicability of traditional materials results in high costs and low product qualification rates associated with the high-value-added transformation of construction waste, severely restricting the large-scale resource utilization and application of construction waste solid waste in the industrial sector. Summary of the Invention
[0004] In view of the aforementioned existing problems, the present invention is proposed.
[0005] Therefore, this invention provides a construction waste-based non-fired brick and its preparation method, which solves the problems of high energy consumption and low efficiency in existing construction waste utilization methods, as well as the technical problems of low early compressive strength, poor water stability, and easy disintegration and mudification of non-fired solidified products when exposed to water.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: This invention provides a method for preparing non-fired bricks based on construction waste, comprising the following steps: S1. By weight, 50-70 parts of composite slag soil base material are dried at a drying temperature of 110-130 ℃, and after crushing and screening, fine-grained slag soil raw material is obtained; wherein, the composite slag soil base material is prepared by mixing deep fine sandy slag soil and high plasticity red clay slag soil. S2. Add 20-40 parts of medium-fine sand and 5-15 parts of rapid-hardening sulfoaluminate cement to the fine-grained slag raw material, and dry mix at 30-50 r / min to obtain a dry-based premix. S3. Dissolve 0.05~0.75 parts of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer in 12~18 parts of tap water to prepare a polymer aqueous solution; while the dry base premix is continuously stirred, spray the polymer aqueous solution into the dry base premix at an atomization pressure of 2~6MPa, and perform wet mixing for 100~140 s to obtain a plastic homogeneous slurry with a water content of 13~17%; S4. The plastic homogeneous clay is injected into a high-tonnage fully automatic bidirectional hydraulic brick press, and held under a vertical forming pressure of 18~22 MPa for 5~10 s. After demolding, a high-density brick blank is obtained. S5. The high-density brick blank is placed in a standard curing room for sealed curing for 25-30 days to obtain finished non-fired bricks.
[0007] As a preferred embodiment of the method for preparing non-fired bricks based on construction waste soil according to the present invention, in step S1, the amount of composite waste soil material added is 60 parts, the ratio of deep fine sandy waste soil to high plasticity red clay waste soil is 3:2, and the drying temperature is 120 ℃.
[0008] As a preferred embodiment of the method for preparing non-fired bricks based on construction waste soil according to the present invention, in step S2, the amount of medium-fine sand added is 30 parts, the amount of rapid-hardening sulfoaluminate cement added is 10 parts, and the dry mixing speed is 40 r / min.
[0009] In a preferred embodiment of the method for preparing non-fired bricks based on construction waste as described in this invention, in step S3, the amount of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer added is 0.3 parts; and the amount of tap water added is 15 parts.
[0010] In a preferred embodiment of the method for preparing non-fired bricks based on construction waste soil according to the present invention, in step S3, the atomization pressure is 4 MPa, the wet mixing time is 120 s, and the water content of the plastic homogeneous mud is 15%.
[0011] In a preferred embodiment of the method for preparing non-fired bricks based on construction waste as described in this invention, in step S4, the vertical molding pressure is 20 MPa and the pressure holding time is 7 s.
[0012] As a preferred embodiment of the method for preparing non-fired bricks based on construction waste soil according to the present invention, in step S1, the crushing and screening adopts a screen with an aperture of 2~5 mm to obtain fine-grained construction waste soil raw materials with a maximum particle size ≤5 mm.
[0013] As a preferred embodiment of the method for preparing non-fired bricks based on construction waste as described in this invention, in step S3, the effective solid content of the acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer is ≥90%, and the weight-average molecular weight is 800,000 to 1,500,000; the mass concentration of the polymer aqueous solution is 0.5% to 4.5%.
[0014] As a preferred embodiment of the method for preparing non-fired bricks based on construction waste soil according to the present invention, wherein: in step S5, the sealed curing conditions are as follows: Intelligent unmanned logistics vehicles are used to transport demolded brick blanks to a large industrial standard curing room for sealed curing for 28 days. The longest interval between demolding and transfer to the standard curing room shall not exceed 2 hours. In the early stage of the sealed curing, a plastic film is used to cover the surface to prevent water loss. The temperature of the standard curing room is 20±2 ℃ and the relative humidity is ≥95%.
[0015] This invention also provides a construction waste-based non-fired brick, prepared by the above method, wherein: the non-fired brick has a three-dimensional cross-linked composite structure: its internal inorganic rigid skeleton is a dense physical accumulation composed of deep fine sandy waste soil / high plasticity red clay waste soil and medium to fine sand; a polymer flexible membrane constructed by extending and curing acrylic-2-acrylamido-2-methylpropanesulfonic acid copolymer seamlessly covers the particle surface of the physical accumulation; and needle-like ettringite crystals generated by deep hydration of fast-hardening sulfoaluminate cement form an interwoven spatial crystal phase network, anchored in the pores of the polymer flexible membrane and skeleton.
[0016] The beneficial effects of this invention are as follows: By employing composite slag gradation and mineral-based cementitious solidification technology, and through specific aggregate ratios, high-pressure semi-dry molding, and curing processes, a high-strength, high-density construction slag-based non-fired brick is prepared. This solves the technical problems of low early strength, insufficient water stability, and easy disintegration and mudification upon contact with water in traditional non-fired brick preparation processes, thereby improving the mechanical load-bearing capacity, water erosion resistance, and long-term structural stability of the non-fired brick.
