A method for welding process holes in the traction housing of a coal mining machine
By adopting a stepped straight bevel design and MAG welding technology for the process holes of the coal mining machine traction shell, combined with welding thermal cycling tempering treatment, the problem of easy cracking of the process holes of the coal mining machine traction shell was solved, and the high efficiency and reliability of the welded joint were achieved.
Patent Information
- Application Number
- CN202611250624.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-10
Smart Images

Figure CN123060198A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mechanical manufacturing technology, and in particular to a method for welding process holes in the traction housing of a coal mining machine. Background Technology
[0002] In electrically driven coal mining machines, the traction housing is the core structural component that supports the traveling transmission mechanism and hydraulic system. Its internal cavity directly serves as the hydraulic oil tank, eliminating the need for a separate oil tank structure. This saves installation space and allows for hydraulic oil cooling through the housing wall. The traction housing is integrally cast using sand casting technology. The material is ZG25CrNiMo medium-carbon quenched and tempered steel. After casting, it undergoes multiple processes including normalizing, tempering, rough machining, and quenching and tempering to achieve the required mechanical properties and basic shape accuracy.
[0003] During the casting process, a process hole is pre-drilled at the corresponding position in the hydraulic oil tank on the traction housing. This process hole penetrates the housing wall thickness and is used to thoroughly clean residual molding sand inside the mold cavity after casting, as well as for subsequent anti-corrosion painting of the hydraulic oil tank's inner wall. After the traction housing is fully finished and the hydraulic oil tank's inner wall is painted, a circular plug plate made of Q355 steel is welded to the process hole using MAG welding to achieve a strict seal and prevent hydraulic oil leakage.
[0004] The traction housing material, ZG25CrNiMo, is a medium-carbon quenched and tempered steel with a high carbon equivalent, resulting in poor weldability. Furthermore, the wall thickness at the process holes is significant, leading to rapid cooling during welding. Preheating to 100℃~150℃ before welding is necessary to slow the cooling rate and prevent cold cracking. Since the traction housing has already undergone precision machining and the hydraulic tank's inner wall is painted, post-weld heat treatment is not possible. This makes it difficult to improve the hardened martensite structure formed in the weld heat-affected zone, and residual welding stress cannot be effectively eliminated. Consequently, there is a significant risk of cracking in the later stages of the process-sealed weld.
[0005] Existing welded joints in process holes mostly employ conventional bevel structures, which allow cracks to propagate rapidly along the fusion line and form penetrating cracks, directly leading to hydraulic oil leakage. Regarding the welding process, direct bevel filling welding results in high welding restraint, high residual stress, and a significant tendency for cracking in the heat-affected zone of medium-carbon tempered steel. If the welded joint structure and welding process are unreasonable, penetrating cracks can form quickly, causing oil leakage from the traction housing, resulting in a drop in hydraulic system pressure and severely impacting the normal operation of the coal mining machine underground. Summary of the Invention
[0006] The purpose of this invention is to provide a method for welding process holes in the traction housing of a coal mining machine, so as to solve the problems existing in the prior art.
[0007] To achieve the above objectives, the present invention provides the following solution: The present invention provides a method for welding process holes in the traction housing of a coal mining machine, comprising: S1, process the process hole of the traction housing to form a stepped straight bevel, process a circular process block plate that matches the process hole, and clean the oil, rust and oxide scale on the bevel and the surface of the base material on both sides until the metal luster is exposed. S2, insert the process plug plate into the process hole and position it on the step surface, so that a uniform circumferential annular welding gap is formed between the outer circle of the process plug plate and the inner wall of the bevel. S3, the process hole bevel area is preheated with a flame, and a layer of fusion layer is deposited on the inner wall of the bevel along the wall thickness direction using MAG welding. S4 uses MAG welding for multi-layer, multi-pass welding to fuse the process plug plate and traction housing into one piece and fill the bevel. S5, Weld a tempering weld bead on the outside of the shell, and use the welding heat cycle to temper the microstructure of the heat-affected zone. S6, remove the tempered weld bead and weld metal protruding above the base metal surface to make the weld surface flush with the base metal, and perform magnetic particle testing on the weld joint.
