A plaster formula for ceramic molds that combines high strength and high water absorption

By compounding raw materials such as β-hemihydrate gypsum and using specific processes, a multi-level porous ceramic mold gypsum structure is constructed, which solves the contradiction between the strength and water absorption of traditional gypsum, improves the service life and production efficiency of molds, and reduces costs.

CN123062227APending Publication Date: 2026-11-10湖北宜化环保科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611127341.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

While existing ceramic mold plaster can guarantee high water absorption rate and high water absorption capacity, it also suffers from low flexural and compressive strength, poor mold wear resistance, and is prone to powdering, flaking, chipping, and cracking, which affects the efficiency and quality of ceramic production.

Method used

By using a compound of raw materials such as β-hemihydrate gypsum, anhydrous gypsum, bentonite, aluminate cement, sodium hexametaphosphate, sodium bicarbonate and dicalcium phosphate, and through screening, premixing, stirring and curing processes, a multi-level porous structure is constructed to improve the density and strength of gypsum.

Benefits of technology

While ensuring high water absorption rate and absorption speed, the structural strength and stability of the mold are greatly improved, the frequency of mold replacement is reduced, raw material consumption is reduced, and production efficiency and quality are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of ceramic mold plaster technology, and specifically provides a ceramic mold plaster formula that balances high strength and high water absorption. The preparation method of the ceramic mold plaster includes the following steps: S1: Independently sieve and remove impurities from powder raw materials such as β-hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clump-like particles and large impurities; S2: Add functional auxiliary materials such as aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, and bentonite into a closed premixing device according to the specified ratio, and fully premix using a medium-speed homogenizing stirring method; S3: Add the sieved qualified β-hemihydrate gypsum and anhydrous gypsum matrix powder into a main mixing device, and perform loosening pretreatment of the matrix powder using a low-speed stirring mode. This invention significantly improves the density and structural strength of the hardened plaster body while ensuring high water absorption rate and high water absorption capacity of the mold, meeting the requirements of rapid ceramic casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic mold plaster technology, and in particular to a ceramic mold plaster formulation that combines high strength and high water absorption. Background Technology

[0002] Sanitary ceramics production commonly employs gypsum mold injection molding technology. Relying on the porous capillary water absorption characteristics of gypsum material, it quickly absorbs the moisture inside the ceramic slurry, achieving body shaping, curing, and demolding. It has advantages such as high molding simulation, low cost, convenient mold repair, and adaptability to complex curved surface shapes, making it the most widely used mold base material in the ceramic industry.

[0003] Currently, most ceramic mold plaster used in industrial production employs a single β-hemihydrate plaster system. However, this system has inherent performance defects that restrict the automated, large-scale, and high-quality production of ceramics. Traditional β-plaster, after hardening, has a simple pore structure, leading to an inherent contradiction between water absorption and mechanical strength: If high water absorption and a high water absorption rate are ensured, the mold's internal porosity is high and its structure is loose, resulting in low flexural and compressive strength, poor wear resistance, and a high risk of powdering, flaking, chipping, and cracking under high-pressure grouting and repeated wet-dry cycles. This results in a short mold lifespan, requiring frequent mold replacements and significantly increasing raw material consumption and labor costs. Conversely, increasing plaster density and reducing porosity to improve mold strength directly leads to blocked pores, decreased capillary absorption capacity, slower water absorption rate, and a significantly extended green body forming cycle, reducing production efficiency and causing quality problems such as incomplete green body forming, difficulty in demolding, and numerous surface defects. Therefore, a ceramic mold plaster formulation that balances high strength and high water absorption is needed to address these issues. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and to propose a ceramic mold plaster formula that combines high strength and high water absorption.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 20-24 parts β hemihydrate plaster, 15-19 parts anhydrous plaster, 8-12 parts bentonite, 9-13 parts aluminate cement, 5-9 parts sodium hexametaphosphate, 11-15 parts sodium bicarbonate, 7-11 parts sodium hexametaphosphate, and 12-16 parts dicalcium phosphate.