[0017] Specifically, this process introduces a specific ratio of sandy slag, clayey slag, and river sand as a composite mix during the aggregate preparation stage. This neutralizes the plasticity defects of individual slag materials. Rapid-hardening sulfoaluminate cement is added to the mixture as a curing agent, overcoming the limitation of traditional cement hydration being hindered in slag materials, thereby improving the macroscopic bonding strength within the unfired bricks. Simultaneously, during the pressing and molding stage, large-scale automated equipment applies a vertical molding pressure of 20 MPa, squeezing out pore air from the material and causing aggregate particles to slip and tightly interlock, increasing the wet density and structural compactness of the molded brick blanks, thus improving slump resistance and reducing the water absorption rate of the finished product. Furthermore, a room-temperature wet curing system is adopted, allowing the high-density brick blanks to rapidly activate the deep hydration and gelation cross-linking of the curing agent in a constant humid and hot environment, forming a dense and robust crystalline network structure. This not only improves the compressive strength and core softening coefficient of the finished product but also avoids the energy consumption and pollution caused by traditional sintering, effectively ensuring high product stability and yield. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 One of the results of optimizing the compounding ratio of slag and soil base materials.
[0020] Figure 2 The second figure shows the results of optimizing the compounding ratio of slag and soil base materials.
[0021] Figure 3 The figure shows the optimization results of the addition amount of medium to fine sand.
[0022] Figure 4 The figure shows the results of optimizing the amount of rapid-hardening sulfoaluminate cement added.
[0023] Figure 5 The result of optimizing the amount of water-reducing agent added is shown in the figure.
[0024] Figure 6 Figure 1 shows the results of optimizing the drying temperature and dry mixing speed.
[0025] Figure 7 The second figure shows the results of optimizing the drying temperature and dry mixing speed.
[0026] Figure 8 Figure 1 shows the optimization results of atomization pressure and wet mixing time.
[0027] Figure 9 The second figure shows the optimization results of atomization pressure and wet mixing time.
[0028] Figure 10 The result of optimizing the pressure holding time is shown in the figure.
[0029] Figure 11 This is a flowchart of a method for preparing non-fired bricks based on construction waste. Detailed Implementation
[0030] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0031] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0032] Secondly, the term "one embodiment" or "example" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the invention. The appearance of an embodiment in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that mutually excludes other embodiments.
[0033] Example 1 This embodiment aims to explore a raw material formulation system for non-fired bricks based on construction waste, and to solve the problems of high energy consumption and low efficiency in existing waste utilization methods, as well as the technical difficulties of low early compressive strength, poor water stability, and easy disintegration and mudification of non-fired solidified products when exposed to water.
[0034] 1.1 Screening of Slag and Soil Base Materials In the construction waste-based non-fired brick system, the waste soil base material is the cornerstone of the physical framework of the non-fired bricks, determining the mechanical load-bearing performance and structural density of the finished product. It needs to possess good macroscopic plasticity and compressive strength potential, but existing single-material waste soil cannot achieve this effect. Therefore, it is necessary to combine different waste soils with complementary physical and chemical properties to neutralize the plasticity defects of single materials. Without affecting the cementation and hydration, this achieves both the tight interlocking required for high-pressure semi-dry molding and the provision of a robust and water-erosion-resistant physical structural barrier, providing a reliable macroscopic carrier for the dense molding and cementation solidification of the overall non-fired brick structure.
[0035] Two representative categories of basic aggregates in the field of construction waste resource utilization were selected for composite use. The binary composite waste (1:1 premix) was blended according to the optimal skeleton support ratio: shallow silty sand / silty clayey waste (82.50 wt%); shallow silty sand / high-plasticity red clay waste (84.15 wt%); shallow silty sand / old loess clayey waste (83.42 wt%); deep fine sand / silty clayey waste (85.24 wt%); deep fine sand / high-plasticity red clay waste (86.36 wt%); deep fine sand / old loess clayey waste (84.73 wt%); coarse sand containing gravel mixed fill / silty clayey waste (81.33 wt%). The blending effect was determined by testing its overall plasticity index, wet compaction compressive strength, and demolding breakage rate. The blending composition was 83.61 wt% (coarse sand containing gravel and mixed fill / high plasticity red clay slag); and 82.84 wt% (coarse sand containing gravel and mixed fill / old loess clay slag).
[0036] Overall plasticity index testing: A fully homogenized binary composite slag soil base material was used. The liquid limit (Wl) and plastic limit (Wp) moisture boundary values of the mixture were measured using a soil liquid and plastic limit combined tester. The plasticity index (Ip = Wl - Wp) was then calculated using the formula. This data characterizes the macroscopic physical morphology neutralization effect after mixing sandy and clayey slag soils. The plasticity index is within a suitable range, indicating that the base material overcomes the inability of single sandy soils to achieve stable shape while avoiding the problem of equipment adhesion caused by single clayey soils.
[0037] Wet brick compressive strength testing: Homogenized slag and soil base material is fed into an industrial bidirectional hydraulic brick-making machine and formed into standard-sized brick blanks under a pressure of 20 MPa. After demolding, a microcomputer-controlled electronic universal testing machine is used to conduct axial compressive strength tests on the uncured wet brick blanks, and the peak load (MPa) at which collapse failure occurs is recorded. This data reflects the initial skeletal interlocking force of the slag and soil mixture under high pressure. The higher the strength, the stronger the resistance to mechanical vibration and self-bearing capacity of the wet brick blank, and the better it can prevent the brick blank from scattering or collapsing.
[0038] Demolding breakage rate detection: Under simulated working conditions, the pressing mold system is linked with an automated palletizing robot to perform pressing and demolding operations at a standard production cycle. Using an industrial vision defect detection system combined with manual sampling, the percentage (%) of defective brick blanks with chipped corners, surface adhesion tearing, or overall breakage is statistically analyzed from the demolded sample. This data reflects the peeling performance between the slag composite system and the metal mold interface. A lower breakage rate indicates better internal toughness and stronger interface anti-adhesion ability, better meeting the requirements of continuous automated mass production in non-fired brick factories.
