Polymerization of pyrrole on molybdenum disulfide nanotubes and preparation method and application thereof
By using a core-shell structured PPy@MoS2 nanotube composite adsorbent material, the problem of easy stacking of MoS2 nanosheets on the PPy framework is solved, achieving a stable and regular tubular framework and high-efficiency adsorption performance, which is suitable for wastewater treatment and biomedical fields.
Patent Information
- Application Number
- CN202611237410.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing PPy@MoS2 nanotube composite adsorbent materials have shortcomings in the construction and maintenance of nanotube morphology. MoS2 nanosheets tend to form stacks between layers on the PPy framework, resulting in irregular morphology and affecting their application efficiency.
A core-shell structured PPy@MoS2 nanotube composite adsorbent material is used, with PPy microtubes as the core layer and MoS2 nanosheets arranged perpendicularly along the PPy microtube axis as the shell layer. By controlling the temperature of the in-situ polymerization reaction and the hydrothermal vulcanization process, the tubular framework is stabilized and the stacking of MoS2 nanosheets is avoided.
It achieves a stable and regular tubular framework morphology, improves specific surface area and surface charge, and has excellent adsorption performance. It is suitable for wastewater treatment and biomedical fields, and exhibits high adsorption capacity and reusability.
Smart Images

Figure CN123059622A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nanocomposite adsorbent materials and their preparation methods, and particularly relates to a PPy@MoS2 nanotube composite adsorbent material, its preparation method, and its application. Background Technology
[0002] Molybdenum disulfide (MoS2), a typical transition metal chalcogenide, has attracted widespread attention in the adsorption field due to its high theoretical specific surface area, abundant edge active sites, and tunable electronic structure. However, MoS2 still suffers from problems such as poor conductivity of the semiconductor 2H phase and irreversible stacking and aggregation caused by interlayer van der Waals forces, which reduce active sites and hinder mass transfer. Compositing with conductive polymers is considered an effective strategy to improve its structural stability and surface functionalization.
[0003] Polypyrrole (PPy), as a π-conjugated conductive polymer, has become a promising component in composite materials due to its good environmental stability, simple synthesis, and the ability of its nitrogen-containing surface groups (–NH–, =N–) to complex metal ions or biomolecules. PPy tends to aggregate without MoS2 support, and existing PPy / MoS2 composite systems still have significant shortcomings: MoS2 nanosheets easily form stacks between layers on the PPy framework, and the composite materials generally suffer from irregular morphology and insufficient surface charge regulation, severely restricting their efficient application.
[0004] Although tubular MoS2 structures possess advantages such as high aspect ratio, open diffusion channels, and resistance to stacking, traditional vulcanization methods are prone to morphological degradation due to volume changes and uncontrollable phase transitions. When the MoO3 precursor transforms into MoS2, it undergoes volume changes and lattice rearrangement, causing the original structure to collapse or fracture. While polymer layers can modulate surface properties, simultaneously maintaining morphology remains a significant technical challenge.
[0005] In summary, existing PPy@MoS2 nanotube composite adsorbent materials have significant shortcomings in the construction and maintenance of nanotube morphology. Therefore, this paper presents a PPy@MoS2 nanotube composite adsorbent material that can achieve both nanotube morphology construction and maintenance, and avoids the tendency for MoS2 nanosheets to stack between layers on the PPy framework, effectively overcoming the common problem of irregular morphology in composite materials. Summary of the Invention
[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide a PPy@MoS2 nanotube composite adsorption material, which realizes the construction and maintenance of nanotube morphology, and avoids the easy formation of stacking between layers of MoS2 nanosheets on the PPy framework, effectively overcoming the problem of irregular morphology that is common in composite materials.
[0007] Technical solution: The PPy@MoS₂ nanotube composite adsorption material of the present invention has a core-shell one-dimensional hierarchical nanotubular structure, wherein the core layer is a PPy microtube, and the shell layer is composed of MoS₂ nanosheets arranged perpendicularly to the axial direction of the PPy microtube and attached to the surface of the PPy microtube.
