A low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation injection molding and its preparation method

By employing cyclic phase transformation and two-stage aging treatment to strengthen martensitic aging steel with low Ni and high Cr multi-element precipitation, the problems of high cost, insufficient corrosion resistance, and coarsening of microstructure in martensitic aging steel have been solved, thus achieving the preparation of martensitic aging steel with high strength, good plasticity and toughness, and corrosion resistance.

CN123060099APending Publication Date: 2026-11-10UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611129577.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing martensitic aging steels have high Ni content, high cost, and insufficient corrosion resistance. Traditional composition systems are difficult to adapt to metal injection molding processes, and the coarsening of the microstructure and residual porosity after sintering are difficult to optimize, resulting in insufficient precipitation strengthening effect.

Method used

Low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel is adopted. The microstructure is refined through cyclic phase transformation treatment and combined with two-stage aging treatment to form a synergistic strengthening mechanism of B2 ordered phase, Ni3Mo phase and Cu-rich phase, thereby optimizing the pore state.

Benefits of technology

It has achieved low-cost, high-strength, good plasticity, toughness and corrosion resistance martensitic aging steel, which is suitable for near-net-shape forming of complex structural parts and significantly improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060099A_ABST
    Figure CN123060099A_ABST
Patent Text Reader

Abstract

This invention relates to a low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation injection molding and its preparation method. The preparation method includes: mixing alloy powder with a binder and then injection molding, followed by debinding, sintering, homogenization heat treatment, cyclic phase transformation treatment, cryogenic treatment, and two-stage aging treatment. The cyclic phase transformation treatment reconstructs and refines the microstructure after sintering through at least two austenitizing-cooling phase transformation cycles. The two-stage aging treatment promotes the dispersed precipitation of B2 ordered phase, Ni3Mo phase, Cu-rich phase, and a selectively small amount of Laves phase in the martensitic matrix, thereby achieving synergistic strengthening of the martensitic matrix and multi-element precipitation strengthening. This invention, through a combination of low-Ni, high-Cr composition design, multi-element precipitation strengthening, and cyclic phase transformation microstructure control, improves material strength, microstructure uniformity, and corrosion resistance while reducing Ni content. It is suitable for near-net-shape forming of complex, high-strength, corrosion-resistant precision structural parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of powder metallurgy metal injection molding (MIM) and high-strength steel materials, specifically relating to a low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation injection molding and its preparation method. Background Technology

[0002] Metal injection molding (MIM) is a near-net-shape forming technology that combines the advantages of powder metallurgy and polymer injection molding. It can efficiently produce small metal components with complex shapes, high dimensional accuracy, and good batch consistency, and has broad application prospects in precision machinery, aerospace, medical devices, weaponry, and high-end industrial parts. Compared to traditional forging, rolling, or machining processes, MIM has significant advantages in the one-step forming of complex structures, and is particularly suitable for producing complex, high-performance metal parts that are difficult to achieve with conventional plastic processing.

[0003] With the increasing demand for high specific strength, high toughness and integrated forming of complex structural parts in fields such as aerospace, defense equipment, precision transmission and high-end molds, the application of ultra-high strength steel materials in MIM process has received more and more attention.

[0004] Martensitic aging steel is a mainstream type of ultra-high-strength steel based on low-carbon or ultra-low-carbon Fe-Ni alloys. It achieves high strength by obtaining a lath martensitic matrix through solution treatment and precipitating nanoscale intermetallic compounds during aging. Traditional martensitic aging steels are typically represented by the 18Ni series, relying mainly on elements such as Ni, Co, Mo, and Ti to form strengthening phases like Ni3Ti and Ni3Mo. These steels possess advantages such as high strength and low heat treatment deformation, making them valuable in aerospace, mold making, and high-end equipment applications.

[0005] However, existing maraging steels and their preparation processes still have the following problems when used in metal injection molding: 1. Traditional martensitic aging steels have high Ni content and high cost. Existing 18Ni-based martensitic aging steels typically contain high Ni content, and some systems also contain high levels of Co and Mo, resulting in high alloy costs and hindering the large-scale, low-cost fabrication of complex parts by metal injection molding.

[0006] 2. Insufficient corrosion resistance of traditional systems. Existing martensitic aging steels are mainly designed around the Fe-Ni-Co-Mo-Ti system, with low or no Cr content, making it difficult to balance high strength and corrosion resistance, thus limiting their application in humid, chlorine-containing, or corrosive environments.