[0039] The test results are as follows:
[0040] Among them, shallow silty sandy soil / silty clayey soil has a high overall plasticity index, but its wet compressive strength is low, making it prone to particle breakage or collapse; coarse sandy soil with gravel / old loess clayey soil has a high wet compressive strength, but its demolding breakage rate is also high, which is not conducive to subsequent stripping operations. Therefore, deep fine sandy soil / high plasticity red clay soil with better overall performance was selected as the soil base material.
[0041] In this invention, the deep fine sandy soil refers to construction waste generated during the construction process, characterized primarily by fine sandy soil; the high-plasticity red clay soil refers to construction waste generated during the construction process, characterized primarily by clayey soil and possessing high plasticity. 1.2 Screening of Auxiliary Aggregates Although the selected slag base material already possesses good molding plasticity and initial interlocking force, its discontinuous micro-particle gradation and high mud powder content result in large internal pores and a lack of rigid support, reducing the mechanical strength and water stability of the finished product. Therefore, auxiliary aggregates are introduced, utilizing their hardness and continuous particle size to fine-tune the gradation and fill the pores of the base material, thereby constructing a denser physical skeleton and improving the compressive strength and water erosion resistance of the product.
[0042] After fixing the slag base material, the river sands were dry-mixed according to the optimal gradation and mixing ratio: very coarse sand (18.53 wt%), coarse sand (22.37 wt%), medium-coarse sand (25.41 wt%), medium-fine sand (28.66 wt%), fine sand (19.25 wt%), and extra-fine sand (12.82 wt%). The filling effect was determined by testing the standard curing compressive strength, immersion softening coefficient, and standard drying shrinkage rate of each group.
[0043] Standard curing compressive strength test: Each pressed specimen was placed in a standard curing room at 20 ℃ and relative humidity ≥ 95% and left to stand for 28 days. After curing, a destructive axial compressive strength test was conducted using an electro-hydraulic servo universal testing machine at a loading rate of 0.5~1.5 MPa / s, and the peak load (MPa) at which the structure fractured and failed was recorded. This value reflects the skeletal support force of the river sand; the higher the strength, the stronger the load-bearing potential and resistance to damage of the finished product, and the better it can meet the pressure-bearing requirements of buildings.
[0044] Water Softening Coefficient Test: Mature specimens from the same batch, cured for 28 days, were divided into two groups. The baseline group was dried to constant weight in an oven to determine its oven-dry compressive strength. The water-immersed group was immersed in a water tank at 20 ℃, and its saturated compressive strength was determined after 96 hours of hydration and erosion. The coefficient was obtained by calculating the ratio of saturated strength to oven-dry strength. This data reflects the compact filling effect of river sand gradation on the micropores of the slag soil. The closer it is to 1, the lower the porosity of the system, the more complete the water-stable barrier, and the more effectively it can resist the stripping and damage caused by external water infiltration.
[0045] Standard shrinkage rate test: The molded specimens were placed in a constant temperature and humidity chamber at 20 ℃ and 50% relative humidity for accelerated dehydration. Probes were pre-embedded at both ends of the specimens, and a high-precision vertical shrinkage meter was used to monitor and record the absolute percentage (%) of axial length reduction within 28 days. This value reflects the volume stability and microcrack formation tendency of the mixture during the moisture evaporation and curing process. The lower the shrinkage rate, the stronger the resistance of the river sand, and the better it can prevent the product from cracking later.
[0046] The test results are as follows:
[0047] Among them, coarse sand has a high standard compressive strength, but its water softening coefficient is low, making it unsuitable for outdoor environments; extra-fine sand has a high water softening coefficient, but its standard shrinkage rate is high, which easily leads to mass cracking. Therefore, medium-fine sand with better overall performance was selected as the auxiliary aggregate of this invention.
[0048] 1.3 Screening of gel curing agents Cementitious curing agents are the core chemical reinforcement for the long-term performance of unfired bricks. Purely physical compaction molding is prone to stress relaxation and water-induced disintegration, resulting in insufficient strength and water stability. By introducing cementitious curing agents, they fill capillary pores in situ and form chemical cross-links with slag and river sand aggregates, transforming loose particles into a dense double-network structure. This improves the product's water stability, compressive strength, and volume stability, and effectively constrains the drying shrinkage of the red clay base material.
[0049] Six materials with typical hydration reactivity and interfacial crosslinking characteristics were selected for screening. Under uniform industrial bidirectional hydraulic molding and standard curing conditions, the selected materials were added in their optimal proportions as follows: PO 42.5 silicate cement (8.53 wt%); potentially hydraulic ultrafine blast furnace slag powder (12.47 wt%); high pozzolanic activity grade I high-calcium fly ash (14.61 wt%); strongly alkaline activated industrial carbide slag (9.35 wt%); rapid-hardening sulfoaluminate cement (10.82 wt%); and industrial quicklime powder (5.50 wt%). The curing effect was determined by testing the demolding compressive strength, standard curing compressive strength, and standard drying shrinkage rate of each group.
[0050] 72-hour early demolding compressive strength test: The slag-soil composite base material and each group of cementitious curing agents were pressed into standard brick blanks using a 20 MPa industrial bidirectional hydraulic brick press. After static activation for 72 hours at 20 ℃ and relative humidity ≥95%, an axial dynamic load was applied using an electro-hydraulic servo microcomputer universal testing machine at a loading rate of 0.5~1.5 MPa / s until the brick blank collapsed. The peak failure load (N) was extracted and divided by the total area of the compressed surface to obtain the individual compressive strength value (MPa). This data reflects the reaction kinetics response of the cementing system and the initial crystal nucleus growth penetration rate. Higher strength indicates stronger in-situ bonding and support effects of the curing agent.