[0008] The method for preparing the above-mentioned PPy@MoS₂ nanotube composite adsorption material of the present invention comprises the following steps:
[0009] (1) Dissolving a molybdenum source in water, adding an acid solution, and carrying out a hydrothermal reaction to obtain MoO₃ nanorods;
[0010] (2) Dispersing the MoO₃ nanorods in water, adding pyrrole monomer, and carrying out a hydrothermal reaction at a temperature of 120≤T≤200°C for 6-24 h to obtain MoO 3-x @PPy precursor, wherein 0≤x≤1;
[0011] (3) Mixing the precursor with a sulfur source, and carrying out a hydrothermal vulcanization reaction to obtain the PPy@MoS₂ nanotube composite adsorption material.
[0012] Further, in step (2) of the preparation method of the present invention, when the hydrothermal reaction temperature is 120≤T≤140°C, the precursor is MoO₃@PPy.
[0013] Further, in step (2) of the preparation method of the present invention, when the hydrothermal reaction temperature is 140<T<160°C, the precursor is a mixed phase composed of MoO 3-x @PPy, MoO₃@PPy and MoO₂@PPy; wherein o<x<1.
[0014] Further, in step (2) of the preparation method of the present invention, when the hydrothermal reaction temperature is 160≤T≤200°C, the precursor is MoO₂@PPy.
[0015] Further, in step (1) of the preparation method of the present invention, the solid-to-liquid ratio of the molybdenum source to the acid solution is 1 g:(1.8-5) mL, the molybdenum source is selected from one of ammonium heptamolybdate tetrahydrate, sodium molybdate dihydrate or molybdenum oxide, and the acid solution is selected from one of nitric acid, hydrochloric acid or sulfuric acid.
[0016] Further, in step (2) of the preparation method of the present invention, the usage ratio of the MoO₃ nanorods to the pyrrole monomer is 0.1 g:(0.1-0.5) mL.
[0017] Further, in step (3) of the preparation method of the present invention, the mass ratio of the precursor to the sulfur source is 1:(4-20), and the sulfur source is selected from one of thiourea, thioacetamide or sodium sulfide.
[0018] Furthermore, in step (1) of the preparation method of the present invention, the temperature of the hydrothermal reaction is 160-200℃ and the reaction time is 12-30 h; in step (3), the temperature of the hydrothermal sulfidation reaction is 180-220℃ and the reaction time is 16-36 h.
[0019] The PPy@MoS2 nanotube composite adsorbent material of the present invention is applied to the removal of cationic dyes in wastewater treatment.
[0020] The PPy@MoS2 nanotube composite adsorbent material described above is applied to the adsorption of lysozyme.
[0021] Beneficial effects: Compared with the prior art, the significant advantages of the present invention are:
[0022] (1) The PPy@MoS2 nanotube composite adsorbent material has a core-shell one-dimensional hierarchical nanotube structure. The core layer is PPy microtubes, and the shell layer consists of MoS2 nanosheets arranged perpendicularly to the PPy microtube axis and attached to the surface of the PPy microtubes, exhibiting a stable and regular tubular framework morphology. The specific surface area of this composite adsorbent material is 28.9978-200.4127 m². 2 / g, the Zeta potential is (-21.13 mV) - (-40.27 mV).
[0023] (2) The preparation method uses MoO3 nanorods as morphology guiding templates and utilizes the in-situ polymerized PPy layer to stabilize the tubular framework throughout the phase transformation and vulcanization process. By controlling the synthesis temperature of the in-situ polymerization reaction, it not only effectively overcomes the morphology degradation problem caused by volume change and uncontrollable phase transformation in the traditional vulcanization method, but also solves the technical problem of irregular morphology and random aggregation of the existing PPy / MoS2 system.
[0024] (3) This preparation process simultaneously improves the specific surface area and surface charge of the nanotube composite adsorbent material, achieving synchronous and precise control of nanotube morphology and surface charge, and obtaining a series of adsorbent materials with differentiated adsorption properties. This can meet the different requirements of different adsorbents for adsorbent morphology and surface properties. The most representative manifestation is:
[0025] 3.1) At an in-situ polymerization temperature of 120-140℃, the obtained PPy@MoS2 nanotube composite adsorbent material has a high surface negative charge (the highest Zeta potential is -40.27 mV) and exhibits excellent adsorption performance for the cationic dye methylene blue, with a maximum adsorption capacity of 148.66 mg / g, which is significantly better than existing MoS2 supported nanofiber membranes (77.7 mg / g), MoS2 / ZIF-8 (88.03 mg / g) and mixed-phase MoO3 nanostructures (141.2 mg / g).