[0007] 3. The microstructure and defect state after injection molding and sintering are complex. Metal injection molding typically includes steps such as feed mixing, injection molding, debinding, and high-temperature sintering. For sintered Fe-based alloys, the following problems often exist: (1) The residual pores after sintering are difficult to completely eliminate, and the pore morphology is irregular, which easily leads to local stress concentration; (2) The original microstructure is relatively coarse after sintering, especially after high-temperature sintering, the original austenite grains are prone to grow; (3) Localized uneven composition, differences in microstructure near the sintering neck, and incoordination of microstructure around pores are observed. (4) If only conventional single solution treatment and aging treatment is used in the future, it is often difficult to simultaneously achieve the effects of tissue refinement, pore state optimization and precipitation strengthening.

[0008] 4. Balancing martensitic matrix stability and precipitation strengthening under high-Cr conditions is challenging. To improve corrosion resistance, the Cr content is typically increased; however, Cr is a ferrite-forming element, and increasing the Cr content makes it more difficult to obtain a martensitic matrix structure. It may also affect the formation and strengthening effect of traditional aging precipitation systems. Therefore, balancing martensitic matrix stability, corrosion resistance, and precipitation strengthening under high-Cr conditions is one of the design challenges for this type of material.

[0009] 5. Existing processes do not adequately utilize the synergistic effect of "post-sintering microstructure reconstruction and aging precipitation". For MIM sintered materials, the post-sintering microstructure is not an ideal homogeneous and dense state, but rather contains residual porosity, coarsened grains, and localized inhomogeneous regions. If only conventional heat treatment is used, it is difficult to fully reconstruct the post-sintering microstructure, and it is also difficult to provide better matrix conditions for subsequent precipitation of B2, Ni3Mo, Cu-rich phases, etc.

[0010] Therefore, there is an urgent need to develop a martensitic aging steel suitable for metal injection molding, with low Ni content and high Cr content, and capable of obtaining high strength, good ductility and toughness and certain corrosion resistance through synergistic strengthening by cyclic phase transformation and multi-element precipitation, as well as its preparation method. Summary of the Invention

[0011] The purpose of this invention is to provide a low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation injection molding and its preparation method, so as to solve the problems of high cost, insufficient corrosion resistance, difficulty in adapting traditional composition systems to MIM process, coarsening of microstructure after sintering, residual porosity and insufficient synergy of precipitation strengthening in existing martensitic aging steels.

[0012] A method for preparing low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel by injection molding based on cyclic phase transformation includes the following steps: S1. Feed preparation and injection molding: Alloy powder with a Ni content of 4.0-8.0 wt.% and a Cr content of 10.5-17.0 wt.% is mixed with an organic binder to prepare a uniform feed. A blank is prepared by metal injection molding. After degreasing, the blank is sintered at 1200-1400℃ under a protective atmosphere to obtain a dense metal injection molded (MIM) sintered body. S2. Homogenization heat treatment: The MIM sintered body is homogenized at 1100-1250℃ for 1-3 hours, and then cooled to room temperature; S3. Cyclic phase transformation treatment: The MIM sintered body at room temperature is placed in the austenitizing temperature range of 850-1100℃ for cyclic phase transformation treatment to obtain a workpiece with martensitic structure. S4. Cryogenic treatment: After the last cycle of phase transformation is completed, the workpiece is cooled to room temperature and placed in a liquid nitrogen environment for cryogenic holding for 1 hour. S5. Two-stage aging treatment: Perform two-stage aging treatment on the workpiece after cryogenic treatment; S6. Finished Product Acquisition: After aging is completed, cool to room temperature to obtain the final product.

[0013] In addition to the aspects described above and any possible implementation, an implementation is further provided in which the number of cycles is 2-6, and each cycle includes: holding for 15-90 minutes to transform the microstructure into austenite, followed by rapid cooling to obtain a martensitic microstructure.

[0014] In addition to the aspects described above and any possible implementation, a further implementation is provided, wherein the two-stage aging process includes: a first-stage pre-aging at 420-480℃ for 0.5-4 hours, and a second-stage final aging at 500-560℃ for 1-8 hours.

[0015] In addition to the aspects and any possible implementations described above, a further implementation is provided in which, in step S2, the cooling method is oil cooling or water cooling.

[0016] In addition to the aspects and any possible implementations described above, a further implementation is provided in which the first-stage pre-aging is maintained at 450-480℃ for 2-3 hours, and the second-stage final aging is maintained at 520-550℃ for 2-5 hours.

[0017] In addition to the aspects described above and any possible implementation, a further implementation is provided in which the temperature in S2 is 1100-1250 ℃ and the time period is 1-3h.

[0018] The present invention also provides an injection-molded low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation, wherein the martensitic aging steel is obtained by the preparation method described above.

