Friction forging and riveting process for sheet metal used in interference fits
By using friction forging riveting technology, the high-speed rotation of the rivet and the forging die generates heat to form a forging riveting head, which solves the problems of insufficient joint strength and high equipment wear in the existing technology, and realizes efficient and low-noise automated riveting.
Patent Information
- Application Number
- CN202510598582.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-10
AI Technical Summary
Existing interference fit riveting processes are prone to uneven interference fit when connecting material combinations with large interlayer thickness or many layers, resulting in reduced joint strength. Furthermore, when riveting difficult-to-form materials, the equipment suffers from high wear and tear, high noise, and low production efficiency, making it difficult to meet the needs of modern large-scale production.
The light alloy rivet is driven by a drive head to rotate at high speed with the forging die and generate heat through friction. This causes the rivet body to undergo plastic deformation due to friction with the forging die, forming a forged rivet head. This reduces the riveting force and increases the joint strength. Real-time temperature control and process parameter optimization are used to achieve automated and low-noise processing.
It improves joint strength and processing efficiency, reduces equipment wear and noise, facilitates automated production, and enhances the fatigue life and sealing performance of the joint.
Smart Images

Figure CN123060046A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a riveting technique, specifically a friction forging riveting process for sheet metal used in interference fits. Background Technology
[0002] Existing interference fit riveting processes refer to the expansion and deformation of solid rivets through high-speed upsetting or multiple hammer riveting operations, filling the rivet holes to achieve an interference fit connection. However, for material combinations with large interlayer thicknesses or numerous layers, uneven interference fits can occur, leading to gaps between the rivet and the rivet hole, resulting in reduced joint strength and difficulty in meeting service requirements. Furthermore, in scenarios involving the riveting of large-diameter rivets and difficult-to-form materials such as titanium alloys, the required riveting force causes wear and tear on the riveting equipment, reducing the lifespan of core components, increasing process costs, and decreasing reliability. Additionally, upsetting and hammer riveting easily cause impact damage to the plates being joined, potentially leading to internal cracks that are difficult to detect. Hammer riveting also suffers from high noise levels, with workers operating in harsh environments (120dB noise), significantly impacting process quality due to human factors. Moreover, compared to automated riveting processes, upsetting and hammer riveting are slower and less efficient, making them unsuitable for modern large-scale production tasks involving a large number of rivets. Summary of the Invention
[0003] This invention addresses the aforementioned shortcomings of existing technologies by proposing a friction forging riveting process for sheet metal joints with interference fits. A drive head drives a light alloy rivet / die to rotate at high speed and feed downwards, causing friction between the rivet body and the forging die. This friction accumulates frictional heat, resulting in plastic deformation of the rivet. The rivet body outside the hole forms a forged riveting head, while the rivet body inside the hole expands, ultimately forming a friction forged riveted joint. By introducing frictional heat during the riveting process, the deformation resistance of the rivet is reduced, the riveting force of difficult-to-deform rivets is reduced, equipment wear is reduced, equipment service life is extended, joint strength is strengthened, joint fatigue life is improved, noise is reduced, processing efficiency is increased, and automation is easily achieved.
[0004] This invention is achieved through the following technical solution:
[0005] This invention relates to a friction forging and riveting process for sheet metal with interference fit. The process involves rotating the end of the rivet relative to the forging die and generating heat through friction until the rivet body softens and deforms, after which it is fixedly positioned on the outside of the sheet metal opposite to the rivet cap.
[0006] The rivet includes a rivet cap and a rivet body connected thereto.
[0007] The plate has pre-drilled holes, the cross-sectional area of which is larger than that of the rivet body and smaller than that of the rivet cap.
[0008] The contact portion between the forging die and the rivet body is provided with a recessed cavity.
[0009] The relative rotation refers to: setting the drive head to mesh with the rivet cover and drive the rivet to rotate and / or setting the forging die to rotate.
[0010] The engagement is preferably achieved by a centrally symmetrical wedge-shaped rotation drive groove structure on the top of the rivet cover.
[0011] When the forging die is set to rotate, the rivet is set to either fixed or rotate in the opposite direction.
[0012] The aforementioned fixing is achieved by, but not limited to, limiting the rivet cap.