[0007] Preferably, a ceramic mold plaster formula that combines high strength and high water absorption comprises the following raw materials in parts by weight: 21-23 parts of β hemihydrate plaster, 16-18 parts of anhydrous plaster, 9-11 parts of bentonite, 10-12 parts of aluminate cement, 6-8 parts of sodium hexametaphosphate, 12-14 parts of sodium bicarbonate, 8-10 parts of sodium hexametaphosphate, and 13-15 parts of dicalcium phosphate.

[0008] Preferably, a ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 22 parts β hemihydrate plaster, 17 parts anhydrous plaster, 10 parts bentonite, 11 parts aluminate cement, 7 parts sodium hexametaphosphate, 13 parts sodium bicarbonate, 9 parts sodium hexametaphosphate, and 14 parts dicalcium phosphate.

[0009] The preparation method of ceramic mold plaster includes the following steps:

[0010] S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities.

[0011] S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing.

[0012] S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode.

[0013] S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles.

[0014] S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

[0015] Preferably, in step S2, the premixing speed is set to 240–300 r / min, and the premixing time is 15–20 min.

[0016] Preferably, in step S3, the stirring speed for the matrix powder pretreatment is 150-200 r / min, and the pretreatment time is 3-5 min.

[0017] Preferably, in step S4, the gradient feeding time is controlled at 12-18 min, the mixing speed is controlled at 350-450 r / min, and the overall mixing time is 32-38 min.

[0018] Preferably, in step S6, the curing environment temperature is controlled at 20–28°C, the relative humidity is controlled at 40%–60%, and the constant temperature curing time is 26–42 hours.

[0019] The beneficial effects of this invention are:

[0020] 1. By compounding β-hemihydrate gypsum and anhydrous gypsum to construct a multi-level porous structure, and combining the combined effects of bentonite, dicalcium phosphate filling and regulation, aluminate cement reinforcement, and salt additive hydration regulation, the density and structural strength of the hardened gypsum body are greatly improved while ensuring the high water absorption rate and high water absorption speed of the mold and meeting the requirements of rapid ceramic injection molding.

[0021] 2. It can significantly reduce the frequency of mold replacement, reduce raw material consumption and solid waste output, reduce the overall cost of ceramic production, and has both excellent performance and environmental and economic benefits, with broad application prospects. Detailed Implementation

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0023] Example 1

[0024] A ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 20 parts β hemihydrate plaster, 15 parts anhydrous plaster, 8 parts bentonite, 9 parts aluminate cement, 5 parts sodium hexametaphosphate, 11 parts sodium bicarbonate, 7 parts sodium hexametaphosphate, and 12 parts dicalcium phosphate.

[0025] The preparation method of ceramic mold plaster includes the following steps:

[0026] S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities.

[0027] S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing.

[0028] S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode.

[0029] S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles.

[0030] S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

[0031] In this embodiment, in step S2, the premixing stirring speed is set to 240 r / min, and the premixing time is 15 min. In step S3, the matrix powder pretreatment stirring speed is 150 r / min, and the pretreatment time is 3 min. In step S4, the gradient feeding time is controlled at 12 min, the mixing stirring speed is controlled at 350 r / min, and the overall mixing time is 32 min. In step S6, the maturation environment temperature is controlled at 20℃, the relative humidity is controlled at 40%, and the constant temperature maturation time is 26 h.

[0032] Example 2

[0033] A ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 21 parts β hemihydrate plaster, 16 parts anhydrous plaster, 9 parts bentonite, 10 parts aluminate cement, 6 parts sodium hexametaphosphate, 12 parts sodium bicarbonate, 8 parts sodium hexametaphosphate, and 13 parts dicalcium phosphate.

[0034] The preparation method of ceramic mold plaster includes the following steps:

[0035] S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities.