[0051] The test results are as follows:
[0052] Among them, PO 42.5 silicate cement has a high early demolding compressive strength at 72 hours, but its standard shrinkage rate is high, making it prone to cracking; Grade I high-calcium fly ash has a lower standard shrinkage rate, but its early demolding compressive strength at 72 hours is low, making it prone to edge spalling or brittle fracture of the brick blank. Therefore, rapid-hardening sulfoaluminate cement, which has a better overall performance, was selected as the gel curing agent.
[0053] 1.4 Screening of water-reducing agents While the aforementioned solidification system possesses good early compressive strength and low shrinkage characteristics, the large amount of hydrophilic clay minerals within the system easily triggers water absorption and agglomeration, leading to a sharp increase in the water demand of the mixture and low compaction. Therefore, a water-reducing agent is introduced, utilizing its unique adsorption anchoring groups and steric hindrance effect to achieve efficient deflocculation and water release of clay agglomerates without compromising the overall high strength and low drying shrinkage baseline of the unfired bricks, thereby improving the molding process and final mechanical compaction properties of the mixture.
[0054] Six representative water-reducing agents were selected as candidates. They were dissolved in tap water and then sprayed into the pre-dry mixed composite powder for mixing. The mixture was then sent to a two-way hydraulic press for pressing and standard curing. The deflocculation and water release effects of different components were judged by testing the wet blank forming density, demolding compressive strength, standard curing compressive strength and standard drying shrinkage rate.
[0055] Wet brick forming density test: After wet mixing with low water content, the mixture is fed into the mold cavity of a fully automatic two-way hydraulic press. It is then pressed in a single stroke at 20 MPa and demolded. The mold cavity filling rate and the density of the wet brick are recorded. This value reflects the deflocculation and water release efficiency of the water-reducing agent in water-scarce and high-mud-content conditions. Higher density indicates that the water-reducing agent can more effectively remove bound water between clay layers, thus ensuring the feasibility of large-scale automated hydraulic granulation.
[0056] The test results are as follows:
[0057] Among them, hydroxyethyl methacrylate copolymer has a high wet molding density, but its standard shrinkage rate is high, making it prone to cracking; sodium naphthalenesulfonic acid formaldehyde condensate has a low standard shrinkage rate, but its demolding compressive strength is low, making it prone to brittle fracture, which is not conducive to subsequent load-bearing requirements. Therefore, acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer, which has better overall performance, was selected as the water-reducing agent.
[0058] Example 2 Reference Figures 1 to 5 This is the second embodiment of the present invention. After clarifying the qualitative functions and microscopic interface anchoring mechanisms of each core component, determining its quantitative proportion in the final unfired brick product is the key to maximizing the hydraulic molding efficiency and balancing hydration shrinkage stress under low water content. Therefore, based on the performance boundary conditions established by the aforementioned screening experiments, this embodiment further explores the optimal addition amount of each core component, aiming to lock in the optimal process formulation that combines absolute volume stability and load-bearing mechanical performance.
[0059] 2.1 Optimization of the mix ratio of slag and soil base materials Having identified deep fine sandy soil and highly plastic red clay as the parent matrix, their ratio determines the balance between physical and mechanical cohesion and later volumetric stability of the unfired brick base. If the proportion of deep fine sandy soil is too high, the mixture will cause the skeleton to collapse during demolding, leading to brick breakage; if the proportion of highly plastic red clay is too high, it will increase the specific surface area and drying shrinkage potential of the system, causing dehydration cracking in the later stages of curing. Therefore, it is essential to select the optimal blending ratio to balance high demolding rate and low drying shrinkage efficiency.
[0060] With the total mass set at 100%, and the amount of medium-fine sand and rapid-hardening sulfoaluminate cement added fixed, the mixture was supplemented with slag base material. The deep fine sandy slag and high plastic red clay were mixed in 10% increments, and nine experimental groups were set up. The wet compressive density, compacted dry density and standard drying shrinkage of the different proportion systems were tested to evaluate their compounding effect.
[0061] Wet brick compressive strength test: After demolding the prepared standard brick blank, an axial dynamic load is applied using an electro-hydraulic servo microcomputer universal testing machine at a loading rate of 0.1~0.5 MPa / s until the wet brick blank undergoes yielding deformation or edge shear collapse failure. The peak failure load (N) is extracted and divided by the total area of the compressed surface to obtain the wet brick compressive strength value (MPa). This data reflects the self-locking efficiency of the microparticles in the system, the surface tension of the capillary water film, and the initial mechanical cohesion of the matrix; the higher the strength, the more stable its resistance to collapse and the more stable its shape-preserving support base.
[0062] Compacted dry density test: The dimensions of the prepared standard brick blanks were measured using digital vernier calipers, and the molding reference volume (cm³) was calculated. Subsequently, the bricks were dried at 60 ℃ until their mass became constant, and their absolute dry weight (g) was measured using an electronic analytical balance. This dry weight was then divided by the molding reference volume to calculate the compacted dry density value (g / cm³). This value characterizes the degree of spatial interlocking and compaction between the rigid skeleton of fine sand and the plastic colloid of red clay; a higher value indicates better overall compaction.
[0063] The results are as follows Figure 1 , Figure 2 As shown, with the increase of the proportion of fine sandy soil, the standard shrinkage rate continuously decreases, and the compressive strength of wet blanks and the compacted dry density both show a trend of first increasing and then decreasing. A nonlinear interpolation fitting was performed on the critical cracking threshold of the standard shrinkage rate to define a safe shrinkage range. Within this range, a quadratic polynomial regression fitting was performed on the maximum gain effect of wet blank compressive strength and compacted dry density, yielding the extreme points of wet blank compressive strength at (58.51, 41.49) and compacted dry density at (61.26, 38.74). To achieve a balance between high-pressure demolding tolerance and hydration network density, the average value (59.89, 40.12) was taken as the optimal theoretical point. Based on the industrialized feeding tolerance, the optimal blending ratio of deep fine sandy soil and high-plasticity red clay was selected as 3:2.