[0013] The length L1 of the rivet body satisfies t1+t2+β1d2≤L1≤t1+t2+β2d2, where β1 and β2 are the locking coefficients, which need to be selected according to the riveting strength. Usually, β1=1.5 and β2=2 can be taken.
[0014] The rivet body is preferably a cylindrical structure and its diameter d1 satisfies the following conditions: Where: t1 and t2 are the thickness of the plate, d2 is the diameter of the pre-drilled hole, and α is the clearance ratio, which needs to be selected according to the assembly requirements of the rivet and the pre-drilled hole, and is usually taken as 0.92.
[0015] The diameter d3 of the cavity satisfies γ1d2≤d3≤γ2d2, where γ1 and γ2 are diameter coefficients, typically γ1=1.4 and γ2=2; the pit depth h of the selected mold satisfies δ1d2≤h≤δ2d2, where δ1 and δ2 are depth coefficients, typically δ1=0.3 and δ2=0.6.
[0016] The original volume of the rivet body before deformation d1 is the diameter of the rivet body, and L1 is the length of the rivet body.
[0017] The expansion volume of the deformed rivet body D is the equivalent diameter of the rivet body after expansion. d1 is the diameter of the rivet body, d2 is the diameter of the hole in the sheet metal, and L2 is the total thickness of the sheet metal.
[0018] The volume V of the deformed forged riveting head 锻铆头 Equal to the volume V of the mold recess 锻模 V 锻铆头 =V 锻模 Where: the volume V of the mold recess 锻模 It can be obtained directly according to the mold design requirements. Taking a mold with a spherical crown-shaped recess as an example, pit depth R is the radius of the center of the recess, and d3 is the diameter of the recess in the mold.
[0019] The relative rotation parameters are determined by real-time acquisition of the process parameters output by the riveting equipment and prediction of the temperature rise at the contact interface. The rivet feed speed and rotation speed are adjusted in real time by judging the temperature range, so that the rivet temperature during the riveting process is between the temperature at which the rivet material can produce plastic deformation and the temperature at which the rivet material becomes excessively soft.
[0020] The aforementioned frictional heat generation, wherein the rotational speed n and feed rate v satisfy the following conditions: Where: θ1 and θ2 are determined by the total heat of riveting Q, the riveting temperature T, and the material yield strength σ. y The calculations show that θ1 is the lower limit of the process window, θ2 is the upper limit of the process window, n is the rotational speed, and v is the feed rate.
[0021] The total heat generated during riveting is Q = Q1 + Q2, where: the heat generated by friction is... M is the frictional torque, μ is the coefficient of friction, n is the rotational speed, r is the contact radius, l is the axial feed rate, v is the axial feed speed, and F is the frictional torque. N Riveting force; heat of material deformation, which is the heat generated when a material undergoes plastic deformation, converting some of its energy into heat. η def The efficiency coefficient for converting deformation energy into heat is typically taken as 0.8 to 0.9, W. def Let σ be the work done by the deformation of the material, σ be the stress of the material, and ε be the strain of the material. y ε represents the yield strain of the material, i.e., the starting point of plastic deformation. f The final strain of the material.
[0022] Taking a mold with a concave shape resembling a spherical crown as an example, the contact radius... R is the radius of the center of the recess, h is the depth of the recess, L1 is the length of the rivet body, L2 is the total thickness of the plate, and l is the axial feed amount.
[0023] The riveting temperature T mentioned above refers to the internal temperature of the forging riveting head. Where: 0≤x≤h, x is the vertical distance from any point inside the forging head to the surface of the forging head, and h is the depth of the pit. ξ is the dissipation coefficient, 0 < ξ < 1, ρ is the density of the rivet material, C p T is the specific heat capacity of the rivet material, T1 is the temperature at the contact interface between the forging head and the die recess, and T... ∞Here, η1h represents the ambient temperature, Δr represents the calculated thickness, and η1h ≤ Δr ≤ η2h. η1 and η2 are thickness coefficients, typically taken as η1 = 0.05 and η2 = 0.1. Riveting heat diffuses within the rivet through heat conduction, exhibiting a linear temperature distribution. The temperature is highest at the interface between the forging head and the die recess, gradually decreasing away from this interface.