[0036] S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing.

[0037] S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode.

[0038] S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles.

[0039] S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

[0040] In this embodiment, in step S2, the premixing stirring speed is set to 250 r / min, and the premixing time is 16 min. In step S3, the matrix powder pretreatment stirring speed is 160 r / min, and the pretreatment time is 3 min. In step S4, the gradient feeding time is controlled at 14 min, the mixing stirring speed is controlled at 370 r / min, and the overall mixing time is 34 min. In step S6, the maturation environment temperature is controlled at 22℃, the relative humidity is controlled at 45%, and the constant temperature maturation time is 30 h.

[0041] Example 3

[0042] A ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 22 parts β hemihydrate plaster, 17 parts anhydrous plaster, 10 parts bentonite, 11 parts aluminate cement, 7 parts sodium hexametaphosphate, 13 parts sodium bicarbonate, 9 parts sodium hexametaphosphate, and 14 parts dicalcium phosphate.

[0043] The preparation method of ceramic mold plaster includes the following steps:

[0044] S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities.

[0045] S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing.

[0046] S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode.

[0047] S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles.

[0048] S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

[0049] In this embodiment, in step S2, the premixing stirring speed is set to 260 r / min, and the premixing time is 18 min. In step S3, the matrix powder pretreatment stirring speed is 180 r / min, and the pretreatment time is 4 min. In step S4, the gradient feeding time is controlled at 17 min, the mixing stirring speed is controlled at 400 r / min, and the overall mixing time is 34 min. In step S6, the maturation environment temperature is controlled at 24℃, the relative humidity is controlled at 50%, and the constant temperature maturation time is 32 h.

[0050] Example 4

[0051] A ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 23 parts β hemihydrate plaster, 18 parts anhydrous plaster, 11 parts bentonite, 12 parts aluminate cement, 8 parts sodium hexametaphosphate, 14 parts sodium bicarbonate, 10 parts sodium hexametaphosphate, and 15 parts dicalcium phosphate.

[0052] The preparation method of ceramic mold plaster includes the following steps:

[0053] S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities.

[0054] S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing.

[0055] S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode.

[0056] S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles.

[0057] S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

[0058] In this embodiment, in step S2, the premixing stirring speed is set to 280 r / min, and the premixing time is 18 min. In step S3, the matrix powder pretreatment stirring speed is 190 r / min, and the pretreatment time is 4 min. In step S4, the gradient feeding time is controlled at 17 min, the mixing stirring speed is controlled at 430 r / min, and the overall mixing time is 36 min. In step S6, the maturation environment temperature is controlled at 27℃, the relative humidity is controlled at 55%, and the constant temperature maturation time is 40 h.

[0059] Example 5

[0060] A ceramic mold plaster formula that combines high strength and high water absorption includes the following raw materials in parts by weight: 24 parts β hemihydrate plaster, 19 parts anhydrous plaster, 12 parts bentonite, 13 parts aluminate cement, 9 parts sodium hexametaphosphate, 15 parts sodium bicarbonate, 11 parts sodium hexametaphosphate, and 16 parts dicalcium phosphate.

[0061] The preparation method of ceramic mold plaster includes the following steps:

[0062] S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities.

[0063] S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing.

[0064] S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode.

[0065] S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles.

[0066] S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

[0067] In this embodiment, in step S2, the premixing stirring speed is set to 300 r / min, and the premixing time is 20 min. In step S3, the matrix powder pretreatment stirring speed is 200 r / min, and the pretreatment time is 5 min. In step S4, the gradient feeding time is controlled at 18 min, the mixing stirring speed is controlled at 450 r / min, and the overall mixing time is 38 min. In step S6, the maturation environment temperature is controlled at 28℃, the relative humidity is controlled at 60%, and the constant temperature maturation time is 42 h.