[0064] 2.2 Optimization of Medium-Fine Sand Addition Amount The amount of medium-fine sand added determines the balance between volumetric stability and structural density of unfired bricks. If the amount of medium-fine sand is too high, the limited slag matrix will not be able to fill the gaps in the skeleton, resulting in a decrease in the compacted dry density and compressive strength of the brick, and making it prone to brittle fracture during demolding. If the amount of medium-fine sand is too low, the continuous shrinkage network of red clay will not be effectively suppressed, leading to dehydration shrinkage cracking in the later stage, weakening the final load-bearing capacity of the brick. Therefore, it is necessary to select the optimal amount of medium-fine sand to construct the densest physical skeleton, taking into account both low shrinkage rate and high mechanical strength as engineering standards.
[0065] With the total mass set at 100%, and the amount of rapid-hardening sulfoaluminate cement added fixed, the amount of medium-fine sand added ranged from 10.0 to 50.0 wt%, with a gradient step of 10.0 wt%, setting up 5 experimental groups with different concentrations. The remaining amount was supplemented using slag and soil base material. The wet compressive strength, compacted dry density, and standard drying shrinkage of the different group systems were tested.
[0066] The results are as follows Figure 3 As shown, with the increase of medium-fine sand content, the standard drying shrinkage rate shows a monotonically decreasing trend, while the compacted dry density and wet green compact compressive strength show a change of first increasing and then decreasing. A nonlinear interpolation fitting was performed on the critical cracking threshold of the standard drying shrinkage rate to define a safe range. Within this range, a quadratic polynomial regression fitting was performed on the maximum gain effect of wet green compact compressive strength and compacted dry density, yielding an addition amount of 29.17 wt% corresponding to the extreme point of wet green compact compressive strength and 30.62 wt% corresponding to the extreme point of compacted dry density. To achieve a balance between demolding cohesion and rigid skeleton interlocking, the average value of 29.90 wt% was taken as the optimal addition amount. Based on industrial feeding accuracy, 30.0 wt% was ultimately selected as the optimal addition amount of medium-fine sand.
[0067] 2.3 Optimization of the Dosage of Rapid-Hardening Sulfoaluminate Cement Rapid-hardening sulfoaluminate cement, as the core cementing agent in the system, determines the final mechanical properties and volume stability of the bricks based on its dosage. If the dosage is too low, the final compressive strength of the finished product will fail to meet engineering acceptance standards; if the dosage is too high, it will disrupt the initial physical framework balance, causing the drying shrinkage rate to exceed the safety limit and inducing microcracks. Therefore, it is essential to determine the optimal dosage to achieve a balance between hydration cementing strength and chemical self-shrinkage stress.
[0068] The addition amount of rapid-hardening sulfoaluminate cement ranged from 5.0 to 15.0 wt%, with a gradient step of 1.0 wt%, and 11 concentration experimental groups were set up. The process effect of different addition amounts was evaluated by detecting the water softening coefficient, standard drying shrinkage rate and standard curing compressive strength.
[0069] The results are as follows Figure 4As shown, with the increase of rapid-hardening sulfoaluminate cement addition, the standard drying shrinkage and immersion softening coefficient monotonically increase, while the standard curing compressive strength shows a trend of first increasing and then decreasing. Through data fitting, the extreme point of standard curing compressive strength is found at an addition amount of 10.23 wt%, and the hydration efficiency saturation point of the immersion softening coefficient is found at an addition amount of 9.89 wt%. To achieve a balance between load-bearing capacity and water-resistant hydration capacity, the average value of 10.06 wt% is taken as the optimal addition amount, and at this point, the standard drying shrinkage is within a safe range. Based on the industrialized feeding error tolerance, 10.0 wt% is finally selected as the optimal addition amount.
[0070] Based on the above optimization experiments, it can be indirectly concluded that the total amount of slag and soil base material added is 60.0 wt%. Based on its optimal compounding ratio of 3:2, the amount of deep fine sandy slag and soil added is 36.0 wt%, and the amount of high plasticity red clay added is 24.0 wt%.
[0071] 2.4 Optimization of Water-Reducing Agent Dosage The amount of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer added was set to 1.0~5.0 wt% of the total mass of rapid hardening sulfoaluminate cement. Five experimental groups were set up with a gradient step of 1.0 wt% to detect the compacted dry density, standard curing compressive strength and standard drying shrinkage of different group systems.
[0072] The results are as follows Figure 5 As shown, with the increase of water-reducing agent dosage, the standard shrinkage rate increases monotonically, while the compacted dry density and standard compressive strength exhibit a quadratic parabolic curve characteristic of first increasing and then decreasing. Data fitting revealed that the extreme point of the standard compressive strength was at an addition amount of 2.91 wt%, and the extreme point of the compacted dry density was at an addition amount of 3.12 wt%. To achieve a balance between mechanical gain and density, the average value of 3.02 wt% was taken as the optimal addition amount, and at this point, the standard shrinkage rate was within a safe range. Based on industrial weighing accuracy, 3 wt% was ultimately selected as the optimal addition amount, meaning the optimal addition amount of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer was 0.3 wt%.