[0024] The yield strength σ y That is, the relationship between the rivet yield strength and temperature satisfies: σ y (T)=σ y0 (T)S(T), where: σ y (T) represents the yield strength of the rivet material at temperature T, σ y0 (T) represents the yield strength of the rivet material at a reference temperature T0, and the temperature-dependent softening function of the rivet material. b represents the material's thermal softening coefficient, which can be determined by obtaining the material's yield strength at different temperatures through standard compression tests, and then calibrating the softening function. During friction forging and riveting, when the temperature rises to a certain value T... c When, yield strength σ y (T) decreases to the critical value σ yc (T), material softening.
[0025] The lower limit value θ1 of the process window is to ensure that the friction between the rivet and the mold generates and accumulates sufficient frictional heat, so that the rivet material softens to the critical value σ. yc (T), and deforms under the action of riveting force, which is determined by σ. y (T)≤ σ yc (T), that is income That is, θ1.
[0026] The upper limit value θ2 of the process window is to avoid excessive frictional heat accumulation between the rivet and the mold, which could lead to excessive softening of the material and joint defects. It is determined as follows: σ y (T)≥(1-τ)σ yc (T), where τ is related to the specific material, 0 < τ < 1, and τ is usually taken as 0.5, i.e. income That is, θ2. Technical effect
[0027] This invention utilizes the rotational friction forging of rivets and dies to form forged rivet heads, reducing the deformation resistance of rivets and the riveting force of difficult-to-deform rivets. Compared with the prior art, this invention can refine the microstructure of the material near the forged rivet head, achieve fine grain strengthening, improve joint strength, reduce equipment wear, enhance joint strength, reduce noise, and the forging die side structure is simple, making it easy to achieve automatic rivet feeding, easy to automate, and improve processing efficiency. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the rivet morphology;
[0029] Figure 2 This is a schematic diagram of the mold morphology;
[0030] Figure 3 This is a schematic diagram of the process in Example 1;
[0031] In the diagram: 1 solid rivet, 2 drive head, 3 pressure ring, 4 forging die, 5 upper workpiece to be connected, 6 lower workpiece to be connected, 7 friction forging and riveting joint;
[0032] Figure 4 This is a schematic diagram of the process in Example 2;
[0033] In the diagram: 1 Forging die, 2 Solid rivet, 3 Pressure ring, 4 Fixture, 5 Upper workpiece to be connected, 6 Lower workpiece to be connected, 7 Friction forging and riveting joint;
[0034] Figure 5 A diagram showing the relationship between rivet expansion and the dimensions of the rivet body and pre-drilled hole;
[0035] Figure 6 This is a diagram of the friction forging and riveting joint in Example 1;
[0036] Figure 7 This is a comparison diagram of the tensile and shear forces of the friction forging and riveting joint in Example 1. Detailed Implementation Example 1
[0037] like Figure 3 As shown, this embodiment illustrates a friction forging riveting connection method, wherein: the upper workpiece 5 to be connected and the lower workpiece 6 to be connected are both 2mm thick aluminum alloy 2A12, the plate hole diameter is 5.1mm, the rivet is 7075-T65 aluminum alloy, the rivet body diameter is 5mm, and the rivet body length is 8.5mm.
[0038] This embodiment specifically includes the following steps:
[0039] 1) Centering stage: The upper layer workpiece 5 and the lower layer workpiece 6 are stacked on the forging die 4, pressed by the pressure ring 3, and the die recess, the pre-made holes of the upper and lower layers workpieces and the rivets are aligned so that their centers are on the same axis.
[0040] 2) Contact stage: Drive mechanism 2, driven by two servo motors and used to realize axial feed motion and circumferential rotation motion respectively, feeds axially until the bottom end of the rivet body contacts the surface of the forging die recess.
[0041] In this embodiment, the axial feed speed of the drive head is set to 2 mm / s to drive the solid rivet 1 to feed axially through the upper and lower layers of workpieces to be connected until the solid rivet 1 contacts the surface of the forging die recess.