[0008] According to the welding method for process holes of the traction housing of the coal mining machine provided by the present invention, in S1, the traction housing material is ZG25CrNiMo medium carbon quenched and tempered steel, and the process plug plate material is Q355 low alloy high strength steel; the stepped straight bevel is formed by CNC milling machine, and the bevel cleaning range is the bevel surface and the surface area of the base material on both sides not less than 20mm.
[0009] According to the coal mining machine traction housing process hole welding method provided by the present invention, in S2, the outer diameter of the process plug plate and the inner diameter of the process hole step are fitted with a clearance. After assembly, the lower surface of the process plug plate is tightly fitted with the step surface, and a circumferentially uniform annular welding gap is formed between the outer circular surface of the process plug plate and the inner wall surface of the bevel.
[0010] According to the welding method for process holes of the coal mining machine traction housing provided by the present invention, in step S3, the specific process of preheating and overlay welding includes the following steps: S31 uses flame heating to preheat the bevel area of the process hole, with the preheating temperature controlled at 100℃~150℃, and the temperature measurement point is located on the surface of the base material outside the bevel. S32, MAG welding is used to deposit a fusion layer along the wall thickness direction on the inner wall of the groove. The thickness of the fusion layer is 3~6mm. The welding wire used is ER70S-6. The welding current is 240~260A. The welding voltage is 25~28V. The welding speed is 13~21cm / min. The shielding gas is a mixture of 80% argon and 20% carbon dioxide. The shielding gas flow rate is 20~30L / min.
[0011] According to the welding method for process holes of the coal mining machine traction shell provided by the present invention, in S4, the filler welding adopts a multi-layer, multi-pass welding method to build up layers one by one, the thickness of each weld bead is controlled at 3~5mm, and the interpass temperature is not lower than the preheating temperature; the welding wire used for filler welding is ER70S-6, the welding current is 260~300A, the welding voltage is 28~32V, the welding speed is 13~21cm / min, the shielding gas is a mixture of 80% argon and 20% carbon dioxide, and the shielding gas flow rate is 20~30L / min.
[0012] According to the welding method for process holes of the traction shell of the coal mining machine provided by the present invention, the tempering weld bead is welded to the side of the filler layer surface close to the shell base material. The welding thermal cycle of the tempering weld bead performs in-situ tempering on the heat-affected zone formed by the last weld bead of the filler weld, causing partial decomposition of the hardened structure. The welding wire used for the tempering weld bead is ER70S-6, the welding current is 260~300A, the welding voltage is 28~32V, the welding speed is 13~21cm / min, the shielding gas is a mixture of 80% argon and 20% carbon dioxide, and the shielding gas flow rate is 20~30L / min.
[0013] According to the welding method for process holes of the coal mining machine traction housing provided by the present invention, the tempered weld bead and the weld metal protruding above the surface of the base material are removed by mechanical grinding or machine tool cutting. After processing, the weld surface is flush with the surface of the base material and the weld reinforcement is zero. No additional scratches or pits shall be caused on the surface of the base material during the processing.
[0014] According to the welding method for process holes of the traction housing of the coal mining machine provided by the present invention, in S6, magnetic particle testing is performed after the weld has completely cooled to room temperature. The testing range covers the weld and the heat-affected zone on both sides of not less than 20 mm. The acceptance criteria for the test results are that the weld and the heat-affected zone are free from surface cracks, lack of fusion, and dense porosity defects.
[0015] The present invention discloses the following technical effects: This invention alters the path of crack propagation along the fusion line by setting a stepped straight bevel. Even if cracks exist, crack propagation will extend to the weld metal and base metal with high plasticity and toughness and good crack resistance, rather than to the fusion zone and heat-affected zone with low plasticity and toughness and poor crack resistance. This significantly delays the formation time of penetrating cracks and avoids oil leakage during use.
[0016] The present invention pre-welds a weld layer on the bevel surface, which results in less constraint during welding and less residual stress, thereby reducing the tendency of cracking in the heat-affected zone of the traction housing. The heat accumulation effect of the weld increases the preheating temperature of the filler weld, and the heat of the weld is equivalent to a secondary preheating of the filler weld, which effectively prevents the generation of cold cracks in the filler weld. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 A schematic diagram of the bevel for the process hole of the traction housing; Figure 2 A schematic diagram of a circular process block. Figure 3 Schematic diagram of the weld overlay of the process hole in the traction housing; Figure 4 A schematic diagram of the welding filling between the traction housing and the circular process block plate; Figure 5 This is a schematic diagram of the tempering weld bead. Figure 6 This is a diagram of the microstructure of the heat-affected zone of the traction housing after tempering weld treatment.