[0073] Example 3 Reference Figures 6 to 10This is the third embodiment of the present invention. This embodiment aims to optimize and correct the parameters of the industrial-scale process for a preferred formulation determined in the laboratory. Although the optimal ratio of the system has been established at the microscopic level, the scale-up process from laboratory pilot-scale trials to ton-scale industrial production is often accompanied by dynamic changes in the physical field. In particular, for steps involving physicochemical rheology, high-pressure atomization micro-encapsulation, and micro-skeletal exhaust construction, changes in the physical field can easily amplify microstructural defects, thus affecting the stability of the finished product. Therefore, it is necessary to adjust the key process parameters for industrial production to ensure large-scale production.
[0074] 3.1 Optimization of drying temperature and dry mixing speed 36.0 wt% deep fine sandy slag and 24.0 wt% high-plasticity red clay were fed into an industrial drying kiln for dewatering pretreatment. After crushing and screening to obtain fine-grained slag, 30.0 wt% medium-to-fine sand was added and dry-mixed in a twin-shaft forced mixer. This stage aims to break down and deconstruct the pseudo-agglomerations of the red clay without inducing secondary grinding of the aggregate or high-moisture clogging of the screen, and to achieve a homogeneous distribution of the binary slag matrix and the medium-fine sand aggregate. Therefore, the thermodynamic matrix formed by the drying temperature and the dry-mixing speed of the main shaft is a key factor determining the final physical density and macroscopic mechanical stability of the formed brick blank.
[0075] The drying temperature was controlled from 80.0 to 150.0 ℃ with a gradient step of 10.0 ℃; the dry mixing speed was controlled from 20 to 60 r / min with a gradient step of 10.0 r / min. Experimental groups were set up by cross-variable setting, and the processing effect of different parameters was evaluated by residual moisture content, micro powder increase rate and compacted dry density.
[0076] Residual moisture content detection: Under simulated operating conditions, the mixed slag material after heat treatment was taken, and the mass percentage (%) of residual free water in the material was measured and calculated using a rapid halogen moisture analyzer combined with a standard constant temperature oven weighing method. This data reflects the balance between the thermal efficiency of the drying system and the water decomposition and adsorption on the surface of the slag microparticles. A value that is too high may cause false agglomeration of the red clay and blockage of the screen, while a value that is too low will cause a surge in dry friction in the system.
[0077] Micropowder increase rate detection: Under simulated working conditions, samples were taken from the feed and discharge ends of a large twin-shaft forced mixer. A laser particle size analyzer, combined with standard test sieves, was used to compare the mass percentage difference of the micropowder components in the system before and after dry mixing, and the micropowder increase rate (%) was calculated. This data reflects the degree of damage to the physical gradation of aggregates caused by thermodynamic field coupling. A higher value indicates more severe secondary grinding of medium and fine sand and slag.
[0078] The results are as follows Figure 6 , Figure 7As shown, with the increase of drying temperature and dry mixing speed, the residual moisture content continuously decreases, the increase rate of micro-powder continuously increases, while the compacted dry density exhibits a three-dimensional parabolic change. A surface boundary fitting was performed on the rheological critical point of residual moisture content to define a safe range. Within this range, the maximum gain effect of micro-powder increase rate and compacted dry density was fitted, revealing that the minimum value of micro-powder increase rate falls at (116.47, 32.68), and the maximum value of compacted dry density falls at (124.21, 46.85). To achieve a balance between gradation preservation and skeleton density, the average value (120.34, 39.77) was taken as the theoretical optimal value. Based on the parameter adjustment accuracy of industrial equipment, 120 ℃ was finally selected as the optimal drying temperature, and 40 r / min as the optimal dry mixing parameter.
[0079] 3.2 Optimization of atomization pressure and wet mixing time The atomization spraying pressure and wet mixing time are the core variables determining the deep penetration of acrylic-2-acrylamido-2-methylpropanesulfonic acid copolymer molecules into the matrix and the in-situ activation of the rapid-hardening hydration network. If the atomization pressure is too low, it may cause severe local hydration and agglomeration of the cement; if the wet mixing time is too long, it will cause the nascent hydration crystals to break down, which not only weakens the electrostatic lubrication effect between particles, but also induces an irreversible transformation of the clay from a highly active plastic rheological state to an inert pseudo-set dead paste. Therefore, it is necessary to find an optimal parameter that can ensure deep coating of the solution without causing the hydration skeleton to break down and plasticity to be lost over time.
[0080] The atomization pressure ranged from 2 to 6 MPa with a gradient step of 1 MPa; the wet mixing time ranged from 60 to 180 s with a gradient step of 30 s. Experimental groups were set up by cross-variables, and the processing effect of different parameters was evaluated by using the actual retained moisture content, the micro-agglomeration rate of the mud, and the standard curing compressive strength.
[0081] Actual moisture content interception test: After wet mixing, a sample was taken from the discharge port of the twin-shaft forced mixer, placed in a sealed constant-weight aluminum box, and weighed using an electronic analytical balance to determine its total wet weight (g). It was then placed in a 105 ℃ electric heating forced-air drying oven until its mass became constant, and its absolute dry weight (g) was measured again. The actual moisture content interception (%) was calculated by determining the percentage of water loss to total wet weight. This value characterizes the dynamic balance between the high-pressure atomization injection of the water-reducing agent solution and the aerosol dispersion loss caused by the strong wind dust removal system; the closer the value is to 15%, the better the microscopic liquid phase is locked into the slag substrate.
[0082] Micro-agglomeration rate test of clay: 1000 g of wet clay was weighed as the total test basis weight and spread evenly on a standard test sieve with a aperture of 4.75 mm for standard low-frequency vibration sieving. The mass (g) of the hard lumps that could not pass through the sieve was collected and weighed using an electronic analytical balance. This mass was then divided by the total test basis weight to calculate the micro-agglomeration rate (%) of the clay. This value reflects the uniformity of diffusion of the atomized liquid phase in the matrix space and the degree of deterioration of local rapid-hardening sulfoaluminate cement hydration agglomeration; the closer the value is to 0%, the better the micro-atomization and coating of the solution, avoiding the generation of micro-rigid defects inside the brick.
