A method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide.
By using a combination of hydrogen sulfide reducing agent and extractant in wet-process phosphoric acid, the problems of low iron recovery rate and high ferrous salt impurity content in wet-process phosphoric acid have been solved, achieving efficient and low-cost ferrous salt recovery and purification.
Patent Information
- Application Number
- CN202611491642.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-10
AI Technical Summary
Existing methods for recovering ferrous salts from wet-process phosphoric acid suffer from low iron recovery rates and high impurity content in the ferrous salt products, making it difficult to meet the needs for the recovery and utilization of high-purity iron resources.
Hydrogen sulfide is used as a reducing agent, and iron ions are extracted using an extractant at a specific pH value. Through multi-stage countercurrent extraction and back-extraction processes, combined with the reduction reaction in the organic phase, the recovery rate and purity of iron ions are separated and improved.
It significantly improves the purity of ferrous salts and the recovery rate of iron, reduces operating costs, and is suitable for large-scale application, realizing efficient recovery of iron resources and preparation of high-purity ferrous salts.
Smart Images

Figure CN123062010A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of wet-process phosphoric acid production technology, mainly to the field of iron recovery technology in phosphoric acid, and specifically to a method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide. Background Technology
[0002] Wet-process phosphoric acid is a fundamental intermediate product in the phosphorus chemical industry, widely used in the preparation of downstream products such as phosphate fertilizers, phosphates, feed-grade phosphates, and electronic-grade phosphoric acid. Industrially, phosphoric acid is typically produced by reacting phosphate rock with sulfuric acid, with phosphogypsum as a byproduct. Due to fluctuations in the composition of raw materials, wet-process phosphoric acid often contains impurities such as iron, aluminum, magnesium, calcium, fluorine, silicon, and small amounts of heavy metals. Iron may exist as ferrous iron (Fe2+) or be converted to ferric iron (Fe3+) in acidic or oxidizing environments, and some may form complex ions with fluoride, sulfate, and phosphate. Excessive iron content reduces the quality of wet-process phosphoric acid, affecting subsequent concentration, crystallization, defluorination, purification, and the whiteness and stability of phosphate products. Therefore, under the trend of resource utilization and refined utilization, how to achieve controlled separation of iron impurities during the acid treatment stage and convert iron into ferrous salt products with reuse value has become an important direction for the coordinated promotion of wet-process phosphoric acid purification and iron resource recovery.
[0003] Existing technologies for separating and recovering iron from wet-process phosphoric acid generally include chemical precipitation, oxidation conversion, ion exchange / adsorption, solvent extraction, and membrane separation-assisted methods. Chemical precipitation involves adjusting pH and adding alkali or sulfides to precipitate iron into ferric hydroxide, ferrous sulfide, etc. This method is mature and relatively cost-effective. However, it often requires large amounts of neutralizing agents in strong acid systems, and the co-precipitates contain aluminum, calcium, magnesium, phosphorus, and organic / inorganic suspended solids, resulting in slow iron sludge settling, difficult filtration, and large washing water volume. If not properly controlled, phosphorus loss is significant, and the filter cake has poor quality and stability, limiting subsequent resource utilization. Oxidation methods often use air, oxygen, hydrogen peroxide, or chlorine-based oxidants to precipitate Fe. 2+ Converted to Fe 3+ Further removal via hydrolysis, precipitation, or extraction can enhance iron removal, but it transforms the usable ferrous form of iron into an iron salt system requiring further reduction or separation, increasing process steps and reducing agent consumption, and potentially introducing new ions or byproducts. Ion exchange and adsorption methods offer good selectivity and mild operating conditions, but are sensitive to acid concentration, fluorine content, and solid content. Resins or adsorbents are easily contaminated by fluorosilicates and organic matter, requiring frequent regeneration, and their economic viability decreases after scaling up. Membrane methods can assist in concentration and stepwise purification, but concentration polarization, membrane fouling, and material lifespan under high acid conditions remain engineering bottlenecks.
