High-strength anti-creep and aging-resistant cable and composite inorganic filler
Patent Information
- Application Number
- CN202611547980.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-03
AI Technical Summary
Existing PVC cable insulation materials are prone to creep deformation and thermo-oxidative aging during long-term service. Traditional inorganic filler modification methods cannot effectively improve creep resistance and aging resistance, resulting in insufficient lifespan and stability of the materials in high-end cable applications.
A type II anhydrous calcium sulfate whisker-supported cerium dioxide composite inorganic filler was prepared by in-situ loading process and modified with silane coupling agent. The one-dimensional skeleton of the whisker enhances the tensile strength of the material, and the UV/thermal-oxidative shielding effect of cerium dioxide improves the aging resistance of the material.
It achieves high strength, low creep, resistance to damp heat and ultraviolet radiation, and stable insulation properties in PVC cable insulation materials, adapting to harsh working conditions, extending cable service life, reducing modification costs, and facilitating industrialization and promotion.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable technology, specifically to a high-strength, creep-resistant, and aging-resistant cable and a composite inorganic filler. Background Technology
[0002] Polyvinyl chloride (PVC) is one of the most widely used insulation substrates in the cable industry due to its excellent insulation properties, mature processing technology, low cost, and balanced mechanical properties. It is widely suitable for cable insulation coating needs in various scenarios such as civil buildings, industrial equipment, rail transportation, and power transmission. However, pure PVC matrix has significant performance shortcomings, which limits its in-depth application in high-end and harsh operating conditions of cables.
[0003] During long-term service, the insulation layer of PVC cables is susceptible to the effects of continuous mechanical stress, temperature fluctuations, ultraviolet radiation, and humid environments, leading to significant creep deformation. Under long-term static and dynamic loads, PVC molecular chains are prone to slippage and relaxation, resulting in decreased dimensional stability and structural collapse of the insulation layer. This, in turn, causes uneven insulation thickness and localized stress concentration, significantly reducing the mechanical protection performance and service life of the cable. Simultaneously, PVC materials are prone to thermo-oxidative aging and photo-aging during long-term service, exhibiting phenomena such as molecular chain breakage, decreased cross-linking degree, material embrittlement and cracking, and decreased insulation resistance. Under extreme operating conditions, this can easily lead to safety hazards such as leakage and short circuits, failing to meet the requirements of long life, high stability, and weather resistance for high-end cables.
[0004] To improve the mechanical properties and aging resistance of PVC insulation materials, existing technologies often employ a combination of single inorganic fillers and organic additives for modification, commonly using calcium carbonate, talc, and ordinary calcium sulfate powder as reinforcing fillers. However, conventional powder fillers suffer from uneven particle size, poor compatibility with the PVC matrix interface, and a tendency to agglomerate. They can only slightly improve the basic mechanical properties of the material and cannot effectively improve the creep resistance of the PVC matrix. Furthermore, stress concentration defects easily occur at the filler-matrix interface, which can reduce the material's aging resistance and insulation consistency. In addition, while single anti-aging fillers such as cerium dioxide and rare earth oxides can improve the weather resistance and aging resistance of PVC, the particles are prone to agglomeration, resulting in poor dispersibility and high modification costs when used alone. They also lack significant mechanical reinforcement and creep resistance effects, making it difficult to achieve a synergistic improvement in the high strength, creep resistance, and aging resistance of PVC materials.