[0042] 3) Forging stage: The solid rivet 1 rotates at high speed under the drive of the drive mechanism 2 and feeds downward at a uniform speed. It rubs against the bottom of the forging die 4 at high speed and generates a lot of frictional heat. The accumulated heat softens the solid rivet 1 and produces plastic deformation under the action of riveting force. The rivet body material flows into the forging die recess to form a forging head until the forging head fills the forging die.
[0043] The high-speed friction described herein involves real-time acquisition of process parameters output by the riveting equipment and prediction of the temperature rise at the contact interface. The rivet feed speed and rotation speed are adjusted in real-time based on the temperature range to ensure that the rivet temperature during the riveting process remains between the temperature at which the rivet material can undergo plastic deformation and the temperature at which the rivet material becomes excessively soft. Specifically, this includes:
[0044] 3.1) Based on the relationship between rivet yield strength and temperature σ y (T)=σ y0 (T)S(T) and temperature-deformation relationship σ y (T)≤σ yc (T) Determine the lower limit T1 of the temperature at which the rivet material can undergo plastic deformation, and the upper limit T2 of the temperature at which the rivet material becomes excessively soft;
[0045] 3.2) Calculate the temperature rise ΔT required for the rivet to undergo plastic deformation based on the initial temperature of the rivet, using the heat-temperature formula Q=ξmC. p ΔT is used to calculate the required heat production Q;
[0046] 3.3) Based on the required heat production Q, use MATLAB software to programmatically solve the heat formula Q=Q1+Q2, where, The ratio of the corresponding rotational speed to the feed rate is calculated.
[0047] 3.4) Based on the ratio of rotational speed to feed rate obtained from the solution... Given a reasonable initial rotational speed n and initial feed rate v, friction forging and riveting are carried out. Based on the quality of the friction forging and riveting joint and the above-mentioned friction forging and riveting theory, the rotational speed n and feed rate v are optimized. The forming quality of the friction forging and riveting joint is used as the evaluation standard, and qualified process parameters are gradually optimized to obtain them.
[0048] In this embodiment, the drive head is set to rotate clockwise at 1500 rpm and feed at 1 mm / s to drive the solid rivet 1 to rub against the surface of the forging die recess at high speed, forming a forging head until the forging head fills the entire forging die.
[0049] 4) Clamping stage: The drive head drives the solid rivet 1 to feed axially until the bottom of the rivet head contacts the upper surface of the workpiece to be connected. After cooling, a friction forging riveting joint is formed.
[0050] In this embodiment, the axial feed speed of the drive head is set to 1 mm / s to drive the solid rivet 1 to expand with the forging die until the rivet cap of the rivet 1 contacts the upper surface of the workpiece to be connected.
[0051] like Figure 3 As shown, the friction forging and riveting joint 7 obtained by the above process forms an interference fit connection between the solid rivet 1 and the upper workpiece 5 and the lower workpiece 6 to be connected. The bottom surface of the joint is smooth and crack-free, and it fits tightly with the lower plate, which improves the sealing performance and corrosion resistance of the joint and broadens the application range of the process.
[0052] like Figure 6 As shown, compared with the traditional riveting process, the friction forging joint obtained in this embodiment has a better filling effect in the hole section, improved joint strength, and the required forging head can be obtained by changing the shape of the mold pit.
[0053] like Figure 7 As shown, the peak tensile shear force of the friction forging and riveting joint in this embodiment is 5.4kN, and the mechanical properties of the joint are improved by 18% compared with the traditional upsetting joint.
[0054] Through specific practical experiments, for riveting 2mm thick 7075-T65 aluminum alloy, a riveting and welding composite gun was used. The above method was implemented with the following process parameters: a clockwise rotation speed of 1500 rpm and an axial feed speed of 1mm / s in the first stage, and an axial feed speed of 1mm / s in the second stage. During the friction forging riveting process, the riveting force increased slowly in the first stage and rapidly in the second stage. The maximum riveting force was 8.3kN, and the maximum noise level was 80 decibels, a reduction of 33.3% compared to the 120 decibels noise level of the traditional upsetting process. The riveting process was stable, resulting in a qualified friction forging riveted joint.