[0083] The results are as follows Figure 8 , 9 As shown, with the increase of atomization pressure and wet mixing time, the actual retained moisture content shows a monotonically decreasing trend, the micro-agglomeration rate of the mud material shows a trend of first decreasing and then increasing, and the standard curing compressive strength shows a parabolic characteristic of first increasing and then decreasing. A surface boundary fitting was performed on the safe critical point of the actual retained moisture content to define a safe range. Within this range, the maximum gain effect of the micro-agglomeration rate of the mud material on the standard curing compressive strength was fitted, and the minimum value of the micro-agglomeration rate of the mud material was obtained at (4.83, 106.44), and the maximum value of the standard curing compressive strength was obtained at (3.96, 118.65). To achieve a balance between uniform liquid phase dispersion and the non-destructive construction of the rapid hardening hydration network, the average value (4.40, 112.55) was taken as the theoretical optimal point. Based on the industrial-scale output adjustment accuracy, 4 MPa was finally selected as the optimal atomization pressure, and 120 s as the optimal wet mixing time.
[0084] 3.3 Optimization of pressure holding time Semi-dry mixtures are fed into specially designed molds in a high-tonnage, fully automatic, bidirectional hydraulic brick press for extreme pressure molding. Based on engineering experience and consensus in materials mechanics regarding extreme pressure preparation from solid waste resources, the molding pressure in industrial production is generally between 18 and 22 MPa to ensure the densification effect of the system in large-scale production and to avoid secondary brittle fracture of rigid fine aggregates. After determining the molding pressure, the elastic internal stress relaxation window formed by the holding time becomes a key control point affecting the demolding volume stability and final mechanical properties of the brick blank.
[0085] The vertical forming pressure was set to 20 MPa, and the holding time ranged from 5 to 10 s. With a gradient step of 1 s, six experimental groups were set up. The demolding breakage rate, compacted dry density, and standard curing compressive strength of different groups were tested to evaluate the processing effect of different holding times.
[0086] The results are as follows Figure 10As shown, with the extension of the holding time, the compacted dry density continuously increases, the demolding breakage rate continuously decreases, while the standard curing compressive strength shows a trend of first increasing and then decreasing. A safe range was defined by fitting the densification saturation point of the compacted dry density. Within this range, the extreme point of the standard curing compressive strength was fitted and found to be at a holding time of 7.12 s, at which point the demolding breakage rate is within the safe range. Based on the time parameter adjustment accuracy of industrial equipment, 7 s was ultimately selected as the optimal holding time.
[0087] 3.4 Standard Curing of Finished Brick Blanks Intelligent unmanned logistics vehicles are used to transport the demolded brick blanks to a large industrial standard curing room for sealed curing, with the indoor temperature set at 20±2 ℃ and relative humidity ≥95%. Under this environment, rapid-hardening sulfoaluminate cement undergoes deep hydration, and the resulting needle-like ettringite crystals interweave and anchor within the dense physical framework, causing the overall structure to solidify and form the finished non-fired brick.
[0088] Example 4 Reference Figure 11 This is the fourth embodiment of the present invention. This embodiment provides a method for preparing non-fired bricks based on construction waste, specifically including the following steps: S1. Raw material pretreatment 36 parts of deep fine sandy slag and 24 parts of high-plasticity red clay slag (mixed in a ratio of 3:2, totaling 60 parts) were weighed as composite slag base material. The above composite slag base material was fed into an industrial drying kiln and dried and dehydrated at 120 ℃; then crushed by a large crusher and introduced into an industrial vibrating screening system, and screened using a screen with an aperture of 2~5 mm to obtain fine slag raw material with a maximum particle size ≤5 mm.
[0089] S2. Dry-based mixture The above-mentioned fine-grained slag raw materials are put into a large industrial mixer, and 30 parts of medium-fine sand and 10 parts of rapid-hardening sulfoaluminate cement are added in sequence. The mixture is stirred and mixed at a speed of 40 r / min to obtain a dry-based premix.
[0090] S3. Atomized wet mixing 0.3 parts of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer were dissolved in 15 parts of tap water to prepare a polymer solution with a mass concentration of approximately 2%. Under continuous stirring in a mixer, the solution was sprayed into the dry-based premix at a pressure of 4 MPa using a high-pressure atomizing spray system, and wet-mixed for 120 s to obtain a plastic homogeneous slurry. Random samples were taken from the outlet to determine the actual retained moisture content, which was found to be 15% for this batch of slurry.
[0091] S4. High-pressure molding The homogeneous plastic clay is injected into the mold of a high-tonnage fully automatic bidirectional hydraulic brick press and pressed for 7 seconds at a vertical forming pressure of 20 MPa to fully expel internal air and compact the aggregate. After automatic demolding by the hydraulic press, a high-density brick blank is obtained.
[0092] S5. Sealed curing and solidification Using an intelligent unmanned logistics vehicle, the demolded brick blanks are delivered to a large-scale industrial standard curing chamber within 30 minutes, where their surfaces are covered with a polyethylene film for early anti-water loss treatment. The indoor sealed curing conditions are set as follows: temperature 20±2℃, relative humidity ≥95%, and standardized curing is carried out for 28 days to obtain the finished non-fired bricks.