[0005] Calcium sulfate whiskers, as a one-dimensional functional inorganic filler, possess high strength, high modulus, excellent dimensional stability, and wear and deformation resistance, effectively compensating for the deficiencies of PVC matrix in terms of creep resistance and insufficient mechanical strength. Cerium dioxide, with its excellent ultraviolet absorption and thermo-oxidative free radical scavenging capabilities, is a highly efficient anti-aging modification component for polymer materials. Currently, there are few existing technologies that use type II anhydrous calcium sulfate whiskers and cerium dioxide in situ to modify PVC cable insulation materials. Conventional physical blending methods suffer from uneven dispersion of the two-phase fillers, weak interfacial bonding, and limited modification effects, failing to simultaneously address the multiple technical pain points of PVC insulation materials, such as low mechanical strength, poor creep resistance, and easy aging, severely restricting the industrial application of high-performance PVC cable insulation materials. Therefore, developing a modification scheme that can synergistically improve the mechanical strength, creep resistance, and aging resistance of PVC insulation materials has significant engineering application value. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a composite inorganic filler. A second objective is to provide a high-strength, creep-resistant, and aging-resistant cable. This is achieved by using an in-situ loading process to prepare a type II anhydrous calcium sulfate whisker-loaded cerium dioxide composite inorganic filler, combined with silane coupling agent modification, to solve problems such as agglomeration and weak interfacial bonding. The one-dimensional skeleton of the whiskers significantly enhances the tensile strength and dimensional stability of the material, inhibiting long-term creep; cerium dioxide plays a role in free radical scavenging and UV / thermal-oxidative shielding, comprehensively improving aging resistance and weather resistance. This achieves a synergistic improvement in mechanical, creep-resistant, and aging-resistant properties, overcoming the limitations of short service life in traditional materials. The resulting insulating material possesses high strength, low creep, resistance to damp heat and UV radiation, and stable insulation, adapting to harsh operating conditions such as high temperature and alternating loads. Simultaneously, the process is simplified, costs are reduced, and industrialization is facilitated.
[0007] To achieve the aforementioned primary objective, the present invention employs the following technical solution: a composite inorganic filler, characterized in that it is prepared according to the following steps:
[0008] α-Calcium sulfate hemihydrate whiskers, prepared by the hydrothermal method of phosphogypsum, were added to deionized water to form a suspension. Cerium nitrate hexahydrate was added at a mass ratio of α-calcium sulfate hemihydrate whiskers to cerium nitrate hexahydrate of 6.5:1-10.0:1, along with 2%-5% (by mass) of polyethylene glycol-4000. The mixture was stirred to dissolve and disperse the precipitate, obtaining a suspension system. Ammonium bicarbonate aqueous solution was slowly added dropwise to the suspension system at 15℃-22℃, controlling the final pH to 4.8-5.2. After the addition was complete, the mixture was aged for 8-12 minutes and then rapidly hot-filtered. The cerium carbonate and α-calcium sulfate hemihydrate... Calcium sulfate whisker mixed filter cake was dispersed in an aqueous solution of 0.3%-0.6% ammonium citrate. The pH of the slurry was adjusted to 7.0-7.4 with dilute ammonium bicarbonate, and the system temperature was controlled at 40℃-45℃. After stirring for 5-12 minutes, the mixture was quickly filtered. The filter cake was then rapidly washed with deionized water with pH adjusted to 7.0-7.2 by ammonium bicarbonate, and dried. The dried solid powder was spread evenly, heated to 650℃-700℃ and calcined for 40-70 minutes. The mixture was then cooled to room temperature in a dry atmosphere to obtain cerium dioxide-supported type II anhydrous calcium sulfate whisker composite inorganic filler.
[0009] The α-hemihydrate calcium sulfate whiskers used in the invention have a diameter of 1-3 μm, a length of 80-150 μm, and an aspect ratio of 40-120. The size of the whiskers can be controlled by the hydrothermal process temperature, holding time, and liquid-to-material ratio.
[0010] In the above scheme, the solid content of the α-hemihydrate calcium sulfate whisker suspension is 5%-6%.
[0011] In the above scheme: the mass concentration of ammonium bicarbonate aqueous solution is 8%-10%, the dropping rate is 0.8-1.2 mL / min, and the filter cake is dried at 100℃-110℃.
[0012] In the above scheme, the heating rate during calcination is 3.0-3.5℃ / min.