[0019] In addition to the aspects described above and any possible implementation, an implementation is further provided, comprising, by mass percentage, the following components: Cr: 8-16 wt.%; Al: 1-5 wt.%; Co: 5-18 wt.%; Ni: 1-8 wt.%; Cu: 0.5-1.8 wt.%; Mo: 0-5 wt.%; W: 0-3 wt.%; Ti: 0-1.0 wt.%; Nb: 0-0.5 wt.%; C: 0.01-0.15 wt.%; B: 0-0.05 wt.%; N: 0-0.20 wt.%; Fe: balance and unavoidable impurities; The martensitic aging steel, after aging treatment, has a martensitic matrix, and one or more of the following phases precipitate on the martensitic matrix: B2 ordered phase, Ni3Mo phase, Cu-rich phase, and optionally Laves phase.

[0020] In addition to the aspects described above and any possible implementations, a further implementation is provided in which the martensitic aging steel comprises, by mass percentage: 9-13 wt.% Cr, 1.2-2.8 wt.% Al, 6-12 wt.% Co, 3-7 wt.% Ni, 0.8-1.5 wt.% Cu, 1.5-4.0 wt.% Mo, 0-1.5 wt.% W, 0.1-0.6 wt.% Ti, 0.03-0.3 wt.% Nb, 0.01-0.06 wt.% C, 0-0.01 wt.% B, and 0.02-0.12 wt.% N.

[0021] In addition to the aspects described above and any possible implementation, an implementation is further provided, comprising, by mass percentage, the following components: Cr: 10.0-12.0 wt.%; Al: 1.4-2.2 wt.%; Co: 7.0-10.0 wt.%; Ni: 4.0-6.0 wt.%; Cu: 0.9-1.3 wt.%; Mo: 2.0-3.5 wt.%; W: 0-0.8 wt.%; Ti: 0.15-0.45 wt.%; Nb: 0.05-0.20 wt.%; C: 0.01-0.04 wt.%; N: 0.03-0.08 wt.%; B: 0-0.005 wt.%; with the balance being Fe and unavoidable impurities.

[0022] Beneficial effects 1. Low Ni and high Cr composition design balances cost, strength and corrosion resistance; This invention adopts a low Ni and high Cr composition design, which reduces the amount of Ni used and the material cost, while improving corrosion resistance through Cr, and uses elements such as Al, Co, Mo and Cu to construct a multi-element precipitation strengthening system, thereby balancing cost, strength and environmental adaptability.

[0023] 2. Formation of a synergistic strengthening mechanism between martensitic matrix and multi-component precipitates: After aging treatment, the present invention can precipitate B2 ordered phase, Ni3Mo phase, Cu-rich phase and controlled small amount of Laves phase on the martensitic matrix, forming a composite strengthening mechanism of "martensitic matrix strengthening + multi-component precipitation strengthening", which is beneficial to obtaining higher strength and excellent comprehensive mechanical properties.

[0024] 3. Cyclic phase transformation treatment can significantly improve the microstructure after MIM sintering; the present invention introduces cyclic phase transformation treatment after sintering, which can refine the original austenite grains and martensite structure, improve the problem of microstructure coarsening and local inhomogeneity after sintering, and optimize the local microstructure and interface state around the pores, thereby improving the microstructure uniformity and subsequent heat treatment response.

[0025] 4. Cyclic phase change and aging treatment work together to improve strengthening efficiency; cyclic phase change treatment can provide a more uniform matrix structure and more potential precipitation sites for subsequent aging precipitation, promote the dispersion precipitation of strengthening phase, and thus achieve synergistic effect of cyclic phase change structure regulation and aging precipitation strengthening. Attached Figure Description

[0026] Figure 1 This is a process flow diagram of the present invention.

[0027] Figure 2 The images show the inverse pole figures obtained by electron backscatter diffraction (EBSD) analysis before and after the cyclic phase transition treatment experiment of this invention. (a) is the inverse pole figure before treatment, and (b) is the inverse pole figure after treatment. Detailed Implementation

[0028] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0029] It should be noted that the terms "comprising" and "having" and any variations thereof in the specification, claims and accompanying drawings of this invention are intended to cover non-exclusive inclusion. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are explicitly listed, but may include other steps or units that are not explicitly listed or that are inherent to such processes, methods, products or devices.

[0030] like Figure 1 As shown, this invention provides a method for preparing low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel by injection molding based on cyclic phase transformation. The alloy powder has a Ni content of 4.0-8.0 wt.% and a Cr content of 10.5-17.0 wt.%. After subsequent sintering and heat treatment, the final product has a Ni content of 1.0-8 wt.% and a Cr content of 8.0-16.0 wt.%, maintaining the overall characteristics of low-Ni and high-Cr. This method is used to prepare the martensitic aging steel and includes the following steps: S1. Feed preparation and injection molding: Mix the proportioned alloy powder with an organic binder to prepare a uniform feed, prepare a billet by metal injection molding, degrease the billet, and sinter it at 1200-1400 ℃ under a protective atmosphere to obtain a dense MIM sintered body. The organic binder comprises: 84-88% polyoxymethylene (POM), 6-10% high-density polyethylene (HDPE), 3-5% paraffin wax (PW), and 2-4% ethylene-vinyl acetate (EVA) (all by weight percentages). The binder's function is to impart good flowability to the alloy powder for injection molding, maintain the shape integrity of the preform, and be completely removed during the debinding stage through catalytic or thermal decomposition, leaving no residue in the final metal product. It has no direct impact on the final product's performance. However, the compatibility between the binder formulation and the debinding process affects the residual carbon content and porosity after sintering, thus indirectly influencing the mechanical properties.