[0019] Among them, 1. Traction housing; 2. Circular process blocking plate; 3. Welded layer; 4. Filler layer; 5. Tempering weld bead. Detailed Implementation
[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0022] Reference Figure 1-6 The present invention provides a method for welding process holes in the traction housing 1 of a coal mining machine, comprising: S1, process the process hole of the traction housing 1 to form a stepped straight bevel, process a circular process block plate 2 that matches the process hole, and clean the oil, rust and oxide scale on the bevel and the surface of the base material on both sides until the metal luster is exposed. S2, insert the process plug plate into the process hole and position it on the step surface, so that a uniform circumferential annular welding gap is formed between the outer circle of the process plug plate and the inner wall of the bevel. S3, the process hole bevel area is preheated with flame, and a layer of fusion layer 3 is deposited on the inner wall of the bevel along the wall thickness direction using MAG welding; S4, using MAG welding for multi-layer, multi-pass welding, to fuse the process plug plate and traction housing 1 into one piece and fill the bevel; S5, a tempering weld bead 5 is welded on the outside of the shell, and the heat-affected zone of the filler is tempered by the welding heat cycle. S6, remove the tempered weld bead 5 and the weld metal that protrudes above the base metal surface to make the weld surface flush with the base metal, and perform magnetic particle testing on the weld joint.
[0023] Further optimization of the scheme: In S1, the traction housing 1 is made of ZG25CrNiMo medium carbon quenched and tempered steel, and the process block plate is made of Q355 low alloy high strength steel; the stepped straight bevel is formed by CNC milling machine, and the bevel cleaning range is the bevel surface and the surface area of the base material on both sides not less than 20mm.
[0024] Further optimization of the scheme: In S2, the outer diameter of the process plug plate and the inner diameter of the process hole step adopt a clearance fit. After assembly, the lower surface of the process plug plate is tightly fitted with the step surface, and a circumferentially uniform annular welding gap is formed between the outer circular surface of the process plug plate and the inner wall surface of the bevel.
[0025] Further optimizing scheme 3, the specific process of preheating welding includes the following steps: S31 uses flame heating to preheat the bevel area of the process hole as a whole, with the preheating temperature controlled at 100℃~150℃, and the temperature measurement point is located on the surface of the base material outside the bevel. S32, MAG welding is used to deposit a fusion layer 3 along the wall thickness direction on the inner wall of the groove. The thickness of the fusion layer 3 is 3~6mm. The welding wire used is ER70S-6. The welding current is 240~260A, the welding voltage is 25~28V, the welding speed is 13~21cm / min, and the shielding gas is a mixture of 80% argon and 20% carbon dioxide with a flow rate of 20~30L / min.
[0026] Further optimization of the scheme: In S4, the filler welding adopts a multi-layer, multi-pass welding method to build up layers one by one, with the thickness of each weld bead controlled at 3~5mm, and the interpass temperature not lower than the preheating temperature; the welding wire used for filler welding is ER70S-6, the welding current is 260~300A, the welding voltage is 28~32V, the welding speed is 13~21cm / min, and the shielding gas is a mixture of 80% argon and 20% carbon dioxide, with a shielding gas flow rate of 20~30L / min.
[0027] In further optimization of the scheme, in S5, the tempering weld 5 is welded to the side of the filler layer 4 near the shell base material. The welding thermal cycle of the tempering weld 5 performs in-situ tempering on the heat-affected zone formed by the last weld bead of the filler weld, causing partial decomposition of the hardened structure. The welding wire used for the tempering weld 5 is ER70S-6, the welding current is 260~300A, the welding voltage is 28~32V, the welding speed is 13~21cm / min, and the shielding gas is a mixture of 80% argon and 20% carbon dioxide with a shielding gas flow rate of 20~30L / min.
[0028] Further optimize the scheme. In S6, mechanical grinding or machine tool cutting is used to remove the tempered weld bead 5 and the weld metal that protrudes above the base material surface. After processing, the weld surface is flush with the base material surface and the weld reinforcement is zero. No additional scratches or pits shall be caused on the base material surface during processing.