[0004] Solvent extraction, with its advantages of rapid mass transfer, good selectivity, and ease of continuous operation, is an important method for the deep purification of wet-process phosphoric acid. Related practices typically utilize acidic phosphorus extractants, amine extractants, or modified systems thereof to extract Fe.3+ Extraction can be performed, or an oxidation-extraction coupled route can be used to enhance iron migration. However, when iron in the target acid is mainly in the form of Fe, 2+ When the extraction conditions are either in a reducing / low potential environment, the extraction mechanism of ferric iron is not entirely applicable. 2+ Distribution coefficients are often low, requiring increased extractant concentration, number of stages, or ratio, leading to organic phase entrainment, extractant loss, and increased acid consumption during back-extraction. While oxidation followed by extraction can improve distribution capacity, it deviates from the goal of directly recovering ferrous salts. Furthermore, in complex phosphoric acid systems, iron exhibits competitive complexation and synergistic extraction phenomena with phosphate, fluoride, and trace metal ions. A single extraction parameter cannot simultaneously achieve both iron yield and product purity: increasing extraction intensity often introduces more co-extracted impurities, while reducing acidity or optimizing washing sacrifices iron yield. If the back-extraction solution is too acidic or contains residual extractant, metal fluoride complexes, and soluble phosphates, direct concentration and crystallization will yield ferrous salt products with high color, large fluctuations in impurity content, and low main content, failing to meet the requirements for Fe in water purification flocculants, battery material precursors, pigments, feed, or reagent grades. 2+ Scenarios with high requirements for content, acid-insoluble matter, heavy metals, and phosphorus, silicon and fluorine indicators.
[0005] Furthermore, the wet-process phosphoric acid system is characterized by high acidity, high solids content, and fluctuating composition, and the iron recovery process also faces safety and environmental constraints. Hydrogen sulfide has strong reducing properties and can react with Fe. 3+ Reduction occurs and promotes the reaction of sulfide ions with Fe. 2+ The formation of extremely insoluble ferrous sulfide theoretically possesses the coupling potential of "reducing ferric iron—stabilizing ferrous iron—directional iron precipitation." However, existing methods for recovering iron ions from wet-process phosphoric acid using H₂S as a reducing agent generally suffer from low iron recovery rates or high impurity content in the resulting ferrous salt products due to unreasonable extraction process design, hindering the efficient recovery and utilization of iron from wet-process phosphoric acid. Therefore, there is an urgent need for a raw material acid treatment method for wet-process phosphoric acid or systems containing wet-process phosphoric acid that can significantly improve the purity of ferrous salt products while maintaining a high iron recovery rate, achieving a balance between efficient iron resource recovery and high-quality ferrous salt preparation. Summary of the Invention
[0006] The purpose of this invention is to overcome the problems of low iron recovery rate and high impurity content in ferrous salts in existing methods for recovering ferrous salts from raw acid. This invention proposes a method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide.
[0007] To achieve the above objectives, the present invention provides a method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide, comprising the following steps: S1: After adjusting the pH of the raw material acid to 0.5-2.5 using an alkaline substance, an extractant is added for extraction and phase separation to obtain aqueous phase A and organic phase A; S2: After washing or dehydrating the organic phase A, add the first back-extraction agent for a first-stage back-extraction, separate the phases, and obtain aqueous phase B and organic phase B; S3: After adding a reducing agent to organic phase B for reduction reaction, a second stripping agent is added for two-stage stripping and phase separation to obtain organic phase C and aqueous phase C; organic phase C is washed or dehydrated to obtain extractant, which is returned to S1 for extraction; aqueous phase C is enriched, cooled and crystallized to obtain ferrous sulfate.