[0031] S2. Homogenization heat treatment: The MIM sintered body is placed at 1100-1250 ℃ for 1-3 h to homogenize and eliminate element segregation and local compositional inhomogeneity inside the sintered body, and then cooled to room temperature. S3. Cyclic Phase Transformation Treatment: The homogenized MIM sintered body is placed in the austenitizing temperature range of 850-1100℃ for cyclic phase transformation treatment. Each cycle includes: holding the body at a temperature close to Ac3, preferably 850-1100℃, adjusted according to composition changes, for 15-90 minutes to partially transform the microstructure into austenite; then removing it and rapidly cooling it to obtain martensitic microstructure. This rapid cooling process is used to freeze the metastable microstructure and stress field formed during the cyclic phase transformation, rather than simply achieving martensitic transformation. The cyclic process is repeated 2-6 times. Figure 2To conduct experiments on the cyclic phase transition treatment of this invention, inverse pole figures were obtained before and after the experiment using electron backscatter diffraction (EBSD) analysis, wherein... Figure 2 (a) is the inverse pole figure before treatment, showing that the MIM sintered structure has coarse grains (average grain size of about 80-120 μm), obvious orientation concentration and local texture, and uneven distribution of residual pores; Figure 2 (b) is the inverse pole figure after treatment, showing that the grains are significantly refined (average grain size is about 15-25 μm) after cyclic phase transformation treatment, the orientation tends to be randomly distributed, the uniformity of the structure is significantly improved, and the structure around the pores is optimized.

[0032] S4. Cryogenic treatment: After the last cycle of phase transformation is completed, the workpiece is cooled to room temperature and placed in a liquid nitrogen environment for cryogenic holding for 1 hour to further reduce the content of residual austenite, improve the stability of the microstructure and reduce the residual metastable phase of the cycle phase transformation.

[0033] S5. Two-stage aging treatment: The cryogenically treated alloy undergoes a two-stage aging treatment. The first stage pre-aging is performed at 420-480℃ for 0.5-4 h, and the second stage final aging is performed at 500-560℃ for 1-8 h. This two-stage aging regime promotes the uniform nucleation of fine precipitates such as the B2 ordered phase and Cu-rich phase through low-temperature pre-aging, and then promotes the further precipitation and growth of the Ni3Mo phase and Laves phase at a higher temperature. This achieves the stepwise precipitation and synergistic strengthening of multi-component precipitates, avoiding the over-aging or uneven distribution of precipitates that may occur with single-stage aging. This results in the precipitation of the B2 ordered phase, Ni3Mo phase, Cu-rich phase, and optionally the Laves phase in the martensitic matrix. The two-stage aging regime is, for example, 420-480℃ × 0.5-4 h + 500-560℃ × 1-8 h.

[0034] S6. Finished Product Acquisition: After aging is completed, cool to room temperature to obtain the final product.

[0035] It should be noted that the chemical composition of the alloy powder in this invention differs from that of the final product. This is because: (1) some low-melting-point elements (such as impurities like Mn and Si) volatilize during sintering; (2) residual carbon from degreasing reacts with oxygen during sintering to form CO or CO2, resulting in a decrease in carbon content; and (3) trace amounts of carbon, oxygen, and nitrogen remaining from the decomposition of the binder partially dissolve in the matrix or form precipitates, affecting the final composition. Therefore, the Ni content of 4.0-8.0 wt.% and the Cr content of 10.5-17.0 wt.% in the alloy powder are designed to be slightly higher than or fall within the range of the final product. After sintering and subsequent heat treatment, the Ni content in the final product is 1-8 wt.% and the Cr content is 8-16 wt.%, which are different processing stages of the same alloy system.

[0036] Considering the sintering volatilization loss, this invention introduces and sets the Cr content to 8-16 wt.%, wherein the Cr content in the alloy powder is designed to be 10.5-17.0 wt.%, which improves the material's corrosion resistance and oxidation resistance, and balances high strength and corrosion resistance, making it more suitable for humid or corrosive environments than traditional low-Cr martensitic aging steel.