[0013] The composite inorganic filler prepared by the aforementioned method is a composite inorganic filler.
[0014] In the above scheme, the mass ratio of type II anhydrous calcium sulfate whiskers to cerium dioxide in the composite inorganic filler is 15:1-24:1.
[0015] In the above scheme: 2%-3% of the silane coupling agent γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560) is added to the composite inorganic filler, and the surface is modified by dry stirring at high speed (2000-3000r / min) to obtain the modified composite inorganic filler.
[0016] The second objective of this invention is achieved as follows: a high-strength, creep-resistant, and aging-resistant cable, comprising an insulation layer, characterized in that the insulation layer is made of the following raw materials in parts by weight:
[0017] 100 parts PVC resin; 3-10 parts of the modified composite inorganic filler; 36-42 parts plasticizer; 2.4-3.2 parts calcium stearate heat stabilizer, 0.7-1.0 parts zinc stearate heat stabilizer, 0.3-1.2 parts hydrotalcite auxiliary heat stabilizer, 0.1-0.4 parts dibenzoylmethane auxiliary heat stabilizer; 0.8-2.0 parts lubricant; 0.3-1.0 parts antioxidant; 1.5-3 parts methyl methacrylate-butyl acrylate graft copolymer processing aid.
[0018] The preparation steps are as follows: Weigh PVC resin, modified composite inorganic filler, heat stabilizer, auxiliary heat stabilizer, antioxidant, and processing aid into a high-speed mixer, stir at high speed (2000-3000 r / min) and heat to 95-110℃, then add plasticizer and lubricant, continue mixing until the temperature reaches 120-130℃ and then discharge to obtain premix; transfer the premix to a cold mixer to cool to 40-55℃, and feed it into a twin-screw extruder for extrusion granulation; set the temperature of each section of the extruder as follows: Zone 1 145-155℃, Zone 2 155-165℃, Zone 3 160-170℃, die head temperature 165-175℃, screw speed 200-350 r / min, extrusion, water cooling and pelletizing; obtain insulating granules, feed the insulating granules into a cable extruder, and extrude an insulating layer onto the conductor surface.
[0019] In the above scheme: the plasticizer is one or a combination of two of dioctyl phthalate (DOP) and trioctyl trimellitate (TOTM).
[0020] In the above scheme: the lubricant is one or both of stearic acid and polyethylene wax; the antioxidant is a compound antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dilauryl thiodipropionate in a mass ratio of 1:1.
[0021] This invention employs an in-situ precipitation-calcination process to grow cerium dioxide in situ and uniformly immobilize it on the surface of type II anhydrous calcium sulfate whiskers, avoiding agglomeration caused by adding cerium dioxide alone. Then, it is dry-modified with KH-560 silane coupling agent to introduce epoxy organic functional groups on the surface of the inorganic filler, thereby improving the interfacial bonding force between the composite filler and the PVC polymer matrix and reducing interfacial defects between the two phases.
[0022] This invention employs an in-situ precipitation-calcination process to grow cerium dioxide in situ and uniformly immobilize it on the surface of type II anhydrous calcium sulfate whiskers. The one-dimensional framework of the whiskers significantly enhances the tensile strength and dimensional stability of the material and inhibits long-term creep. Cerium dioxide plays a role in free radical scavenging and UV / thermal-oxidative shielding, comprehensively improving aging resistance and weather resistance.
[0023] Type II anhydrous calcium sulfate whiskers are one-dimensional rigid inorganic whiskers that interlock within the PVC matrix to form a rigid network structure. This effectively anchors the PVC molecular chains, inhibiting polymer chain slippage and relaxation under external forces, thereby improving the tensile strength and modulus of the material, reducing creep deformation, and enhancing the dimensional stability of the insulation layer under long-term service conditions. Cerium dioxide loaded on the whisker surface possesses excellent ultraviolet light absorption and free radical scavenging capabilities, quenching active free radicals generated during the thermo-oxidative and photo-aging processes of PVC, inhibiting the breakage and degradation of PVC molecular chains, delaying material embrittlement, and maintaining stable insulation resistance.