[0026] 3.2) The PPy@MoS2 nanotube composite adsorbent material synthesized at an in-situ polymerization temperature of 160-200℃ exhibits a high specific surface area (up to 200.41 m²). 2 With its abundant mesoporous and macroporous structure, it has a maximum adsorption capacity of 63.77 mg / g for protein lysozyme, which is far superior to materials such as BEA-OH-50 (11.8 mg / g), Fe3O4@SiO2 (20.0 mg / g), and PI / HAP mixed matrix membrane (34 mg / g), providing a new and highly efficient adsorption material for protein separation and purification.
[0027] Furthermore, the obtained PPy@MoS2 nanotube composite adsorbent material conforms to both the Langmuir isotherm model and the pseudo-second-order kinetic model during the adsorption process, indicating that the adsorption is a monolayer chemisorption controlled process on a uniform surface. It can be directly used for the removal of cationic dyes in wastewater treatment and the separation and purification of lysozyme in the biopharmaceutical field.
[0028] Furthermore, the material maintains stable adsorption performance after five adsorption-elution cycles, demonstrating good reusability. Attached Figure Description
[0029] Figure 1 This is a schematic diagram illustrating the preparation mechanism of the PPy@MoS2 nanotube composite adsorption material of the present invention.
[0030] Figure 2 X-ray diffraction (XRD) patterns of the precursors and PPy@MoS2 prepared in Examples 1 to 4; wherein: (a) precursor, (b) PPy@MoS2;
[0031] Figure 3 The X-ray diffraction (XRD) pattern of the precursor prepared in Example 5;
[0032] Figure 4 The X-ray photoelectron spectroscopy (XPS) spectra of the PPy@MoS2 nanotube composite adsorbent material prepared in Example 1 are shown below; where: (a) full spectrum, (b) C 1s spectrum, (c) N 1s spectrum, (d) O 1s spectrum, (e) Mo 3d spectrum, and (f) S 2p spectrum.
[0033] Figure 5 SEM images of the precursors prepared in Examples 1 to 4; wherein: (a) MoO3@PPy (120℃), (b) MoO3@PPy (140℃), (c) MoO2@PPy (160℃), (d) MoO2@PPy (200℃);
[0034] Figure 6SEM images of the PPy@MoS2 nanotube composite adsorbent materials prepared in Examples 1 to 4; where: (a) PPy@MoS2 (120℃), (b) PPy@MoS2 (140℃), (c) PPy@MoS2 (160℃), (d) PPy@MoS2 (200℃);
[0035] Figure 7 The image shows the SEM image of the precursor prepared in Example 5; where (a) is 2 μm and (b) is 500 nm.
[0036] Figure 8 SEM images of the PPy@MoS2 nanotube composite adsorbent material prepared in Example 5; where (a) is 2 μm and (b) is 500 nm.
[0037] Figure 9 The N2 adsorption-desorption isotherms and pore size distribution curves of the PPy@MoS2 nanotube composite adsorbent materials prepared in Examples 1 to 4 are shown; where (a) is the N2 adsorption-desorption isotherm; and (b) is the pore size distribution curve.
[0038] Figure 10 The zeta potential diagrams are for the PPy@MoS2 nanotube composite adsorbent materials prepared in Examples 1 to 4.
[0039] Figure 11 The diagram shows the adsorption and elution of methylene blue and lysozyme by the nanotube composite adsorbent material prepared in the example.
[0040] Figure 12 The graphs show the adsorption performance of the PPy@MoS2 nanotube composite adsorbent materials prepared in Examples 1 to 5 for methylene blue and lysozyme; wherein, (a) is a comparison graph of the adsorption performance of different PPy@MoS2 samples for MB in Examples 1 to 5; and (b) is a comparison graph of the adsorption performance of different PPy@MoS2 samples for lysozyme in Examples 1 to 5.
[0041] Figure 13 The images show the adsorption isotherm fitting and model fitting diagram of the PPy@MoS2 nanotube composite adsorbent material prepared in Example 1 for methylene blue; where: (a) adsorption isotherm, (b) Langmuir model, (c) Freundlich model, and (d) Temkin model.