[0037] This invention controls the Ni content within the range of 4-8 wt.% in alloy powder and 1-8 wt.% in the final product, thereby reducing alloy costs while ensuring the formation of martensitic matrix and precipitation strengthening potential.

[0038] Compared with conventional single solution treatment, this invention introduces cyclic phase transformation treatment to refine the original austenite grains and martensite lath structure, improve the coarsening and local microstructure inhomogeneity after sintering, and optimize the local interface state around the pores.

[0039] During the aging process, B2 ordered phase, Ni3Mo phase, Cu-rich phase and controlled small amount of Laves phase are formed. The synergistic effect of multiple precipitates significantly improves yield strength and tensile strength.

[0040] The dispersed MC or M(C,N) particles formed by Ti, Nb and C, N can inhibit grain growth, enhance microstructure stability, and improve the strength-toughness balance.

[0041] This invention is prepared using the MIM process, which can be used for near-net-shape manufacturing of complex structures and high-dimensional precision parts, combining the advantages of material properties and process.

[0042] In a preferred embodiment, the chemical composition of the alloy powder in step S1 is: Cr: 10.5-17.0 wt.%; Al: 1.5-5.5 wt.%; Co: 7.0-18.0 wt.%; Ni: 4.0-8.0 wt.%; Cu: 0.8-1.8 wt.%; Mo: 1.5-5.0 wt.%; W: 0-3.0 wt.%; Ti: 0.15-1.0 wt.%; Nb: 0.05-0.5 wt.%; C: 0.02-0.15 wt.%; N: 0.02-0.20 wt.%; B: 0.005-0.05 wt.%; Fe: Balance and unavoidable impurities.

[0043] The element content in the above alloy powder refers to the proportion of the powder raw materials. Due to the volatilization loss of some elements and the carbon-oxygen reaction during sintering, the content in the final product will change, with some elements decreasing in content and less volatile elements such as Fe becoming relatively enriched, but the overall alloy system remains unchanged. The design of the content of each element in the alloy powder is based on the target composition of the final product, taking into account both volatilization loss and the densification requirements of sintering.

[0044] The final product obtained according to this method contains: Cr: 8-16 wt.%; Al: 1-5 wt.%; Co: 5-18 wt.%; Ni: 1-8 wt.%; Cu: 0.5-1.8 wt.%; Mo: 0-5 wt.%; W: 0-3 wt.%; Ti: 0-1.0 wt.%; Nb: 0-0.5 wt.%; C: 0.01-0.15 wt.%; N: 0-0.20 wt.%; B: 0-0.05 wt.%; Fe: balance and unavoidable impurities.

[0045] (1) Cr: improves corrosion resistance and participates in phase stability regulation; Cr is used to improve the corrosion resistance and oxidation resistance of alloys, but Cr is a ferrite forming element. If the content is too high, it may weaken the stability of the martensite matrix. Therefore, it is preferred to control it at 10.5-17.0 wt.%, which corresponds to 8-16 wt.% in the final product.

[0046] (2) Al: Promotes the formation of B2 ordered phase; Al is one of the important elements for the formation of B2 ordered precipitate phase. In synergy with elements such as Ni and Fe, nanoscale B2 phase can be precipitated during aging, thus providing a significant precipitation strengthening effect. Too low Al content is not conducive to the formation of B2 phase, while too high Al content may cause embrittlement or be detrimental to matrix stability. It is preferred to control it at 1.5-5.5 wt.%, corresponding to 1-5 wt.% in the final product.

[0047] (3) Co: Improves the aging strengthening response of martensite; Co helps to improve the aging strengthening response, promotes the formation of Ni-Al and Ni-Mo precipitates, and improves the strength level. It is preferred to control it at 7.0-18.0 wt.%, corresponding to 5-18 wt.% in the final product.

[0048] (4) Ni: Regulates the martensitic matrix and precipitation strengthening system; Ni is an austenitic stabilizing element that can assist in obtaining a martensitic matrix under high Cr conditions and participate in the formation of precipitation strengthening systems such as B2 phase and Ni3Mo phase. Compared with traditional 18Ni martensitic aging steel, this invention adopts a low Ni design to balance cost and performance. Preferably controlled at 4.0-8.0 wt.%, more preferably 4.5-6.5 wt.%, corresponding to 1-8 wt.% in the final product.

[0049] (5) Cu: Cu-rich nano-precipitates are formed; Cu can form Cu-rich nano-precipitates during aging, which can serve as an auxiliary strengthening phase to improve the aging strengthening response, and can also work together with other precipitates to improve strength. It is preferably controlled at 0.8-1.8 wt.%, corresponding to 0.5-1.8 wt.% in the final product.