[0024] In the formulation system, calcium stearate and zinc stearate act as the main heat stabilizers to absorb hydrogen chloride released from PVC decomposition; hydrotalcite further adsorbs acidic small molecules, and dibenzoylmethane inhibits the "zinc burning" phenomenon, synergistically improving the thermal stability of PVC; pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dilauryl thiodipropionate are combined as antioxidants to further capture free radicals in thermo-oxidative aging; processing aids improve the plasticizing behavior of PVC and ensure that the composite material has good processing fluidity; the components work together to ultimately obtain a PVC cable insulation material that combines high strength, low creep, aging resistance, and excellent insulation performance.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) This invention uses phosphogypsum-based α-hemihydrate calcium sulfate whiskers as a precursor. Cerium dioxide is uniformly loaded onto the whisker surface through in-situ precipitation and calcination to avoid particle agglomeration. After KH-560 dry modification, the compatibility between the filler and the PVC matrix is improved, and interface defects are reduced. Type II anhydrous calcium sulfate whiskers form a rigid interwoven network in the PVC matrix, which inhibits molecular chain slippage and relaxation, improves the material strength modulus, reduces creep, and ensures the long-term dimensional stability of the insulation layer.
[0027] (2) The in-situ loaded cerium dioxide can absorb ultraviolet light, capture active free radicals, inhibit the thermal and photo-aging of PVC, delay material embrittlement, maintain stable insulation resistance, and effectively improve the service life of the cable under outdoor alternating temperature conditions.
[0028] (3) The filler utilizes phosphogypsum-derived whiskers, which reduces rare earth consumption and has a wide range of raw material sources. The whole process can be adapted to existing PVC cable material production equipment, which is convenient for industrial implementation and produces insulation materials with high strength, creep resistance, aging resistance and excellent processing and insulation properties. Detailed Implementation
[0029] The specifications of the raw materials used in the embodiments of this invention are as follows:
[0030] PVC resin: SG-5 type cable insulation grade polyvinyl chloride resin, K value 66-68;
[0031] Hydrotalcite: Magnesium aluminum hydrotalcite suitable for PVC cable insulation, with a particle size D50≤2μm, and soluble ions and heavy metal impurities meet the requirements for use in wire and cable insulation materials;
[0032] Processing aid methyl methacrylate-butyl acrylate graft copolymer (ACR): a special processing modifier for PVC cables.
[0033] The present invention will be further described in detail below through specific embodiments:
[0034] Example 1
[0035] Preparation of composite inorganic fillers:
[0036] Take α-calcium sulfate hemihydrate whiskers synthesized by hydrothermal synthesis of phosphogypsum. The α-calcium sulfate hemihydrate whiskers have a diameter of 1-3 μm, a length of 80-150 μm, and an aspect ratio of 40-120. Prepare an aqueous suspension with a solid content of 5%. Add cerium nitrate hexahydrate at a ratio of α-calcium sulfate hemihydrate whiskers to cerium nitrate hexahydrate of 7.5:1. Then add PEG-4000 at a mass of 3% of cerium nitrate hexahydrate and stir to dissolve and disperse. The system temperature was controlled at 15℃-22℃. A 9% ammonium bicarbonate aqueous solution was added dropwise at 1.0 mL / min, and the final pH was adjusted to 5.0. After aging for 10 min, the mixture was rapidly hot filtered and washed with warm water. The filter cake containing cerium carbonate and α-hemihydrate calcium sulfate whiskers was dispersed in a 0.4% ammonium citrate aqueous solution. The pH of the slurry was adjusted to 7.2 with dilute ammonium bicarbonate. The system temperature was controlled at 40℃, and the mixture was stirred for 8 min before rapid filtration. The filter cake was rapidly rinsed three times with deionized water with pH adjusted to 7.2 by ammonium bicarbonate. The filter cake was then dried promptly (at 105±5℃). The dried solid powder was spread out and heated to 680℃ at 3.2℃ / min, held at that temperature for 55min, and cooled in a dry atmosphere to obtain a type II anhydrous calcium sulfate whisker in situ supported cerium dioxide composite inorganic filler with a mass ratio of type II anhydrous calcium sulfate whisker to cerium dioxide of 18:1. 2% of the total filler mass of KH-560 was added, and the filler was dry-modified by high-speed stirring to obtain a composite modified filler.