[0042] Figure 14 The image shows the adsorption kinetics of methylene blue by the PPy@MoS2 nanotube composite adsorbent material prepared in Example 1; where: (a) kinetic adsorption of PPy@MoS2 (120℃), (b) pseudo-first-order kinetic curve of MB adsorption, and (c) pseudo-second-order kinetic curve of MB adsorption.
[0043] Figure 15 The images show the adsorption isotherm fitting and model fitting diagram of the PPy@MoS2 nanotube composite adsorbent material prepared in Example 4 for lysozyme; where: (a) adsorption isotherm, (b) Langmuir model, (c) Freundlich model, (d) Temkin model.
[0044] Figure 16 The image shows the kinetics of lysozyme adsorption on the PPy@MoS2 nanotube composite adsorbent material prepared in Example 4; where: (a) kinetic adsorption of PPy@MoS2 (200℃), (b) pseudo-first-order kinetic curve of MB adsorption, and (c) pseudo-second-order kinetic curve of MB adsorption.
[0045] Figure 17 The change in the adsorption capacity of lysozyme by the PPy@MoS2 nanotube composite adsorbent material prepared in Example 4 after 5 adsorption-desorption cycles is shown. Detailed Implementation
[0046] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0047] It should be noted that all raw materials used in this invention are commercially available.
[0048] The preparation process of the PPy@MoS2 nanotube composite adsorbent material of this invention is shown in the flowchart below. Figure 1 As shown, it includes the following steps:
[0049] (1) MoO3 nanorods were obtained by dissolving molybdenum source in water, adding acid solution, and undergoing hydrothermal reaction.
[0050] (2) MoO3 nanorods were dispersed in water, pyrrole monomer was added, and the mixture was subjected to a hydrothermal reaction at 120≤T≤200℃ for 6-24 h to obtain MoO3 nanorods. 3-x @PPy precursor, where 0≤x≤1;
[0051] (3) The precursor is mixed with the sulfur source and subjected to hydrothermal sulfidation reaction to obtain PPy@MoS2 nanotube composite adsorbent material.
[0052] The structure and properties of the composite material of the present invention are characterized and verified based on specific preparation examples and application cases.
[0053] Example 1
[0054] The composite material of Example 1 was prepared by the following steps:
[0055] (1) Preparation of MoO3 nanorods: 1 g of ammonium heptamolybdate tetrahydrate was dissolved in 20 mL of deionized water, and 5 mL of 65% nitric acid was added. The mixture was sonicated for 5 min until the solution was evenly dispersed. The resulting mixed solution was transferred to the lining of a 50 mL hydrothermal reactor and placed in a forced-air drying oven. The reaction was carried out at 180 °C for 20 h. After naturally cooling to room temperature, the product was centrifuged and washed three times each with deionized water and anhydrous ethanol. The product was then dried at 60 °C for 12 h to obtain white MoO3 powder.
[0056] (2) Preparation of precursor: Take 0.1 g of MoO3 powder and add it to 30 mL of deionized water. Slowly sonicate to disperse it evenly. Add 0.18 mL of pyrrole monomer to the white dispersion and stir for 15 min. Transfer the mixed solution to a 50 mL hydrothermal reactor and react hydrothermally at 120 °C for 12 h. After the reaction is complete, filter the black product, wash it three times each with deionized water and anhydrous ethanol, and dry it at 60 °C for 12 h to obtain black precursor powder.
[0057] (3) Preparation of composite material: 0.3425 g of thiourea was dissolved in 30 mL of deionized water as the sulfur source. 50 mg of precursor powder was added to the sulfur source solution and sonicated for 5 min. The mixed solution was transferred to a hydrothermal reactor and reacted at 200 °C for 24 h. After the reaction, the mixture was centrifuged, washed three times each with deionized water and anhydrous ethanol, and dried at 60 °C for 12 h to obtain the composite adsorbent material.
[0058] Example 2
[0059] The preparation method of Example 2 is basically the same as that of Example 1, except that the hydrothermal temperature in step (2) is 140°C when preparing the precursor.
[0060] Example 3
[0061] The preparation method of Example 3 is basically the same as that of Example 1, except that the hydrothermal temperature in step (2) is 160°C when preparing the precursor.
[0062] Example 4
[0063] The preparation method of Example 4 is basically the same as that of Example 1, except that the hydrothermal temperature in step (2) is 200°C when preparing the precursor.