[0029] In S6, magnetic particle testing is performed after the weld has completely cooled to room temperature. The testing range covers the weld and the heat-affected zone on both sides of the weld, which is no less than 20 mm. The acceptance criteria for the test results are that the weld and the heat-affected zone are free of surface cracks, lack of fusion, and dense porosity defects.
[0030] In the description of this invention, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this invention, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.
[0031] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for welding process holes in the traction housing (1) of a coal mining machine, characterized in that, include: S1, process the process hole of the traction housing (1) to form a stepped straight bevel, process a circular process block plate (2) that matches the process hole, and clean the oil, rust and oxide scale on the bevel and the surface of the base material on both sides until the metal luster is exposed. S2, insert the process plug plate into the process hole and position it on the step surface, so that a uniform circumferential annular welding gap is formed between the outer circle of the process plug plate and the inner wall of the bevel. S3, the process hole bevel area is preheated with flame, and a layer of fusion layer is deposited on the inner wall of the bevel along the wall thickness direction using MAG welding (3). S4, MAG welding is used to perform multi-layer and multi-pass welding to fuse the process plug plate and the traction housing (1) into one piece and fill the bevel; S5, a tempering weld bead (5) is welded on the outside of the shell, and the heat-affected zone of the filler weld is tempered by the welding heat cycle; S6, remove the tempered weld bead (5) and the weld metal that protrudes above the base metal surface to make the weld surface flush with the base metal, and perform magnetic particle testing on the weld joint.
2. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S1, the traction housing (1) is made of ZG25CrNiMo medium carbon tempered steel, and the process block plate is made of Q355 low alloy high strength steel. The stepped straight bevel is formed by CNC milling machine, and the bevel cleaning range is the bevel surface and the surface area of the parent material on both sides not less than 20mm.
3. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S2, the outer diameter of the process plug plate and the inner diameter of the process hole step are fitted with a clearance. After assembly, the lower surface of the process plug plate is tightly fitted with the step surface, and a uniform circumferential annular welding gap is formed between the outer circular surface of the process plug plate and the inner wall surface of the bevel.
4. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S3, the specific process of preheating and welding includes the following steps: S31 uses flame heating to preheat the bevel area of the process hole, with the preheating temperature controlled at 100℃~150℃, and the temperature measurement point is located on the surface of the base material outside the bevel. S32, MAG welding is used to deposit a weld layer (3) along the wall thickness direction on the inner wall of the groove. The thickness of the weld layer (3) is 3~6mm. The welding wire used for the weld is ER70S-6. The welding current is 240~260A. The welding voltage is 25~28V. The welding speed is 13~21cm / min. The shielding gas is a mixture of 80% argon and 20% carbon dioxide. The shielding gas flow rate is 20~30L / min.
5. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S4, the filler welding adopts a multi-layer, multi-pass welding method to build up layers one by one. The thickness of each weld bead is controlled at 3~5mm, and the interpass temperature is not lower than the preheating temperature. The welding wire used for filler welding is ER70S-6, the welding current is 260~300A, the welding voltage is 28~32V, the welding speed is 13~21cm / min, and the shielding gas is a mixture of 80% argon and 20% carbon dioxide with a shielding gas flow rate of 20~30L / min.
6. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S5, the tempering weld (5) is welded to the side of the filler layer (4) near the shell base material. The tempering weld (5) welding heat cycle tempers the heat-affected zone formed by the last weld of the filler weld in situ, causing the hardened structure to partially decompose. The welding wire used for the tempering weld (5) is ER70S-6, the welding current is 260~300A, the welding voltage is 28~32V, the welding speed is 13~21cm / min, the shielding gas is a mixture of 80% argon and 20% carbon dioxide, and the shielding gas flow rate is 20~30L / min.
7. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S6, the tempered weld bead (5) and the weld metal that protrudes above the base material surface are removed by mechanical grinding or machine tool cutting. After processing, the weld surface is flush with the base material surface and the weld reinforcement is zero. No additional scratches or pits shall be caused on the base material surface during processing.
8. The method for welding process holes in the traction housing (1) of a coal mining machine according to claim 1, characterized in that, In S6, magnetic particle testing is performed after the weld has completely cooled to room temperature. The testing range covers the weld and the heat-affected zone on both sides of the weld, which is no less than 20 mm. The acceptance criteria for the test results are that the weld and the heat-affected zone are free of surface cracks, lack of fusion, and dense porosity defects.