[0008] This invention discloses a method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide. First, the pH value of the raw acid is specifically adjusted to allow the extractant to better extract iron ions from the acid into the organic phase, effectively improving the iron ion recovery rate. Then, by specifically adjusting the composition and extraction conditions of the first back-extraction agent, effective back-extraction separation of magnesium, aluminum, and calcium ions is achieved while ensuring the iron ion recovery rate. Finally, the reduction reaction of iron ions by introducing hydrogen sulfide into the organic phase effectively avoids side reactions caused by hydrogen sulfide reduction in the aqueous phase, significantly reducing impurity ions in the aqueous phase after the second-stage back-extraction, thereby significantly improving the purity of the final ferrous salt. This method effectively achieves efficient recovery of iron ions from the raw acid while significantly improving the purity of the ferrous salt product. It also has the advantages of low operating costs, overall environmental friendliness and economic efficiency, making it suitable for large-scale application.
[0009] In step S1, preferably, the alkaline substance is one or more of NH3, Na2CO3, NaHCO3, K2CO3, and KHCO3.
[0010] Preferably, the raw material acid is one or more of the following: wet-process phosphoric acid (dilute acid), concentrated acid, residual raffinate acid, slag acid, industrial phosphoric acid, and waste phosphoric acid (phosphoric acid used in the electronics and other industries).
[0011] Preferably, the extractant is at least one of di(2-ethylhexyl) phosphate, 2-ethylhexyl phosphate, di(2,4,4-trimethylpentyl)phosphine, 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester, N,N-n-octylaminedimethylenephenylphosphonic acid, N,N-n-hexylaminedimethylenephenylphosphonic acid, toluenesulfonic acid, p-toluenesulfonic acid, benzenesulfonic acid, xylenesulfonic acid, dodecylbenzenesulfonic acid, dinonylnaphthalenesulfonic acid, cinnamic acid, and lauric acid; more preferably, the extractant is at least one of 2-ethylhexyl phosphate and 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester.
[0012] Preferably, the extraction employs a 1-5 stage countercurrent extraction process, and more preferably, a 3-stage countercurrent extraction process.
[0013] Preferably, in the extraction process, the temperature of the single-stage extraction is 50-85℃ and the time is 1-60 min.
[0014] Preferably, the volume ratio of the extractant to the raw acid (compared to O / A) is 1-6:1; more preferably, it is 4:1.
[0015] In step S2, preferably, the organic phase A is washed with phosphoric acid or water at a concentration of 1-8 wt%. Preferably, the washing temperature is 10-95℃.
[0016] Preferably, the volume ratio of the washing solution (1-8 wt% phosphoric acid or water) to organic phase A is 1:1-10; more preferably, it is 1:3.
[0017] Preferably, the phosphorus content washed into organic phase A is less than 10 wt%.
[0018] Preferably, the sulfuric acid concentration in the first stripping agent is 10-50 wt%; more preferably, the sulfuric acid concentration is 30 wt%.
[0019] Preferably, the back-extraction stage employs a 1-5 stage countercurrent back-extraction process; more preferably, a 1-stage countercurrent back-extraction process is used.
[0020] Preferably, in the single-stage back-extraction, the temperature of the single-stage back-extraction is 10-90℃ and the time is 1-60min.
[0021] Preferably, the volume ratio of the first stripping agent to organic phase A is 1-8:1; more preferably, it is 3:1.
[0022] Preferably, the method further includes: cooling and crystallizing the aqueous phase A to obtain phosphates (ammonium phosphate, potassium phosphate, sodium phosphate).
[0023] In step S3, preferably, the sulfuric acid concentration in the second stripping agent is 10-30 wt%; the preferred second stripping agent can better strip out iron ions, achieving efficient recovery of iron ions.
[0024] Preferably, the reduction reaction is carried out at a temperature of 0-100°C for 5-120 minutes.