[0064] Example 5
[0065] The preparation method of Example 5 is basically the same as that of Example 1, except that the hydrothermal temperature in step (2) is 150°C when preparing the precursor.
[0066] Performance Test 1 - Structural Characterization
[0067] 1. Characterization of phase composition
[0068] An X-ray diffractometer (XRD) was used to characterize the phase composition of the precursors prepared in step (2) of Example 1 to Example 4 and the finally prepared composite materials, and the obtained results are shown in Figure 2 .
[0069] It can be seen from Figure 2 (a) that the precursors synthesized at 120°C and 140°C retain the characteristic diffraction peaks of MoO3, which are MoO3@PPy precursors. Under the conditions of 120°C and 140°C, the relative crystallinity at 140°C is higher. When the temperature rises to 160°C and 200°C, the precursors are MoO2@PPy precursors. Under the hydrothermal condition of 150°C, both the MoO3 phase and the MoO2 phase exist, and there are also miscellaneous peak phases, which is the phase transition transition period. As shown in Figure 3 , the precursor is a mixed phase, that is, the precursor is a mixed phase composed of MoO 3-x @PPy, MoO3@PPy and MoO2@PPy; where 0<x<1. Combined with Figure 2 (b), no diffraction peaks of the MoO3 phase are detected in the XRD patterns of all samples after vulcanization, which confirms that the precursors have been completely converted into MoS2, which is PPy@MoS2.
[0070] 2. Element and valence state analysis of PPy@MoS2 nanotube composite adsorbent material
[0071] An X-ray photoelectron spectrometer (XPS) was used to analyze the elemental composition and chemical valence states of PPy@MoS2 (120°C), PPy@MoS2 (140°C), PPy@MoS2 (160°C) and PPy@MoS2 (200°C) prepared in Example 1 to Example 4. The obtained results are shown in Figure 4 .
[0072] As shown in Figure 4As shown, the full spectrum reveals characteristic peaks for C 1s, N 1s, O 1s, Mo 3d, and S 2p, confirming the coexistence of Mo, S, C, N, and O elements in the composite adsorbent material. The high-resolution C 1s spectrum shows three peaks at 284.8, 285.4, and 287.5 eV, corresponding to C-β and CC in the pyrrole ring and CN in the polypyrrole backbone, respectively. The peak at 394.75 eV in the N 1s spectrum is attributed to the Mo-N bond (acting as a bridging bond between the MoS2 nanosheets and the PPy coating), while the peaks at 399.75 eV and 397.2 eV correspond to pyrrole nitrogen and pyridine nitrogen, respectively. Two main peaks are observed in the Mo 3d region at 232.04 eV and 228.92 eV, corresponding to Mo in the MoS2 shell. 4+ Mo 3d 3 / 2 and Mo 3d 5 / 2 The S 2p spectrum shows two peaks at 163.05 eV and 162.80 eV, originating from S 2p. 1 / 2 and S 2p 3 / 2 Spin-orbit splitting.
[0073] Performance Testing 2 - Morphological Characterization
[0074] The morphology of the precursors prepared in Examples 1 to 5 and the PPy@MoS2 nanotube composites after sulfurization was observed using scanning electron microscopy (SEM). The results are as follows: Figures 5 to 8 As shown.
[0075] like Figure 5 As shown, the precursor of Example 1 is as follows Figure 5 (a) The precursor of Example 2 is as follows Figure 5 (b) The precursor of Example 3 is as follows Figure 5 (c) The precursor of Example 4, such as Figure 5 As shown in (d), the precursor of Example 5 is as follows Figure 7 As shown, the precursor surface is relatively smooth. Furthermore, during the preparation of the precursor, as the hydrothermal synthesis temperature increases, the precursor surface gradually changes from relatively smooth (120℃) to having a small amount of particles precipitated (140℃), then to a large amount of particles precipitated (150℃, 160℃), until the surface is almost completely covered (200℃).
[0076] like Figure 6 and Figure 8 As shown, after vulcanization, all five PPy@MoS2 composite materials retained the uniform microrod morphology of the precursor, with layered MoS2 nanosheets arranged vertically on their rough surfaces. Furthermore, the density of the MoS2 nanosheets gradually increased with the increase of the precursor synthesis temperature.