[0037] The insulation layer is prepared by weight of the following raw materials: 100 parts of SG-5 type PVC resin, 6 parts of composite modified filler, 40 parts of TOTM plasticizer; 2.4 parts of calcium stearate, 0.8 parts of zinc stearate, 0.6 parts of hydrotalcite, 0.2 parts of dibenzoylmethane; 0.8 parts of stearic acid, 0.5 parts of polyethylene wax; 0.6 parts of a compound antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dilauryl thiodipropionate in a mass ratio of 1:1; and 2 parts of processing aid methyl methacrylate-butyl acrylate graft copolymer.
[0038] The insulation layer preparation method is as follows: PVC resin, composite modified filler, heat stabilizer, auxiliary heat stabilizer, antioxidant, and processing aid are put into a high-speed mixer, heated to 100℃, plasticizer and lubricant are added, and the mixture is discharged at 125℃; after cold mixing and cooling to 50℃, it is fed into a twin-screw extruder, with zone 1 at 145-155℃, zone 2 at 155-165℃, zone 3 at 160-170℃, die head temperature at 165-175℃, screw speed at 280r / min, and water-cooled pelletizing to obtain PVC cable insulation material granules.
[0039] The PVC cable insulation material granules obtained above are fed into a cable extruder. The extruder body temperature is 150-170℃ and the die temperature is 165-175℃. An insulation layer is extruded onto the conductor surface. After water cooling, traction, and winding, a high-strength, creep-resistant, and aging-resistant PVC cable is obtained.
[0040] Example 2
[0041] Preparation of composite inorganic fillers:
[0042] Take α-calcium sulfate hemihydrate whiskers synthesized by hydrothermal synthesis of phosphogypsum. The α-calcium sulfate hemihydrate whiskers have a diameter of 1-3 μm, a length of 80-150 μm, and an aspect ratio of 40-120. Prepare an aqueous suspension with a solid content of 6%. Add cerium nitrate hexahydrate at a ratio of α-calcium sulfate hemihydrate whiskers to cerium nitrate hexahydrate of 6.5:1. Then add PEG-4000 at a mass of 2% of cerium nitrate hexahydrate and stir to dissolve and disperse. The system temperature was controlled at 15℃-22℃. A 10% ammonium bicarbonate aqueous solution was added dropwise at 0.8 mL / min, and the final pH was adjusted to 5.2. After aging for 12 min, the mixture was rapidly hot filtered and washed with warm water. The cerium carbonate and α-hemihydrate calcium sulfate whiskers were dispersed in a 0.6% ammonium citrate aqueous solution. The pH of the slurry was adjusted to 7.0 with dilute ammonium bicarbonate. The system temperature was controlled at 45℃, and the mixture was stirred for 12 min before rapid filtration. The mixture was then rapidly rinsed three times with deionized water with a pH adjusted to 7.2 by ammonium bicarbonate. The filter cake was dried promptly (at 105±5℃). The dried solid powder was spread out and heated to 700℃ at 3.5℃ / min, held for 40 min, and cooled in a dry atmosphere to obtain a type II anhydrous calcium sulfate whisker in situ supported cerium dioxide composite inorganic filler with a mass ratio of type II anhydrous calcium sulfate whisker to cerium dioxide of 15:1. 3% of the total filler mass of KH-560 was added, and the mixture was dry-modified by high-speed stirring to obtain the composite modified filler.