[0068] Research on plaster for ceramic molds:

[0069] The ceramic mold plaster prepared in Examples 1 to 5 was used to test its water absorption rate, water absorption speed, and flexural strength. The results are shown below:

[0070]

[0071] While ensuring rapid water absorption and molding of ceramic slurry, the strength and stability of the mold structure are greatly improved, which can significantly increase the cycle life of ceramic molds, reduce the probability of mold deformation, cracking and powdering, and adapt to the needs of high-pressure automated slurry injection production. Furthermore, Example 5 is the best embodiment.

Claims

1. A plaster formula for ceramic molds that combines high strength and high water absorption, characterized in that, The raw materials include the following parts by weight: 20-24 parts β-hemihydrate gypsum, 15-19 parts anhydrous gypsum, 8-12 parts bentonite, 9-13 parts aluminate cement, 5-9 parts sodium hexametaphosphate, 11-15 parts sodium bicarbonate, 7-11 parts sodium hexametaphosphate, and 12-16 parts dicalcium phosphate.

2. The ceramic mold plaster formula according to claim 1, characterized in that, The raw materials include the following parts by weight: 21-23 parts β-hemihydrate gypsum, 16-18 parts anhydrous gypsum, 9-11 parts bentonite, 10-12 parts aluminate cement, 6-8 parts sodium hexametaphosphate, 12-14 parts sodium bicarbonate, 8-10 parts sodium hexametaphosphate, and 13-15 parts dicalcium phosphate.

3. The ceramic mold plaster formula according to claim 1, characterized in that, The raw materials include the following parts by weight: 22 parts β hemihydrate gypsum, 17 parts anhydrous gypsum, 10 parts bentonite, 11 parts aluminate cement, 7 parts sodium hexametaphosphate, 13 parts sodium bicarbonate, 9 parts sodium hexametaphosphate, and 14 parts dicalcium phosphate.

4. The ceramic mold plaster formula according to claim 1, characterized in that, The preparation method of ceramic mold plaster includes the following steps: S1: Independently screen and remove impurities from powder raw materials such as β hemihydrate gypsum, anhydrous gypsum, and bentonite to remove damp, clumped particles and large impurities. S2: Aluminate cement, sodium hexametaphosphate, sodium bicarbonate, dicalcium phosphate, bentonite and other functional auxiliary materials are put into a closed premixing equipment according to the proportion and fully premixed by medium-speed homogenizing mixing. S3: The qualified β hemihydrate gypsum and anhydrous gypsum matrix powder are fed into the main mixing equipment, and the matrix powder is loosened and pretreated by low-speed mixing mode. S4: The premixed functional additives are gradually incorporated into the matrix gypsum powder using a continuous micro-feeding method to gradually complete the powder compound mixing. Through long-term stirring at a constant speed, the inorganic filler components and hydration control components are uniformly coated on the gypsum particles. S5: The modified and mixed powder is placed in a constant temperature and humidity sealed environment for static curing to stabilize the internal hydration activity and structural stress of the powder. After curing, the water absorption rate, water absorption speed and flexural strength are tested. After meeting the standards, it is packaged and stored to obtain the finished ceramic mold plaster.

5. The ceramic mold plaster formula according to claim 4, characterized in that, In step S2, the premixing speed is set to 240–300 r / min, and the premixing time is 15–20 min.

6. The ceramic mold plaster formula according to claim 4, characterized in that, In step S3, the stirring speed for the matrix powder pretreatment is 150-200 r / min, and the pretreatment time is 3-5 min.

7. The ceramic mold plaster formula according to claim 4, characterized in that, In step S4, the gradient feeding time is controlled at 12-18 min, the mixing speed is controlled at 350-450 r / min, and the overall mixing time is 32-38 min.

8. The ceramic mold plaster formula according to claim 4, characterized in that, In step S6, the curing environment temperature is controlled at 20–28°C, the relative humidity is controlled at 40%–60%, and the constant temperature curing time is 26–42 hours.