[0050] (6) Mo and W: Promote the formation of Ni3Mo and Laves phases; Mo is an important strengthening element and can promote the formation of Ni3Mo type precipitates; when the Mo content is high and synergistic with Cr and W, a controlled small amount of Laves phase can also be formed during aging, further improving the strength. W can partially replace Mo and increase the tendency of Laves phase formation. Mo is preferably controlled at 1.5-5.0 wt.%, and W is preferably controlled at 0-3.0 wt.%, corresponding to 0-5 wt.% Mo and 0-3 wt.% W in the final product.

[0051] (7) Ti, Nb, C, N: form MC / M(C,N) and stabilize the microstructure; Ti, Nb, C, and N can form dispersed MC-type carbides and / or M(C,N) carbonitrides, which are used to pin grain boundaries, inhibit the growth of original austenite grains, and improve the microstructure stability after sintering and during cyclic phase transformation. N can also be used as an interstitial element to enhance solid solution strengthening and regulate the stability of austenite under high Cr conditions. Among them, Ti is preferably controlled at 0.15-1.0 wt.%, Nb is preferably controlled at 0.05-0.5 wt.%, C is preferably controlled at 0.02-0.15 wt.%, and N is preferably controlled at 0.02-0.20 wt.%; corresponding to Ti being 0-1.0 wt.%, Nb being 0-0.5 wt.%, C being 0.01-0.15 wt.%, and N being 0-0.20 wt.% in the final product.

[0052] (8) B: Improve grain boundary state; B can improve the grain boundary bonding state under trace conditions, but too high content may be detrimental to toughness. Therefore, it is preferred to control it at 0.005-0.05wt.%, which corresponds to 0-0.05wt.% in the final product.

[0053] This invention achieves a composite strengthening mechanism of martensitic matrix strengthening + cyclic phase transformation microstructure control + multi-element precipitation synergistic strengthening by synergistically designing elements such as Cr, Al, Co, Ni, Cu, Mo, W, Ti, Nb, C, N, and B, which allows the alloy to obtain a refined and uniform martensitic matrix structure through cyclic phase transformation treatment after sintering. During the subsequent aging process, ordered B2 phase, Laves phase, Cu-rich phase, and Ni3Mo phase precipitate. At the same time, Cr is used to improve corrosion resistance, N is used to control phase stability under high Cr conditions and provide interstitial strengthening, and Ti, Nb and low C content are used to form dispersed MC-type carbides or carbonitrides to inhibit grain growth. Finally, injection-formed martensitic aging steel with high strength, good plasticity and toughness and certain corrosion resistance is obtained.

[0054] In a preferred embodiment, the homogenization treatment temperature in step S2 is 1100-1250℃, the holding time is 1-12 hours, preferably 1-6 hours, and the cooling method is oil cooling or water cooling.

[0055] In a preferred embodiment, the parameters for the cyclic phase transition treatment in step S3 are as follows: Each cycle involves holding at 850-1100℃ for 15-90 minutes to achieve complete austenitization and homogenization of the microstructure; then removing and rapidly cooling; the number of cycles is 2-6.

[0056] In a preferred embodiment, the aging processing parameters in step S6 are as follows: Pre-aging: 450-480℃×2-3h, Secondary aging: 520-550℃×2-5h.

[0057] As an embodiment of the present invention, the present invention also provides a low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation injection molding, which is obtained by the preparation method of the present invention. The martensitic aging steel obtained has the following physical and mechanical advantages: (1) fine and uniform grains; (2) residual porosity ≤1.5%, pore size ≤10μm and uniform distribution; (3) room temperature tensile strength ≥1800MPa, yield strength ≥1600MPa, elongation ≥8%; (4) corrosion potential in 3.5% NaCl solution is about 200mV higher than that of traditional 18Ni martensitic aging steel, and corrosion resistance is significantly improved; (5) hardness ≥52HRC, with both high strength and certain toughness, suitable for precision structural parts.

[0058] The martensitic aging steel obtained comprises the following components by mass percentage: Cr: 8-16 wt.%; Al: 1-5 wt.%; Co: 5-18 wt.%; Ni: 1-8 wt.%; Cu: 0.5-1.8 wt.%; Mo: 0-5 wt.%; W: 0-3 wt.%; Ti: 0-1.0 wt.%; Nb: 0-0.5 wt.%; C: 0.01-0.15 wt.%; N: 0-0.20 wt.%; B: 0-0.05 wt.%; Fe: Balance and unavoidable impurities.

[0059] The martensitic aging steel, after aging treatment, has a martensitic matrix, and at least one or more of the following precipitates on the martensitic matrix: an ordered B2 phase and a Ni3Mo phase, as well as a Cu-rich phase and an optional Laves phase.