[0043] PVC insulation material raw materials (by weight): SG-5-PVC resin 100 parts; composite modified filler 10 parts; TOTM plasticizer 42 parts; heat stabilizer calcium stearate 3.2 parts; heat stabilizer zinc stearate 1.0 part; hydrotalcite 1.2 parts; auxiliary heat stabilizer dibenzoylmethane 0.4 parts; stearic acid 1.0 part; antioxidant 0.8 parts (a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dilauryl thiodipropionate in a mass ratio of 1:1); processing aid (methyl methacrylate-butyl acrylate graft copolymer) 3 parts.
[0044] The preparation method is as follows: PVC resin, composite modified filler, heat stabilizer, auxiliary heat stabilizer, antioxidant, and processing aid are put into a high-speed mixer, heated to 110℃, plasticizer and lubricant are added, and the mixture is discharged at 130℃; after cold mixing and cooling to 55℃, it is fed into a twin-screw extruder, with zone 1 at 145-155℃, zone 2 at 155-165℃, zone 3 at 160-170℃, die head temperature at 165-175℃, screw speed at 200r / min, and water-cooled pelletizing to obtain PVC cable insulation material granules.
[0045] The PVC cable insulation material granules obtained above are fed into a cable extruder. The extruder body temperature is 150-170℃ and the die temperature is 165-175℃. An insulation layer is extruded onto the conductor surface. After water cooling, traction, and winding, a high-strength, creep-resistant, and aging-resistant PVC cable is obtained.
[0046] Example 3
[0047] Preparation of composite inorganic filler: The mass ratio of α-hemihydrate calcium sulfate whiskers to cerium nitrate hexahydrate is 10:1. The diameter of the α-hemihydrate calcium sulfate whiskers is 1-3μm, the length is 80-150μm, and the aspect ratio is 40-120. The other process parameters are the same as in Example 1. After calcination, the mass ratio of type II anhydrous calcium sulfate whiskers to cerium dioxide is 24:1.
[0048] PVC insulation material raw materials (by weight): SG-5-PVC resin 100 parts; composite modified filler 4 parts; plasticizer composed of DOP and TOTM in a 1:1 mass ratio 36 parts; heat stabilizer calcium stearate 2.5 parts, heat stabilizer zinc stearate 0.7 parts, hydrotalcite 0.3 parts, auxiliary heat stabilizer dibenzoylmethane 0.1 parts, polyethylene wax 2.0 parts; antioxidant composed of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dilauryl thiodipropionate in a 1:1 mass ratio 0.4 parts; processing aid methyl methacrylate-butyl acrylate graft copolymer ACR 1.5 parts.
[0049] The preparation method is as follows: PVC resin, composite modified filler, heat stabilizer, auxiliary heat stabilizer, antioxidant, and processing aid are put into a high-speed mixer, heated to 95°C, plasticizer and lubricant are added, and the mixture is discharged at 120°C; after cold mixing and cooling to 40°C, it is fed into a twin-screw extruder, with the temperature of zone 1 being 145-155°C, zone 2 being 155-165°C, zone 3 being 160-170°C, the die head temperature being 165-175°C, and the screw speed being 350 r / min. After water cooling and pelletizing, PVC cable insulation material granules are obtained.
[0050] The PVC cable insulation material granules obtained above are fed into a cable extruder. The extruder body temperature is 150-170℃ and the die temperature is 165-175℃. An insulation layer is extruded onto the conductor surface. After water cooling, traction, and winding, a high-strength, creep-resistant, and aging-resistant PVC cable is obtained.
[0051] Comparative Example 1 (Traditional physical blending process)
[0052] Compared with Example 1, the filler was replaced with an equal mass of physically blended composite filler (type II anhydrous calcium sulfate whiskers and cerium dioxide were mixed evenly at a mass ratio of 18:1), and the other raw materials and processes were the same.