[0025] Preferably, the temperature of the second-stage back-extraction is 0~80℃, and the time is 1-120min; the pH value during the second-stage back-extraction is controlled to be no greater than 2; the volume ratio of the second back-extraction agent to organic phase B is 1-10:1; more preferably 3:1. Preferably, the cooling and crystallization temperature of the aqueous phase C is 0-10℃.
[0026] Preferably, stirring is performed during the second-stage back-extraction, with a stirring speed of 400-900 r / min.
[0027] Preferably, the process further includes step S4: treating the aqueous phase B to obtain substances containing magnesium, aluminum, and calcium; the specific treatment method includes any of the following: (1) First, adjust the temperature of aqueous phase B to above 35℃ to crystallize and precipitate calcium sulfate; then crystallize and precipitate at 15-30℃ to separate magnesium sulfate; finally crystallize and precipitate at 0-10℃ to separate aluminum sulfate. (2) First, adjust the temperature of aqueous phase B to above 35℃ to crystallize and precipitate calcium sulfate; then add alkali solution to adjust the pH value. Collect the precipitate with a pH value of 3.8-7.5 to obtain aluminum hydroxide; collect the precipitate with a pH value of 9-11.5 to obtain magnesium hydroxide.
[0028] The beneficial effects of this invention are: 1. This invention utilizes hydrogen sulfide to extract and recover high-purity ferrous salts from raw acid. By specifically adjusting the pH value of the raw acid, the extractant can better extract iron ions from the raw acid into the organic phase, effectively improving the iron ion recovery rate.
[0029] 2. This invention utilizes hydrogen sulfide to extract and recover high-purity ferrous salts from raw acid. By introducing hydrogen sulfide into the organic phase to reduce ferrous ions, the side reactions caused by hydrogen sulfide reduction in the aqueous phase are effectively avoided, significantly reducing impurity ions in the aqueous phase after the second-stage back-extraction, thereby significantly improving the purity of the final ferrous salt.
[0030] 3. The present invention utilizes hydrogen sulfide to extract and recover high-purity ferrous salts from raw acid. This method effectively achieves efficient recovery of ferrous ions from the raw acid while significantly improving the purity of the ferrous salt product. It also has the advantages of low operating cost, good overall environmental protection and economy, and is suitable for large-scale promotion and application. Attached Figure Description
[0031] Figure 1 This is a process flow diagram of the method for extracting and recovering high-purity ferrous salts in Example 1 of the present invention. Detailed Implementation
[0032] The technical solution of the present invention will be further described in detail below with reference to the embodiments.
[0033] In this process, hydrogen sulfide needs to be introduced into a closed reactor, and the tail gas generated by the reaction is treated by alkaline absorption. The process of hydrogen sulfide reducing ferric ions will produce elemental sulfur solid as a byproduct. This solid needs to be removed by filtration to prevent elemental sulfur from entering the subsequent back-extraction system and contaminating the ferrous salt product.