[0077] Performance Test 3 -- Specific Surface Area
[0078] The specific surface area and pore structure of PPy@MoS2 (120℃), PPy@MoS2 (140℃), PPy@MoS2 (160℃), and PPy@MoS2 (200℃) prepared in Examples 1 to 4 were determined using a specific surface area and porosity analyzer via N2 adsorption-desorption isotherms. The results are as follows: Figure 9 As shown.
[0079] like Figure 9 As shown in (a), the N2 adsorption-desorption isotherms of PPy@MoS2 (120℃), PPy@MoS2 (140℃), PPy@MoS2 (160℃), and PPy@MoS2 (200℃) prepared in Examples 1 to 4 are all type II isotherms. An H3 type hysteresis loop appears at P / P0≈0.6, indicating the coexistence of mesoporous structures. The sharp increase at high P / P0 indicates the presence of macropores on the material surface.
[0080] like Figure 9 (b) shows the BET (m) values of PPy@MoS2 (120℃), PPy@MoS2 (140℃), PPy@MoS2 (160℃), and PPy@MoS2 (200℃) prepared in Examples 1 to 4. 2 The specific surface area ( / g) was further calculated to be 28.9978, 32.1711, 86.2275, and 200.4127, respectively, and the micropore volume (cm³) was also calculated. 3 The values ( / g) were 0.0051, 0.0053, 0.0153 and 0.022, respectively.
[0081] Performance testing 4 -- Surface charge
[0082] The surface charges of PPy@MoS2 (120℃), PPy@MoS2 (140℃), PPy@MoS2 (160℃), and PPy@MoS2 (200℃) prepared in Examples 1 to 4 were measured using a Zeta potential analyzer at 25℃. The results are as follows: Figure 10 As shown.
[0083] Depend on Figure 10 It can be seen that PPy@MoS2 (120℃) has the highest surface negative charge, with a Zeta potential of -40.27 mV; the Zeta potentials of PPy@MoS2 (140℃), PPy@MoS2 (160℃) and PPy@MoS2 (200℃) are -36.53 mV, -31.77 mV and -21.13 mV, respectively.
[0084] Application Case 1: Adsorption of Cationic Dyes
[0085] The PPy@MoS2 nanotube composite materials prepared in Examples 1 to 5 were applied to the adsorption of methylene blue (MB) cationic dye, as follows: Figure 11 As shown, the specific application method is as follows:
[0086] Take 1 mg each of PPy@MoS2 (120℃), PPy@MoS2 (140℃), PPy@MoS2 (150℃), PPy@MoS2 (160℃), and PPy@MoS2 (200℃) prepared in Examples 1 to 5 respectively; add them to 10 ml of methylene blue (MB) solution with a concentration of 10 mg / L, and shake on a constant temperature shaker at room temperature for 2 h.
[0087] Performance Testing 5 – Cationic Dye Adsorption Performance Test
[0088] After oscillation in Application Case 1, a sample was taken, and the absorbance was measured at a wavelength of 664 nm using a UV-Vis spectrophotometer. For example... Figure 12 As shown in (a), among the five materials, PPy@MoS2 (120℃) prepared in Example 1 showed the highest adsorption capacity for MB, with a saturated adsorption capacity of 148.66 mg / g for MB.
[0089] Using PPy@MoS2 (120℃) prepared in Example 1 as the adsorbent, 100 ml of a 200 mg / L methylene blue solution was prepared by first mixing 20 mg of methylene blue with 100 ml of pure water. The initial concentration of the MB solution was then varied systematically, ranging from 1 to 20 mg / L. Specifically, 10 ml of each of the 3, 6, 9, 12, 14, 16, 18, and 20 mg / L methylene blue solutions were diluted with pure water, and the equilibrium adsorption capacity was measured. The experimental data were fitted using the Langmuir isotherm model, the Freundlich isotherm model, and the Temkin isotherm model, respectively. The results are shown below. Figure 13 As shown.