[0053] The difference lies in the preparation of the physically blended composite filler: using the experimental conditions of the in-situ calcination loading process in Example 1, two inorganic fillers, type II anhydrous calcium sulfate whiskers and grade cerium dioxide powder, were prepared respectively (for type II anhydrous calcium sulfate whiskers, the method in Example 1 was followed, first preparing a 5% suspension without adding cerium nitrate hexahydrate, and then continuing with the subsequent steps. For cerium nitrate hexahydrate, water was directly added to dissolve and disperse it, and then it was prepared according to the subsequent steps). Then, the two fillers were physically stirred and mixed.
[0054] Similarly, 2% of the total mass of KH-560 was added for dry modification, and the subsequent extrusion granulation and cable preparation processes were exactly the same as in Example 1.
[0055] Comparative Example 2 (Traditional Physical Blending Process)
[0056] Compared with Example 2, the filler was replaced with an equal mass of physically blended composite filler (type II anhydrous calcium sulfate whiskers and cerium dioxide were mixed evenly at a mass ratio of 15:1), and the other raw materials and processes were the same.
[0057] The difference is that this comparative composite filler does not use the in-situ calcination loading process. Instead, it directly mixes commercial type II anhydrous calcium sulfate whiskers with cerium dioxide powder using simple physical stirring. It also uses 2% KH-560 dry modification. The subsequent extrusion granulation and cable preparation processes are exactly the same as in Example 2.
[0058] The PVC insulation materials prepared in Examples 1-3 and Comparative Examples 1 and 2 were pressed into standard samples. The following standards were applied to each performance test: Tensile strength and elongation at break: GB / T1040.1-2018; Creep rate at room temperature: GB / T11546.1-2008, test conditions: 23℃, constant stress 2MPa, loading time 100h; Ultraviolet aging test: GB / T-16422.3-2014, ultraviolet aging for 500h, testing the retention rate of tensile strength after aging; Volume resistivity: GB / T-1410-2006, test conditions 23℃. The results are shown in Table 1.
[0059] Table 1 - Comparison of performance test results of cable insulation materials prepared in the examples and comparative examples
[0060]
[0061] Table 1 shows the performance test results of the materials in each embodiment and comparative example. As can be seen from the table, Examples 1-3, which used the in-situ loading process to prepare composite fillers, showed significantly improved tensile strength, elongation at break, creep resistance, UV aging retention, and volume resistivity compared to Comparative Examples 1 and 2, which were physically blended with the same filler ratio. With increasing composite filler content, the tensile strength, creep resistance, UV aging resistance, and volume resistivity of the material gradually increased, while the elongation at break decreased slightly. Specifically, Example 2 showed a tensile strength of 24.1 MPa, a creep rate as low as 3.5% after 100 hours, and a strength retention rate of 91.1% after 500 hours of UV aging; Example 3 showed an elongation at break of 351%, demonstrating excellent material flexibility. The in-situ loading process uniformly loaded cerium dioxide onto the surface of calcium sulfate whiskers, inhibiting cerium dioxide agglomeration and improving the interfacial bonding between the filler and the matrix. While ensuring high toughness, it significantly improved the mechanical strength, creep resistance, dimensional stability, and UV aging resistance of PVC insulation materials.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention, as long as they do not depart from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A composite inorganic filler, characterized in that, Prepare according to the following steps: α-Calcium sulfate hemihydrate whiskers, prepared by the hydrothermal method of phosphogypsum, were added to deionized water to form a suspension. Cerium nitrate hexahydrate was added at a mass ratio of α-calcium sulfate hemihydrate whiskers to cerium nitrate hexahydrate of 6.5:1-10.0:1, along with 2%-5% (by mass) of polyethylene glycol-4000. The mixture was stirred to dissolve and disperse the precipitate, obtaining a suspension system. Ammonium bicarbonate aqueous solution was slowly added dropwise to the suspension system at 15℃-22℃, controlling the final pH to 4.8-5.