[0034] Example 1
[0035] A method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide (process flow diagram shown) Figure 1 ), including the following steps: S1: After adjusting the pH of the raw material acid (wet-process phosphoric acid: 23wt% phosphoric acid, 1.2wt% magnesium ions, 0.85wt% aluminum ions, 0.3wt% calcium ions, and 0.9wt% iron ions) to 1.5 using an alkaline substance (Na2CO3), an extractant (2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester) was added for extraction (3-stage countercurrent extraction process; single-stage extraction temperature was 65℃, time was 30min; volume ratio of extractant to raw material acid (O / A) was 3:1), and phase separation was performed to obtain aqueous phase A and organic phase A. S2: After washing organic phase A (water; volume ratio 1:5; washing temperature 60℃), add the first back-extraction agent (containing 30wt% sulfuric acid) for a single-stage back-extraction process (one-stage countercurrent back-extraction process; single-stage back-extraction temperature 60℃, time 30min; volume ratio of the first back-extraction agent to organic phase A 3:1), and separate the phases to obtain aqueous phase B and organic phase B; Aqueous phase A was cooled (2°C) and crystallized to obtain phosphate (a mixture of ammonium phosphate, potassium phosphate, and sodium phosphate). S3: Hydrogen sulfide is introduced into organic phase B (to remove Fe from the solution). 3+ Completely reduced to Fe 2+ After a reduction reaction (at 30°C for 60 min) was carried out, the solution was filtered. Then, a second stripping agent (containing 30 wt% sulfuric acid, with a volume ratio of 3:1 to organic phase B) was added to the filtrate for stripping (at 30°C for 70 min; the pH value during stripping was controlled at 1; the stirring speed was 600 r / min). The phases were separated to obtain organic phase C and aqueous phase C. Organic phase C was washed and dehydrated to obtain the extractant, which was returned to S1 for extraction. Aqueous phase C was cooled and crystallized (at 5°C) to obtain ferrous sulfate. S4: First, adjust the temperature of aqueous phase B to 50℃ to crystallize and precipitate calcium sulfate; then add alkali solution to adjust the pH value. Collect the precipitate with a pH value of 3.8-7.5 to obtain aluminum hydroxide; collect the precipitate with a pH value of 9-11.5 to obtain magnesium hydroxide.
[0036] Example 2
[0037] A method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide includes the following steps: S1: After adjusting the pH of the raw material acid (wet-process phosphoric acid: 23wt% phosphoric acid, 1.2wt% magnesium ions, 0.85wt% aluminum ions, 0.3wt% calcium ions, and 0.9wt% iron ions) to 2.5 using an alkaline substance (NaHCO3), an extractant (2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester) was added for extraction (5-stage countercurrent extraction process; single-stage extraction temperature was 50℃, time was 30min; volume ratio of extractant to raw material acid (O / A) was 6:1), and phase separation was performed to obtain aqueous phase A and organic phase A. S2: After washing organic phase A (5wt% phosphoric acid; volume ratio 1:10; washing temperature 30℃), add the first back-extraction agent (containing 50wt% sulfuric acid) for a single-stage back-extraction process (single-stage countercurrent back-extraction process; single-stage back-extraction temperature 10℃, time 30min; volume ratio of the first back-extraction agent to organic phase A 8:1), and separate the phases to obtain aqueous phase B and organic phase B; Aqueous phase A was cooled (5°C) and crystallized to obtain phosphate (a mixture of ammonium phosphate, potassium phosphate, and sodium phosphate). S3: Hydrogen sulfide is introduced into organic phase B (to remove Fe from the solution). 3+ Completely reduced to Fe 2+ After a reduction reaction (at 20°C for 70 min) was carried out, the solution was filtered. Then, a second stripping agent (containing 10 wt% sulfuric acid, with a volume ratio of 10:1 to organic phase B) was added to the filtrate for stripping (at 50°C for 70 min; the pH value during stripping was controlled at 2; the stirring speed was 400 r / min). The phases were separated to obtain organic phase C and aqueous phase C. Organic phase C was washed and dehydrated to obtain the extractant, which was returned to S1 for extraction. Aqueous phase C was cooled and crystallized (at 0°C) to obtain ferrous sulfate. S4: First, adjust the temperature of aqueous phase B to 50℃ to crystallize and separate calcium sulfate; then crystallize at 15℃ to separate magnesium sulfate; finally, crystallize at 5℃ to separate aluminum sulfate.