[0055] Compared with the prior art, the maximum riveting force in the entire friction forging process in this embodiment is 8.3kN, which is 80.5% lower than the 42.5kN riveting force of the existing traditional upsetting method. This effectively reduces the wear and tear on the riveting equipment and significantly reduces noise. The maximum tensile shear force of the joint is 5.4kN, which is 18% higher than the existing upsetting process. Example 2
[0056] like Figure 4 As shown, this embodiment illustrates a friction forging riveting connection method, wherein: the upper workpiece 5 to be connected and the lower workpiece 6 to be connected are both 2mm thick aluminum alloy 2A12, the plate hole diameter is 5.1mm, the rivet is 7075-T65 aluminum alloy, the rivet body diameter is 5mm, and the rivet body length is 8.5mm.
[0057] This embodiment specifically includes the following steps:
[0058] 1) Centering stage: Rivet 2, upper layer workpiece 5 to be connected and lower layer workpiece 6 to be connected are stacked on fixture 4, pressed by pressure ring 3, and the rivet, the pre-made holes of the upper and lower layer workpieces to be connected and the mold recess are aligned so that their centers are on the same axis.
[0059] 2) Contact stage: The forging die 1 is driven axially by two servo motors, which are used to realize the axial feed motion and the circumferential rotation motion respectively, until the surface of the forging die recess contacts the rivet body.
[0060] The axial feed process parameters are as follows: the axial feed speed of the drive mechanism is 2 mm / s, driving the forging die 1 to feed axially until the surface of the forging die recess contacts the solid rivet 2.
[0061] 3) Forging stage: Under the drive of the drive mechanism, the forging die 1 rotates at high speed and feeds downward at a uniform speed to rub against the solid rivet 2 at high speed and generate a large amount of frictional heat. The accumulated heat softens the solid rivet 2 and produces plastic deformation under the action of riveting force. The rivet material flows into the forging die cavity to form the forging head until the forging head fills the forging die.
[0062] The process parameters for the axial high-speed rotation and feed are as follows: the drive head rotates clockwise at 1500 rpm and the feed speed is 1 mm / s to drive the forging die 1 to rub against the solid rivet 2 at high speed to form a forging head until the forging head fills the entire forging die.
[0063] 4) Clamping stage: The drive head drives the forging die 1 to feed axially until the bottom surface of the forging die contacts the upper surface of the workpiece to be connected. After cooling, a friction forging and riveting joint is formed.
[0064] In this embodiment, the axial feed speed of the drive head is set to 1 mm / s to drive the forging die 1 and the rivet to forge and expand until the bottom surface of the forging die 1 contacts the upper surface of the workpiece to be connected.
[0065] like Figure 4 As shown, the friction forging and riveting joint 7 obtained by the above process forms an interference fit connection between the solid rivet 2 and the upper workpiece 5 and the lower workpiece 6 to be connected. The bottom surface of the joint is smooth and crack-free, and it fits tightly with the lower plate, which improves the sealing performance and corrosion resistance of the joint and broadens the application range of the process.
[0066] Through specific practical experiments, for riveting 2mm thick 7075-T65 aluminum alloy, a riveting and welding composite gun was used. The above method was implemented with the following process parameters: a clockwise rotation speed of 1500 rpm and an axial feed speed of 1mm / s in the first stage, and an axial feed speed of 1mm / s in the second stage. In this embodiment, the riveting force during the friction forging riveting process increased slowly in the first stage and rapidly in the second stage. The maximum riveting force during the riveting process was 8.1kN, and the maximum noise level was 80 decibels, a reduction of 33.3% compared to the 120 decibels noise level of the traditional upsetting process. The riveting process was stable, resulting in a qualified friction forging riveted joint.
[0067] Compared with the prior art, the maximum riveting force in the entire friction forging and riveting process in this embodiment is 8.1kN, which is 80.9% lower than the riveting force of 42.5kN using the traditional upsetting method. This effectively reduces the wear and tear on the riveting equipment and significantly reduces noise. The maximum tensile and shear force of the joint is 5.6kN, which is 23.6% higher than the existing upsetting process.
[0068] The above-described specific implementations can be partially adjusted by those skilled in the art in different ways without departing from the principles and purpose of the present invention. The scope of protection of the present invention is defined by the claims and is not limited to the above-described specific implementations. All implementation schemes within the scope of the claims are bound by the present invention.