[0060] Preferably, the martensitic aging steel comprises, by mass percentage: Cr: 9.0-13.0 wt.%; Al: 1.2-2.8 wt.%; Co: 6.0-12.0 wt.%; Ni: 3.0-7.0 wt.%; Cu: 0.8-1.5 wt.%; Mo: 1.5-4.0 wt.%; W: 0-1.5 wt.%; Ti: 0.10-0.60 wt.%; Nb: 0.03-0.30 wt.%; C: 0.01-0.06 wt.%; N: 0.02-0.12 wt.%; B: 0-0.01 wt.%; Fe: Balance and unavoidable impurities.

[0061] More preferably, the martensitic aging steel comprises, by mass percentage: Cr: 10.0-12.0 wt.%; Al: 1.4-2.2 wt.%; Co: 7.0-10.0 wt.%; Ni: 4.0-6.0 wt.%; Cu: 0.9-1.3 wt.%; Mo: 2.0-3.5 wt.%; W: 0-0.8 wt.%; Ti: 0.15-0.45 wt.%; Nb: 0.05-0.20 wt.%; C: 0.01-0.04 wt.%; N: 0.03-0.08 wt.%; B: 0-0.005 wt.%; Fe: Balance and unavoidable impurities.

[0062] The following specific examples will be used for illustration.

[0063] Example 1:

[0064] High-purity commercial powders with a purity of not less than 99.9 wt.% are selected, including Cr powder, Al powder, Co powder, Ni powder, Cu powder, Mo powder, Ti powder, Nb powder, C powder, Fe powder, etc. Each powder is weighed separately according to the target component and mixed evenly. The selected powders are mixed evenly according to the following formula: 10.5Cr-2.2Al-10.0Co-4.5Ni-1.2Cu-2Mo-0.25Ti-0.1Nb-0.03C-0.03N. The powders are then mixed with a binder to form a feedstock. The powder loading is approximately 65 vol.%, and the binder ratio is: 84% polyoxymethylene, 8% high-density polyethylene, 4% paraffin wax, and 4% ethylene-vinyl acetate. The preform was prepared by injection molding, and then subjected to solvent degreasing and thermal degreasing. It was then sintered at 1360 °C for 2 h under vacuum to obtain a sintered body. The sintered body was then subjected to cyclic phase transformation treatment: held at 900 °C for 1 h and air-cooled to room temperature, repeated twice. Single-stage aging was then performed: held at 500 °C for 5 h and air-cooled. The martensitic aging steel prepared in this embodiment has the following advantages: fine and uniform microstructure with an average grain size of approximately 20 μm; tensile strength ≥1850 MPa, yield strength ≥1650 MPa, elongation ≥9%; hardness approximately 53 HRC; and significantly improved corrosion resistance compared to traditional 18Ni steel, making it suitable for high-strength, corrosion-resistant precision parts for aerospace applications.

[0065] Example 2:

[0066] High-purity commercial powder with a purity of not less than 99.9 wt.% was selected and mixed uniformly according to the following formula: 9.5Cr-2.5Al-12Co-5.5Ni-1.3Cu-3Mo-1W-0.3Ti-0.1Nb-0.03C-0.02N. The alloy powder was then mixed with a binder and injection molded. After debinding, the mixture was sintered at 1370 ℃ for 2 h under vacuum. The sintered body underwent cyclic phase transformation treatment: holding at 900 ℃ for 1 h followed by air cooling to room temperature, repeated twice. Subsequently, a two-stage aging treatment was performed: holding at 480 ℃ for 2 h + holding at 520 ℃ for 4 h, followed by air cooling. The martensitic aging steel prepared in this embodiment has the following advantages: the grain size is refined to about 18 μm, and the B2 and Ni3Mo precipitates are dispersed; the tensile strength is ≥1900 MPa, the yield strength is ≥1700 MPa, and the elongation is ≥8%; the hardness is about 54 HRC; the porosity is ≤1.2%, and the comprehensive mechanical properties are excellent, making it suitable for high-stress precision structural parts.

[0067] Example 3:

[0068] High-purity commercial powder with a purity of not less than 99.9 wt.% was selected and mixed uniformly according to the formula 13Cr-1.8Al-8Co-5Ni-1Cu-1.5Mo-0.15Ti-0.05Nb-0.02C-0.06N. The alloy powder was then mixed with a binder, with a powder loading of approximately 63 vol.%. The preform was obtained by injection molding. After debinding, it was sintered at 1350 ℃ for 2 h under vacuum. The sintered body underwent cyclic phase transformation treatment: held at 920 ℃ for 0.5 h and then air-cooled, repeated twice. Subsequently, aging treatment was performed: held at 490 ℃ for 6 h and then air-cooled. The martensitic aging steel prepared in this embodiment has the following advantages: high Cr content, with the final product containing about 12-13%, and the best corrosion resistance; tensile strength ≥1750MPa, yield strength ≥1550MPa, elongation ≥10%; hardness about 51HRC; it has both good corrosion resistance and sufficient strength, and is suitable for precision parts in humid or weakly corrosive environments.