[0038] Example 3
[0039] S1: After adjusting the pH of the raw material acid (wet-process phosphoric acid: 23wt% phosphoric acid, 1.2wt% magnesium ions, 0.85wt% aluminum ions, 0.3wt% calcium ions, and 0.9wt% iron ions) to 0.5 using an alkaline substance (K2CO3), an extractant (2-ethylhexyl phosphate, 2-ethylhexyl ester) was added for extraction (two-stage countercurrent extraction process; single-stage extraction temperature was 85℃, time was 60min; volume ratio of extractant to raw material acid (O / A) was 1:1), and phase separation was performed to obtain aqueous phase A and organic phase A. S2: After washing organic phase A (water; volume ratio 1:1; washing temperature 95℃), add the first back-extraction agent (containing 10wt% sulfuric acid) for a single-stage back-extraction process (3-stage countercurrent back-extraction process; single-stage back-extraction temperature 90℃, time 20min; volume ratio of the first back-extraction agent to organic phase A 1:1), and separate the phases to obtain aqueous phase B and organic phase B; Aqueous phase A was cooled (2°C) and crystallized to obtain phosphate (a mixture of ammonium phosphate, potassium phosphate, and sodium phosphate). S3: Hydrogen sulfide is introduced into organic phase B (to remove Fe from the solution). 3+ Completely reduced to Fe 2+ After a reduction reaction (at 30°C for 60 min) was carried out, the solution was filtered. Then, a second stripping agent (containing 20 wt% sulfuric acid, with a volume ratio of 1:1 to organic phase B) was added to the filtrate for stripping (at 30°C for 70 min; the pH value during stripping was controlled at 1; the stirring speed was 900 r / min). The phases were separated to obtain organic phase C and aqueous phase C. Organic phase C was washed and dehydrated to obtain the extractant, which was returned to S1 for extraction. Aqueous phase C was cooled and crystallized (at 10°C) to obtain ferrous sulfate. S4: First, adjust the temperature of aqueous phase B to 35℃ to crystallize and separate calcium sulfate; then crystallize at 20℃ to separate magnesium sulfate; finally, crystallize at 2℃ to separate aluminum sulfate.
[0040] Comparative Example 1
[0041] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S3, sulfur dioxide is used instead of hydrogen sulfide for reduction.
[0042] Comparative Example 2
[0043] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S3, sodium sulfide is used instead of hydrogen sulfide for reduction.
[0044] Comparative Example 3
[0045] A method for extracting and recovering ferrous salts from raw acid, with the same steps as in Example 1, except that in step S3, a second extractant and hydrogen sulfide are simultaneously added to organic phase B. Specifically, a second back-extraction agent (containing 30 wt% sulfuric acid, with a volume ratio of 3:1 to organic phase B) is added to organic phase B, and hydrogen sulfide is introduced (to remove Fe from the solution). 3+ Completely reduced to Fe 2+(For reference), while performing reduction back-extraction (temperature 30℃, time 70min; control the pH value during back-extraction to 1; stirring speed 600r / min), filter, and then separate the filtrate to obtain organic phase C and aqueous phase C; wash and dehydrate organic phase C to obtain extractant, which is returned to S1 for extraction; cool and crystallize aqueous phase C (temperature 5℃) to obtain ferrous sulfate.
[0046] Comparative Example 4
[0047] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that the pH value during the second-stage back-extraction in S3 is adjusted to 3.
[0048] Comparative Example 5
[0049] A method for efficiently extracting and recovering metal cations from raw acid has the same steps as in Example 1, except that in S1, the extractant is changed to lauric acid.
[0050] Comparative Example 6
[0051] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S1, the extractant is changed to stearic acid (octadecanoic acid).
[0052] Comparative Example 7
[0053] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S1, the extraction temperature is adjusted to 40°C.
[0054] Comparative Example 8
[0055] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S1, the extraction temperature is adjusted to 90°C.
[0056] Comparative Example 9
[0057] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S1, the volume ratio of the extractant to the raw acid is adjusted to 0.5:1.
[0058] Comparative Example 10
[0059] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S1, the volume ratio of the extractant to the raw acid is adjusted to 7:1.
[0060] Comparative Example 11
[0061] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S2, the concentration of sulfuric acid in the first stripping agent is adjusted to 55 wt%.
[0062] Comparative Example 12
[0063] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S2, the concentration of sulfuric acid in the first stripping agent is adjusted to 5 wt%.