2. After the addition was complete, the mixture was aged and then rapidly hot-filtered. The cerium carbonate and α-calcium sulfate hemihydrate... Calcium sulfate whisker mixed filter cake was dispersed in an aqueous solution of ammonium citrate with a mass concentration of 0.3%-0.6%. The pH of the slurry was adjusted to 7.0-7.4 using dilute ammonium bicarbonate, and the system temperature was controlled at 40℃-45℃. After stirring, the mixture was quickly filtered. The filter cake was then rapidly washed with deionized water with a pH adjusted to 7.0-7.2 using ammonium bicarbonate, and dried. The dried solid powder was spread evenly, heated to 650℃-700℃ and calcined, held at that temperature for 40-70 minutes, and then cooled to room temperature in a dry atmosphere to obtain cerium dioxide-supported type II anhydrous calcium sulfate whisker composite inorganic filler.
2. The composite inorganic filler according to claim 1, characterized in that: The solid content of the α-hemihydrate calcium sulfate whisker suspension is 5%-6%.
3. The composite inorganic filler according to claim 1 or 2, characterized in that: The ammonium bicarbonate aqueous solution has a mass concentration of 8%-10%, a dropping rate of 0.8-1.2 mL / min, and the filter cake is dried at 100℃-110℃.
4. The composite inorganic filler according to claim 3, characterized in that: The heating rate during calcination is 3.0-3.5℃ / min.
5. The composite inorganic filler according to claim 4, characterized in that: The mass ratio of type II anhydrous calcium sulfate whiskers to cerium dioxide in the composite inorganic filler is 15:1-24:
1.
6. The composite inorganic filler according to claim 5, characterized in that: The modified composite inorganic filler is obtained by adding 2%-3% of the silane coupling agent γ-(2,3-epoxypropoxy)propyltrimethoxysilane to the composite inorganic filler and then performing surface modification by high-speed stirring and dry method.
7. A high-strength, creep-resistant, and aging-resistant cable, comprising an insulation layer, characterized in that, The insulating layer is made of the following raw materials in parts by weight: 100 parts of PVC resin; 3-10 parts of the modified composite inorganic filler as described in claim 6; 36-42 parts of plasticizer; 2.4-3.2 parts of heat stabilizer calcium stearate; 0.7-1.0 parts of heat stabilizer zinc stearate; 0.3-1.2 parts of auxiliary heat stabilizer hydrotalcite; 0.1-0.4 parts of auxiliary heat stabilizer dibenzoylmethane; 0.8-2.0 parts of lubricant; 0.3-1.0 parts of antioxidant; 1.5-3 parts of processing aid methyl methacrylate-butyl acrylate graft copolymer. The preparation steps are as follows: Weigh PVC resin, modified composite inorganic filler, heat stabilizer, auxiliary heat stabilizer, antioxidant, and processing aids into a high-speed mixer, stir at high speed and heat to 95-110℃, then add plasticizer and lubricant, continue mixing until the temperature reaches 120-130℃, and then discharge to obtain a premix; transfer the premix to a cold mixer to cool to 40-55℃, and then feed it into a twin-screw extruder for granulation; the temperature settings for each section of the extruder are: Zone 1 145-155℃, Zone 2 155-165℃, Zone 3 160-170℃, and the die head... The process involves extrusion at 165-175℃ and screw speed at 200-350 r / min, followed by water cooling and pelletizing to obtain insulating granules. These granules are then fed into a cable extruder to extrude an insulating layer onto the conductor surface. The plasticizer is one or a combination of dioctyl phthalate and trioctyl trimellitate. The lubricant is one or a combination of stearic acid and polyethylene wax. The antioxidant is a compound antioxidant consisting of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dilauryl thiodipropionate in a mass ratio of 1:1.