[0069] The foregoing description illustrates and describes several preferred embodiments of the present invention. However, as previously stated, it should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the inventive concept described herein through the foregoing teachings or techniques or knowledge in related fields. Any modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A method for preparing low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel by injection molding based on cyclic phase transformation, characterized in that, Includes the following steps: S1. Feed preparation and injection molding: Alloy powder with a Ni content of 4.0-8.0 wt.% and a Cr content of 10.5-17.0 wt.% is mixed with an organic binder to prepare a uniform feed. A billet is prepared by metal injection molding. After degreasing, the billet is sintered at 1200-1400℃ under a protective atmosphere to obtain a dense metal injection molded (MIM) sintered body. S2. Homogenization heat treatment: The MIM sintered body is homogenized at 1100-1250℃ for 1-3 hours, and then cooled to room temperature; S3. Cyclic phase transformation treatment: The MIM sintered body at room temperature is placed in the austenitizing temperature range of 850-1100℃ for cyclic phase transformation treatment to obtain a workpiece with martensitic structure. S4. Cryogenic treatment: After the last cycle of phase transformation is completed, the workpiece is cooled to room temperature and placed in a liquid nitrogen environment for cryogenic holding for 1 hour. S5. Two-stage aging treatment: Perform two-stage aging treatment on the workpiece after cryogenic treatment; S6. Finished Product Acquisition: After aging is completed, cool to room temperature to obtain the final product.

2. The method according to claim 1, characterized in that, The number of cycles is 2-6, and each cycle includes: holding for 15-90 minutes to transform the tissue into austenite, followed by rapid cooling to obtain a martensitic tissue.

3. The method according to claim 1, characterized in that, The two-stage aging process includes: a first-stage pre-aging process of holding at 420-480℃ for 0.5-4 hours, and a second-stage final aging process of holding at 500-560℃ for 1-8 hours.

4. The method according to claim 1, characterized in that, In step S2, the cooling method is either oil cooling or water cooling.

5. The method according to claim 3, characterized in that, The first stage of pre-aging involves holding at 450-480℃ for 2-3 hours, and the second stage of final aging involves holding at 520-550℃ for 2-5 hours.

6. The method according to claim 1, characterized in that, The temperature in S2 is 1100-1250℃, and the time period is 1-3 hours.

7. A low-Ni, high-Cr multi-element precipitation-strengthened martensitic aging steel based on cyclic phase transformation injection molding, characterized in that... The martensitic aging steel is obtained by the preparation method according to any one of claims 1-6.

8. The martensitic aging steel according to claim 7, characterized in that, The composition, by mass percentage, includes the following components: Cr: 8-16 wt.%; Al: 1-5 wt.%; Co: 5-18 wt.%; Ni: 1-8 wt.%; Cu: 0.5-1.8 wt.%; Mo: 0-5 wt.%; W: 0-3 wt.%; Ti: 0-1.0 wt.%; Nb: 0-0.5 wt.%; C: 0.01-0.15 wt.%; B: 0-0.05 wt.%; N: 0-0.20 wt.%; Fe: Balance and unavoidable impurities; The martensitic aging steel, after aging treatment, has a martensitic matrix, and one or more of the following phases precipitate on the martensitic matrix: B2 ordered phase, Ni3Mo phase, Cu-rich phase, and optionally Laves phase.

9. The martensitic aging steel according to claim 7, characterized in that, The martensitic aging steel comprises the following components by mass percentage: Cr content of 9-13 wt.%, Al content of 1.2-2.8 wt.%, Co content of 6-12 wt.%, Ni content of 3-7 wt.%, Cu content of 0.8-1.5 wt.%, Mo content of 1.5-4.0 wt.%, W content of 0-1.5 wt.%, Ti content of 0.1-0.6 wt.%, Nb content of 0.03-0.3 wt.%, C content of 0.01-0.06 wt.%, B content of 0-0.01 wt.%, N content of 0.02-0.12 wt.%, Fe balance and unavoidable impurities.

10. The martensitic aging steel according to claim 8, characterized in that, By mass percentage, it consists of the following components Composition: Cr: 10.0-12.0 wt.%; Al: 1.4-2.2 wt.%; Co: 7.0-10.0 wt.%; Ni: 4.0-6.0 wt.%; Cu: 0.9-1.3 wt.%; Mo: 2.0-3.5 wt.%; W: 0-0.8 wt.%; Ti: 0.15-0.45 wt.%; Nb: 0.05-0.20 wt.%; C: 0.01-0.04 wt.%; N: 0.03-0.08 wt.%; B: 0-0.005 wt.%; balance is Fe and unavoidable impurities.