[0093] The prepared unfired bricks had the following characteristics: compacted dry density 2.04 g / cm³, standard curing compressive strength 25.86 MPa, immersion softening coefficient 0.88, standard drying shrinkage rate 0.042%, wet compressive strength 3.21 MPa, demolding breakage rate 0.35%, and actual retained moisture content 15%. Furthermore, leaching toxicity tests were conducted, and all leaching indicators for heavy metals and organic pollutants were below the limits specified in the "Standard for Identification of Leaching Toxicity of Solid Waste".
[0094] In summary, by employing composite slag gradation and mineral-based cementitious solidification technology, and through specific aggregate ratios, high-pressure semi-dry molding, and curing processes, a high-strength, high-density construction slag-based non-fired brick was prepared. This solves the technical problems of low early strength, insufficient water stability, and easy disintegration and mudification upon contact with water in traditional non-fired brick preparation processes, thereby improving the mechanical load-bearing capacity, water erosion resistance, and long-term structural stability of the non-fired brick.
[0095] Specifically, this process introduces a specific ratio of sandy slag, clayey slag, and river sand as a composite mix during the aggregate preparation stage. This neutralizes the plasticity defects of individual slag materials. Rapid-hardening sulfoaluminate cement is added to the mixture as a curing agent, overcoming the limitation of traditional cement hydration being hindered in slag materials, thereby improving the macroscopic bonding strength within the unfired bricks. Simultaneously, during the pressing and molding stage, large-scale automated equipment applies a vertical molding pressure of 20 MPa, squeezing out pore air from the material and causing aggregate particles to slip and tightly interlock, increasing the wet density and structural compactness of the molded brick blanks, thus improving slump resistance and reducing the water absorption rate of the finished product. Furthermore, a room-temperature wet curing system is adopted, allowing the high-density brick blanks to rapidly activate the deep hydration and gelation cross-linking of the curing agent in a constant humid and hot environment, forming a dense and robust crystalline network structure. This not only improves the compressive strength and core softening coefficient of the finished product but also avoids the energy consumption and pollution caused by traditional sintering, effectively ensuring high product stability and yield.
[0096] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing non-fired bricks based on construction waste, characterized in that, Includes the following steps: S1. By weight, 50-70 parts of composite slag soil base material are dried at a drying temperature of 110-130 ℃, and after crushing and screening, fine-grained slag soil raw material is obtained; wherein, the composite slag soil base material is prepared by mixing deep fine sandy slag soil and high plasticity red clay slag soil. S2. Add 20-40 parts of medium-fine sand and 5-15 parts of rapid-hardening sulfoaluminate cement to the fine-grained slag raw material, and dry mix at 30-50 r / min to obtain a dry-based premix. S3. Dissolve 0.05~0.75 parts of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer in 12~18 parts of tap water to prepare a polymer aqueous solution; while the dry premix is continuously stirred, spray the polymer aqueous solution into the dry premix at an atomization pressure of 2~6 MPa and perform wet mixing for 100~140 s to obtain a plastic homogeneous slurry with a water content of 13~17%; S4. The plastic homogeneous clay is injected into a high-tonnage fully automatic bidirectional hydraulic brick press, and held under a vertical forming pressure of 18~22 MPa for 5~10 s. After demolding, a high-density brick blank is obtained. S5. The high-density brick blank is placed in a standard curing room for sealed curing for 25-30 days to obtain finished non-fired bricks.
2. The method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S1, the amount of composite slag base material added is 60 parts, the ratio of deep fine sandy slag to high plasticity red clay slag is 3:2, and the drying temperature is 120 ℃.
3. The method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S2, the amount of medium-fine sand added is 30 parts, the amount of rapid-hardening sulfoaluminate cement added is 10 parts, and the dry mixing speed is 40 r / min.
4. The method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S3, the amount of acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer added is 0.3 parts; the amount of tap water added is 15 parts.
5. A method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S3, the atomization pressure is 4 MPa, the wet mixing time is 120 s, and the moisture content of the plastic homogeneous mud is 15%.
6. A method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S4, the vertical forming pressure is 20 MPa and the holding time is 7 s.
7. A method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S1, the crushing and screening process uses a screen with a aperture of 2-5 mm to obtain fine-grained slag raw materials with a maximum particle size of ≤5 mm.
8. The method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S3, the effective solid content of the acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer is ≥90%, and the weight-average molecular weight is 800,000 to 1,500,000; the mass concentration of the polymer aqueous solution is 0.5% to 4.5%.
9. The method for preparing non-fired bricks based on construction waste according to claim 1, characterized in that, In step S5, the sealed curing conditions are as follows: Intelligent unmanned logistics vehicles are used to transport demolded brick blanks to a large industrial standard curing room for sealed curing for 28 days. The longest interval between demolding and transfer to the standard curing room shall not exceed 2 hours. In the early stage of the sealed curing, a plastic film is used to cover the surface to prevent water loss. The temperature of the standard curing room is 20±2 ℃ and the relative humidity is ≥95%.
10. A type of non-fired brick based on construction waste, prepared by any one of the methods described in claims 1 to 9, characterized in that, The unfired brick has a three-dimensional cross-linked composite structure: its internal inorganic rigid skeleton is a dense physical accumulation composed of deep fine sandy soil / high plasticity red clay soil and medium to fine sand; a polymer flexible membrane constructed by extending and curing acrylic-2-acrylamido-2-methylpropanesulfonic acid copolymer seamlessly covers the particle surface of the physical accumulation; needle-like ettringite crystals generated by deep hydration of fast-hardening sulfoaluminate cement form a spatial crystalline network, anchored in the pores of the polymer flexible membrane and skeleton.
Citation Information
Patent Citations
Water-containing undisturbed shield muck baking-free building material and preparation method thereof
CN111393117A
Preparation method of residue soil baking-free brick
CN115107144A