[0090] Figure 13 In the figure, (a) shows a typical Type I isotherm, and the PPy@MoS2 (120℃) adsorbent conforms to the Langmuir monolayer adsorption characteristics: sufficient adsorption sites at low concentrations, rapid adsorption; adsorption sites are gradually filled, approaching saturation adsorption capacity; (b) shows the R of the Langmuir model. 2 The values were significantly higher than those of the (c) Freundlich and (d) Temkin models, indicating that the adsorption of MB on the PPy@MoS2 composite follows a uniform monolayer adsorption mechanism. The adsorption amount of MB on PPy@MoS2 (120℃) was monitored every 10 min at room temperature. The experimental data were fitted using pseudo-first-order and pseudo-second-order kinetic models, respectively. Figure 14 As shown. R of the pseudo-second-order dynamic model. 2 A value closer to 1 indicates that the adsorption process is rate-limited.
[0091] Application Case 2: Lysozyme Adsorption Application
[0092] The application of the PPy@MoS2 nanotube composite materials prepared in Examples 1 to 5 above in lysozyme adsorption is illustrated in the flowchart below. Figure 11 As shown, the specific application method is as follows:
[0093] Take 5 mg each of PPy@MoS2 (120℃), PPy@MoS2 (140℃), PPy@MoS2 (150℃), PPy@MoS2 (160℃), and PPy@MoS2 (200℃) prepared in Examples 1 to 5; add them to 5 ml of lysozyme solution with a concentration of 0.3 mg / mL (prepared with phosphate buffer at pH=7.4), and shake on a constant temperature shaker at room temperature for 2 h.
[0094] Performance Testing 6 – Lysozyme Adsorption Performance Test
[0095] After oscillation in Application Case 2, a sample was taken, and the absorbance was measured at a wavelength of 280 nm using a UV-Vis spectrophotometer. For example... Figure 12 As shown in (b), among the five materials, PPy@MoS2 (200℃) prepared in Example 4 showed the best adsorption performance for lysozyme, with a saturated adsorption capacity of 63.77 mg / g for lysozyme.
[0096] Using PPPy@MoS2 (200℃) prepared in Example 4 as the adsorbent, 100 ml of a 1 mg / mL lysozyme solution was prepared by first taking 100 mg of lysozyme and 100 ml of phosphate buffer. The initial concentration of the lysozyme solution was systematically changed to a range of 0.3-0.8 mg / mL. Specifically, 5 ml of each of the lysozyme solutions with phosphate buffer were added to prepare concentrations of 0.3 mg / mL, 0.35 mg / mL, 0.4 mg / mL, 0.45 mg / mL, 0.5 mg / mL, 0.55 mg / mL, 0.6 mg / mL, 0.65 mg / mL, 0.7 mg / mL, 0.75 mg / mL, and 0.8 mg / mL. The equilibrium adsorption capacity was then measured. The experimental data were fitted using the Langmuir isotherm model, the Freundlich isotherm model, and the Temkin isotherm model, respectively.
[0097] like Figure 15As shown, (a) is a typical Type I isotherm, and the PPy@MoS2 (200℃) adsorbent conforms to the Langmuir monolayer adsorption characteristics: sufficient adsorption sites at low concentrations, rapid adsorption; adsorption sites are gradually filled, approaching saturation adsorption capacity; (b) R of the Langmuir model. 2 The value is significantly higher than that of the (c) Freundlich and (d) Temkin models, indicating that the adsorption of lysozyme on the PPy@MoS2 composite follows a uniform monolayer adsorption mechanism.
[0098] At room temperature, the adsorption capacity of lysozyme by PPy@MoS2 (200℃) was monitored every 10 min. The experimental data were fitted using pseudo-first-order and pseudo-second-order kinetic models, respectively. Figure 16 As shown, the R of the pseudo-second-order dynamic model 2 A value closer to 1 indicates that the adsorption process is rate-limited.
[0099] The above experiments show that the adsorption mechanisms of different adsorbates on the PPy@MoS2 composite material are as follows: For small molecule cationic dyes (MB), the surface charge is the key factor that determines the adsorption capacity, and electrostatic attraction is the main driving force. Therefore, the composite adsorption materials obtained in Examples 1 and 2 have excellent effects in the adsorption of small molecule cationic dyes. The main driving force for adsorption is electrostatic attraction, supplemented by π-π stacking and chemical bonding.
[0100] For large protein molecules (lysozyme), specific surface area is the key factor determining adsorption capacity. Therefore, the composite adsorbent materials obtained in Examples 3 and 4 have better adsorption performance for lysozyme.