[0064] Comparative Example 13
[0065] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S2, the volume ratio of the first stripping agent to organic phase A is adjusted to 9:1.
[0066] Comparative Example 14
[0067] A method for extracting and recovering ferrous salts from raw acid has the same steps as in Example 1, except that in S2, the volume ratio of the first stripping agent to organic phase A is adjusted to 0.5:1.
[0068] The recovery rate of iron and the purity of the products in Examples 1-3 and Comparative Examples 1-14 were statistically analyzed, and the results are shown in the table below:
[0069] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide, characterized in that, Includes the following steps: S1: After adjusting the pH of the raw material acid to 0.5-2.5 using an alkaline substance, an extractant is added for extraction and phase separation to obtain aqueous phase A and organic phase A; S2: Add the first stripping agent to the organic phase A for a first-stage stripping, separate the phases, and obtain the aqueous phase B and the organic phase B; S3: After adding hydrogen sulfide to organic phase B for reduction reaction, a second stripping agent is added for stripping and phase separation to obtain organic phase C and aqueous phase C; organic phase C is washed or dehydrated to obtain extractant, which is returned to S1 for extraction; aqueous phase C is enriched, cooled and crystallized to obtain ferrous sulfate.
2. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, In step S1, the alkaline substance is one or more of NH3, Na2CO3, NaHCO3, K2CO3, and KHCO3.
3. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, Step S1, the raw material acid is one or more of wet-process phosphoric acid, concentrated acid, raffinate acid, slag acid, industrial phosphoric acid, and waste phosphoric acid.
4. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, In step S1, the extractant is at least one of the following: di(2-ethylhexyl) phosphate, 2-ethylhexyl phosphate, di(2,4,4-trimethylpentyl)phosphine, 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester, N,N-n-octylaminedimethylenephenylphosphonic acid, N,N-n-hexylaminedimethylenephenylphosphonic acid, toluenesulfonic acid, p-toluenesulfonic acid, benzenesulfonic acid, xylenesulfonic acid, dodecylbenzenesulfonic acid, dinonylnaphthalenesulfonic acid, cinnamic acid, and lauric acid; the extraction temperature is 50-85℃; and the volume ratio of extractant to raw acid is 1-6:
1.
5. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, Step S2 also includes washing organic phase A with phosphoric acid or water at a concentration of 1-8 wt%.
6. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 5, characterized in that, The volume ratio of the washing liquid to organic phase A is 1:1-10.
7. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, In step S2, the sulfuric acid concentration in the first stripping agent is 10-50 wt%; the volume ratio of the first stripping agent to organic phase A is 1-8:1; and the temperature of the first stripping step is 10-90℃.
8. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, Step S3, the temperature of the reduction reaction is 0~100℃.
9. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, Step S3: In the second stripping agent, the sulfuric acid concentration is 10-30 wt%; the pH value during the second-stage stripping is controlled to be no greater than 2; the temperature of the second-stage stripping is 0-80℃; and the volume ratio of the second stripping agent to organic phase B is 1-10:
1.
10. The method for extracting and recovering high-purity ferrous salts from raw acid using hydrogen sulfide according to claim 1, characterized in that, It also includes S4: treating aqueous phase B to obtain substances containing magnesium, aluminum, and calcium; the specific treatment method includes any of the following: (1) First, adjust the temperature of aqueous phase B to above 35℃ to crystallize and precipitate calcium sulfate; then crystallize and precipitate at 15-30℃ to separate magnesium sulfate; finally crystallize and precipitate at 0-10℃ to separate aluminum sulfate. (2) First, adjust the temperature of aqueous phase B to above 35℃ to crystallize and precipitate calcium sulfate; then add alkali solution to adjust the pH value. Collect the precipitate with a pH value of 3.8-7.5 to obtain aluminum hydroxide; collect the precipitate with a pH value of 9-11.5 to obtain magnesium hydroxide.