Claims
1. A friction forging and riveting process for sheet metal used in interference fits, characterized in that, The rivet is fixed to the plate by rotating relative to the forging die at its end and generating heat through friction until the rivet body softens and deforms, and then being positioned opposite the rivet cap on the outside of the plate. The plate has a pre-drilled hole, the cross-sectional area of which is larger than that of the rivet body and smaller than that of the rivet cap. The relative rotation refers to: setting the drive head to mesh with the rivet cover and drive the rivet to rotate and / or setting the forging die to rotate; The relative rotation parameters are determined by real-time acquisition of the process parameters output by the riveting equipment and prediction of the temperature rise at the contact interface. The rivet feed speed and rotation speed are adjusted in real time by judging the temperature range, so that the rivet temperature during the riveting process is between the temperature at which the rivet material can produce plastic deformation and the temperature at which the rivet material becomes excessively soft.
2. The plate friction forging and riveting process for interference fit according to claim 1, characterized in that, The rivet includes a rivet cap and a rivet body connected thereto.
3. The plate friction forging and riveting process for interference fit according to claim 1, characterized in that, The contact portion between the forging die and the rivet body is provided with a recessed cavity.
4. The plate friction forging and riveting process for interference fit according to claim 1, characterized in that, The engagement is achieved by a centrally symmetrical wedge-shaped rotation drive groove structure on the top of the rivet cover.
5. The plate friction forging and riveting process for interference fit according to claim 1, characterized in that, When the forging die is set to rotate, the rivet is set to either fixed or rotate in the opposite direction.
6. The plate friction forging and riveting process for interference fit according to claim 1, characterized in that, The aforementioned frictional heat generation, wherein the rotational speed n and feed rate v satisfy the following conditions: Where: θ1 and θ2 are determined by the total heat of riveting Q, the riveting temperature T, and the material yield strength σ. y The calculations show that θ1 is the lower limit of the process window, θ2 is the upper limit of the process window, n is the rotational speed, and v is the feed rate. The total heat generated during riveting is Q = Q1 + Q2, where: the heat generated by friction is... M is the frictional torque, μ is the coefficient of friction, n is the rotational speed, r is the contact radius, l is the axial feed rate, v is the axial feed speed, and F is the frictional torque. N Riveting force; heat of material deformation, which is the heat generated when a material undergoes plastic deformation, converting some of its energy into heat. η def W is the efficiency coefficient for converting deformation energy into heat. def Let σ be the work done by the deformation of the material, σ be the stress of the material, and ε be the strain of the material. y ε represents the yield strain of the material, i.e., the starting point of plastic deformation. f The final strain of the material; The riveting temperature T mentioned above refers to the internal temperature of the forging riveting head. Where: 0≤x≤h, x is the vertical distance from any point inside the forging head to the surface of the forging head, and h is the depth of the pit. ξ is the dissipation coefficient, 0 < ξ < 1, ρ is the density of the rivet material, C p T is the specific heat capacity of the rivet material, T1 is the temperature at the contact interface between the forging head and the die recess, and T... ∞ The ambient temperature is η1h, Δr is the calculated thickness, η1h ≤ Δr ≤ η2h, and η1 and η2 are thickness coefficients. The yield strength σ y That is, the relationship between the rivet yield strength and temperature satisfies: σ y (T)=σ y0 (T)S(T), where: σ y (T) represents the yield strength of the rivet material at temperature T, σ y0 (T) represents the yield strength of the rivet material at a reference temperature T0, and the temperature-dependent softening function of the rivet material. b is the thermal softening coefficient of the material.
7. The plate friction forging and riveting process for interference fit according to claim 6, characterized in that, The lower limit value θ1 of the process window is to ensure that the friction between the rivet and the mold generates and accumulates sufficient frictional heat, so that the rivet material softens to the critical value σ. yc (T), and deforms under the action of riveting force, which is determined by σ. y (T)≤σ yc (T), that is income That is, θ1; The upper limit value θ2 of the process window is to avoid excessive frictional heat accumulation between the rivet and the mold, which could lead to excessive softening of the material and joint defects. It is determined as follows: σ y (T)≥(1-τ)σ yc (T), where τ is related to the specific material, 0 < τ < 1, and τ is usually taken as 0.5, i.e. income That is, θ2.