[0101] Performance Testing 7 - Adsorption Cycle Performance Test
[0102] Take 5 mg of the PPy@MoS2 (200℃) composite material prepared in Example 4 and add 5 mL of lysozyme solution (0.8 mg·mL). -1 After reaching adsorption equilibrium, the adsorbent is separated using 1 mol·L⁻¹ -1 Washing with NaCl solution, the process is as follows: Figure 11 As shown, the next protein adsorption cycle is then performed, and the results are as follows. Figure 17 As shown, after five consecutive adsorption-elution cycles, the difference in adsorption capacity between the fifth and first cycles is negligible, and the material still exhibits good adsorption performance.
[0103] This study chose lysozyme as the model adsorbate for the cycling test because protein desorption involves multiple interactions and is a technical challenge in the field; while dye desorption mainly relies on electrostatic interactions, and its stability cycling test is far less demanding than that of protein cycling tests. Therefore, achieving five stable cycles in a protein system is sufficient to demonstrate the structural stability and reusability of the material.
[0104] In summary, this invention not only enables the fabrication of stable, regular tubular framework PPy@MoS2 composite adsorbent materials, solving the technical challenge of irregular morphology and random aggregation in existing PPy / MoS2 systems, but also achieves simultaneous and precise control of nanotube morphology and surface charge, resulting in a series of adsorbent materials with differentiated adsorption properties. These materials can meet the varying requirements of different adsorbent targets regarding adsorbent morphology and surface properties. Furthermore, after multiple adsorption-elution cycles, the material maintains stable adsorption performance, demonstrating excellent reusability.
[0105] In addition to the above embodiments, the technical effects claimed by the present invention can be achieved by using the PPy@MoS2 composite material, its preparation method, and the parameter range defined in its application. Therefore, no further examples will be provided to support these claims.
Claims
1. A PPy@MoS2 nanotube composite adsorbent material, characterized in that, The composite adsorbent material is a one-dimensional hierarchical nanotube structure with a core and a shell. The core layer is PPy microtubes, and the shell layer is composed of MoS2 nanosheets that are arranged perpendicularly to the PPy microtube axis and attached to the surface of the PPy microtubes.
2. A method for preparing the PPy@MoS2 nanotube composite adsorbent material according to claim 1, characterized in that, Includes the following steps: (1) MoO3 nanorods were obtained by dissolving molybdenum source in water, adding acid solution, and undergoing hydrothermal reaction. (2) MoO3 nanorods were dispersed in water, pyrrole monomer was added, and the mixture was subjected to a hydrothermal reaction at 120≤T≤200℃ for 6-24 h to obtain MoO3 nanorods. 3-x @PPy precursor, where 0≤x≤1; (3) The precursor is mixed with the sulfur source and subjected to hydrothermal sulfidation reaction to obtain PPy@MoS2 nanotube composite adsorbent material.
3. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (2), when the hydrothermal reaction temperature is 120≤T≤140℃, the precursor is MoO3@PPy.
4. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (2), when the hydrothermal reaction temperature satisfies 140<T<160°C, the precursor is composed of MoO 3-x @PPy, MoO3@PPy and MoO2@PPy; where 0<x<1.
5. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (2), when the hydrothermal reaction temperature is 160≤T≤200℃, the precursor is MoO2@PPy.
6. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (1), the solid-liquid ratio of the molybdenum source to the acid solution is 1 g: (1.8-5) mL. The molybdenum source is selected from one of ammonium heptamolybdate tetrahydrate, sodium molybdate dihydrate, or molybdenum oxide. The acid solution is selected from one of nitric acid, hydrochloric acid, or sulfuric acid.
7. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (2), the ratio of the amount of MoO3 nanorods to pyrrole monomers is 0.1 g: (0.1-0.5) mL.
8. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (3), the mass ratio of the precursor to the sulfur source is 1:(4-20), and the sulfur source is selected from thiourea, thioacetamide or sodium sulfide.
9. The method for preparing PPy@MoS2 nanotube composite adsorbent material according to claim 2, characterized in that, In step (1), the temperature of the hydrothermal reaction is 160-200℃ and the reaction time is 12-30 h; in step (3), the temperature of the hydrothermal sulfidation reaction is 180-220℃ and the reaction time is 16-36 h.
10. The PPy@MoS2 nanotube composite adsorbent material according to claim 1 or 2 is applied to the adsorption of methylene blue and lysozyme.